Preparation of bimetallic nanoparticles with antibacterial function

Through the design of green reducing liquid and core-shell structures of plants, the problem of particle size and stability in the preparation of silver-copper bimetallic nanoparticles is solved, and efficient and economical antibacterial effect is achieved, providing a green and environmentally friendly nano-anti-bacterial nano-anti-bacterial Material.

CN119032968APending Publication Date: 2024-11-29HUZHOU COLLEGE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411143298.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

It is difficult to accurately control the size, shape and distribution of existing silver-copper bimetallic nanoparticles during the preparation process, and the nanoparticles are prone to agglomeration during long-term use, affecting the stability of antibacterial properties.

Method used

The green reducing liquid prepared by plants is used to form silver-copper bimetallic nanoparticles through magnetic stirring and heating. The core-shell structure is designed. Silver provides antibacterial properties as the shell, and copper serves as the core support structure to ensure the stability of the nanoparticles and coordinated antibacterial. effect.

Benefits of technology

A green, simple and fast synthesis process is realized, and silver-copper bimetallic nanoparticles with uniform size and dispersion are prepared, with continuous and long-term antibacterial effects, reducing the amount of silver used, saving costs, and maintaining efficient antibacterial properties. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032968A_ABST
    Figure CN119032968A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of bimetallic nanoparticles with an antibacterial function. The preparation method comprises the following steps: (1) preparing a green reducing solution; (2) transferring the green reducing solution into a reactor, immediately adding stock solutions of two metal salts of silver and copper, magnetically stirring and heating until the stock solutions are boiled; (3) stopping heating, after the temperature of the reactor is reduced to room temperature, continuously adding the green reducing solution, and continuously stirring and reacting to obtain a mixture; and (4) centrifuging the mixture at a high speed, collecting precipitates, washing and drying to obtain the bimetallic nanoparticles with the antibacterial function. According to the method, the reduction liquid is prepared from plants, the bimetallic nanoparticles with the antibacterial function can be synthesized in a green, simple and rapid mode, and the bimetallic nanoparticles are uniform in size, not prone to agglomeration and capable of being directly used as an antibacterial material for killing bacteria or fungi.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibacterial metal nanomaterials, and in particular to the preparation of bimetallic nanoparticles with antibacterial function. Background Art

[0002] With the rapid development and widespread application of nanotechnology, nanomaterials have shown great potential in the field of antibacterial. Nano antibacterial materials have the advantages of high safety, good heat resistance and durability, and are not easy to develop drug resistance. Among many nanomaterials, silver and copper have attracted widespread attention due to their unique antibacterial properties. Silver ions have broad-spectrum antibacterial activity and can destroy the cell walls of bacteria, thereby achieving the purpose of antibacterial. Copper ions have the effect of inhibiting bacterial growth and reproduction, and have good antibacterial effects on a variety of bacteria.

[0003] In order to further improve the antibacterial effect, the method of combining silver and copper to form bimetallic nanoparticles was explored. Silver-copper bimetallic nanoparticles combine the antibacterial advantages of silver and copper, and enhance the ability to inhibit bacteria through synergistic effects. In addition, bimetallic nanoparticles also have higher stability and lower toxicity, making their application in the antibacterial field more promising.

[0004] At present, the methods for preparing silver-copper bimetallic nanoparticles include synchronous precipitation, sequential precipitation and assisted reduction. The synchronous precipitation method forms silver-copper bimetallic nanoparticles by introducing silver and copper salts into the solution at the same time, and then reducing or precipitating them simultaneously through a reducing agent or a precipitant. The sequential precipitation method forms silver-copper bimetallic nanoparticles by first preparing nanoparticles of one of the metals and then depositing another metal on its surface. Although silver-copper bimetallic nanoparticles have excellent antibacterial properties, there are still some challenges in their preparation process. Precisely controlling the size, shape and distribution of bimetallic nanoparticles remains a technical challenge. In addition, nanoparticles may agglomerate or mutate during long-term use, affecting the stability of their antibacterial properties.

[0005] Based on the above technical background, the present invention aims to develop a method for synthesizing antibacterial metal nanoparticles by green plants with certain commercial application prospects. Summary of the invention

[0006] Based on the problems existing in the background technology, the present invention provides a preparation of bimetallic nanoparticles with antibacterial function. By using plants to prepare a reducing solution, a green, simple and fast synthesis of bimetallic nanoparticles with antibacterial function can be achieved. The bimetallic nanoparticles are uniform in size and not easy to agglomerate, and can be directly used as an antibacterial material to kill bacteria or fungi.

[0007] The present invention is implemented by the following technical solutions:

[0008] The first aspect of the present invention discloses a method for preparing bimetallic nanoparticles with antibacterial function, comprising the following steps:

[0009] (1) preparing a green reducing solution;

[0010] (2) transferring the green reducing solution in step (1) to a reactor, immediately adding silver and copper metal salt stock solutions, stirring with a magnetic stirrer and heating to boiling;

[0011] (3) stopping heating, and waiting for the reactor temperature to drop to room temperature, continuing to add the green reducing solution in step (1), and continuing to stir the reaction to obtain a mixture;

[0012] (4) Centrifuging the mixture in step (3) at high speed, collecting the precipitate, washing and drying to obtain the bimetallic nanoparticles with antibacterial function.

[0013] Furthermore, the preparation method of the green reducing liquid in step (1) is specifically as follows: the plant to be extracted is washed and dried, deionized water is added to extract the juice, the obtained juice is placed in a magnetic stirrer and heated to boil, and maintained for 5-20 minutes, and when the temperature drops to room temperature, the precipitate is removed by centrifugation, and the supernatant is collected to obtain the green reducing liquid.

[0014] Furthermore, the plant to be extracted is any one or more of lemon peel, lemon seed, lemon pulp, orange peel, and orange pulp.

[0015] Furthermore, the mass ratio of the plant to be extracted to deionized water is (5-30):100.

[0016] Furthermore, in step (2), the silver and copper metal salt stock solutions are both water-soluble salt stock solutions, and the total concentration of the silver and copper metal ions is 10-40 mM.

[0017] Furthermore, the molar ratio of silver to copper elements in the silver and copper metal salt stock solutions is (1-10): (1-10).

[0018] Furthermore, in step (2), the volume ratio of the reducing solution to the stock solutions of the two metal salts of silver and copper is (50-200):(1-20).

[0019] Furthermore, the volume ratio of the amount of the green reducing solution added in step (3) to the amount of the green reducing solution in step (2) is (0.05-0.2):1.

[0020] The second aspect of the present invention discloses antibacterial bimetallic nanoparticles prepared by the preparation method of the above-mentioned antibacterial bimetallic nanoparticles, characterized in that the antibacterial bimetallic nanoparticles are a core-shell structure, and the particle size of the antibacterial bimetallic nanoparticles is 10-100nm.

[0021] The third aspect of the present invention discloses the application of the above-mentioned bimetallic nanoparticles with antibacterial function, wherein the bimetallic nanoparticles with antibacterial function are directly used as antibacterial materials to kill bacteria or fungi.

[0022] Beneficial effects of the present invention:

[0023] 1. In the present invention, plants are used to prepare the reducing solution, and the high performance of proteins, enzymes and other biological molecules secreted by plants, such as redox and catalysis, can be used to achieve green, simple and fast synthesis of bimetallic nanoparticles with antibacterial function. The preparation method is simple, energy-saving and highly efficient, and is a green and environmentally friendly synthesis route.

[0024] 2. The silver-copper bimetallic nanoparticles prepared by the present invention are uniform in size, well dispersed, and not easy to agglomerate. The silver and copper metals coexist with silver and copper ions in the prepared bimetallic nanoparticles, and have a synergistic antibacterial effect. The silver-copper bimetallic nanoparticles prepared by the present invention belong to a core-shell structure. Silver, as the outer shell part, not only provides excellent antibacterial performance, but also plays a role in protecting the internal copper core. Silver ions have a broad spectrum of antibacterial activity and can effectively destroy the cell wall of bacteria, thereby achieving a rapid sterilization effect; the internal copper core plays a role in supporting and stabilizing the structure. Copper itself also has antibacterial ability, especially at low concentrations, it can continuously inhibit bacterial growth and reproduction. By placing copper in the core position, the overall stability of the nanoparticles can be ensured, and a continuous and long-term antibacterial effect can be achieved. The use of silver-copper bimetallic saves the amount of silver used, reduces costs, and maintains efficient antibacterial performance. It belongs to a new generation of nano antibacterial materials that can replace nano silver. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings are used to provide further explanation of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0026] Figure 1 The particle size distribution result of the silver-copper bimetallic nanoparticles prepared in Example 1;

[0027] Figure 2 is a SEM image of the silver-copper bimetallic nanoparticles prepared in Example 1;

[0028] Figure 3 This is a graph showing the coliform bacteria count results of the silver-copper bimetallic nanoparticle antibacterial experiment prepared in Example 1;

[0029] Figure 4 This is the coliform bacteria test piece counting result diagram of the control group antibacterial experiment;

[0030] Figure 5This is a comparison chart of the sterilization efficiency of the silver-copper bimetallic nanoparticles prepared in Example 1, the silver nanoparticles prepared in Comparative Example 1, and the copper nanoparticles prepared in Comparative Example 2;

[0031] Figure 6 This is a comparison chart of the sterilization efficiency of silver-copper bimetallic nanoparticles with different concentrations. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the following embodiments.

[0033] Example 1

[0034] The preparation of silver-copper bimetallic nanoparticles with antibacterial function comprises the following steps:

[0035] (1) Preparation of green reducing solution:

[0036] 40g of dried lemon peel (dried at room temperature for two weeks) was added to 200mL of deionized water to extract the juice, and the obtained juice was placed in a magnetic stirrer and heated to boil for 20 minutes. When the temperature dropped to room temperature, the precipitate was removed by centrifugation, and the supernatant was collected to obtain a green reduced solution;

[0037] (2) 150 mL of the green reducing solution in step (1) was transferred to the reactor, and 10 mL of CuSO4 and AgCl stock solutions were immediately added (the molar ratio of Cu element to Ag element in the stock solution was 1:1, and the corresponding actual added concentration was 15 mM), and the mixture was heated to boiling with magnetic stirring for 5 min;

[0038] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0039] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0040] Figure 1 This is the particle size distribution result of the silver-copper bimetallic nanoparticles prepared in this example. It can be seen from the figure that the particle size of the silver-copper bimetallic nanoparticles is 10-100nm.

[0041] Figure 2 This is the SEM image of the silver-copper bimetallic nanoparticles prepared in this example. It can be seen from the figure that the particle size of the silver-copper bimetallic nanoparticles is 10-100nm, which is consistent with the particle size distribution result. The nanoparticles are uniform in size and are not agglomerated together.

[0042] Example 2

[0043] The preparation of silver-copper bimetallic nanoparticles with antibacterial function comprises the following steps:

[0044] (1) Preparation of green reducing solution:

[0045] Wash and dry 50g of dried lemon peel (dry at room temperature for two weeks), add 200mL of deionized water to squeeze the juice, stir the obtained juice in a magnetic stirrer and heat to boil for 20min, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reduced solution;

[0046] (2) 150 mL of the green reducing solution in step (1) was transferred to the reactor, and 10 mL of CuSO4 and AgCl stock solutions were immediately added (the molar ratio of Cu element to Ag element in the stock solution was 1:1, and the corresponding actual added concentration was 15 mM), and the mixture was heated to boiling with magnetic stirring for 5 min;

[0047] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0048] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0049] Example 3

[0050] The preparation of silver-copper bimetallic nanoparticles with antibacterial function comprises the following steps:

[0051] (1) Preparation of green reducing solution:

[0052] Wash and dry 40g of dried lemon peel (dry at room temperature for two weeks), add 200mL of deionized water to squeeze the juice, stir the obtained juice in a magnetic stirrer and heat to boil for 20min, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reduced solution;

[0053] (2) 150 mL of the green reducing solution in step (1) was transferred to the reactor, and 10 mL of CuSO4 and AgCl stock solutions were immediately added (the molar ratio of Cu element to Ag element in the stock solution was 1:1, and the corresponding actual added concentration was 20 mM), and the mixture was heated to boiling with magnetic stirring for 5 min;

[0054] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0055] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0056] Example 4

[0057] The preparation of silver-copper bimetallic nanoparticles with antibacterial function comprises the following steps:

[0058] (1) Preparation of green reducing solution:

[0059] Wash and dry 40g of dried lemon peel (dry at room temperature for two weeks), add 200mL of deionized water to squeeze the juice, stir the obtained juice in a magnetic stirrer and heat to boil for 20min, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reduced solution;

[0060] (2) 150 mL of the green reducing solution in step (1) was transferred to the reactor, and 10 mL of CuSO4 and AgCl stock solutions were immediately added (the molar ratio of Cu element to Ag element in the stock solution was 2:1, and the corresponding actual added concentration was 15 mM), and the mixture was heated to boiling with magnetic stirring for 5 min;

[0061] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0062] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0063] Example 5

[0064] The preparation of silver-copper bimetallic nanoparticles with antibacterial function comprises the following steps:

[0065] (1) Preparation of green reducing solution:

[0066] Wash and dry 40g of dried lemon peel (dry at room temperature for two weeks), add 200mL of deionized water to squeeze the juice, stir the obtained juice in a magnetic stirrer and heat to boil for 20min, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reduced solution;

[0067] (2) 150 mL of the green reducing solution in step (1) was transferred to the reactor, and 10 mL of CuSO4 and AgCl stock solutions were immediately added (the molar ratio of Cu element to Ag element in the stock solution was 1:2, and the corresponding actual added concentration was 15 mM), and the mixture was heated to boiling with magnetic stirring for 5 min;

[0068] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0069] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0070] Comparative Example 1

[0071] The preparation of silver nanoparticles comprises the following steps:

[0072] (1) Preparation of green reducing solution:

[0073] Wash and dry 40g of dried lemon peel (dry at room temperature for two weeks), add 200mL of deionized water to squeeze the juice, stir the obtained juice in a magnetic stirrer and heat to boil for 20min, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reduced solution;

[0074] (2) Transfer 150 mL of the green reducing solution in step (1) to the reactor, immediately add 10 mL of AgCl stock solution, stir magnetically and heat to boiling for 5 min;

[0075] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0076] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0077] Comparative Example 2

[0078] The preparation of copper nanoparticles comprises the following steps:

[0079] (1) Preparation of green reducing solution:

[0080] Wash and dry 40g of dried lemon peel (dry at room temperature for two weeks), add 200mL of deionized water to squeeze the juice, stir the obtained juice in a magnetic stirrer and heat to boil for 20min, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reduced solution;

[0081] (2) 150 mL of the green reducing solution in step (1) was transferred to the reactor, and 10 mL of CuSO4 stock solution was immediately added, and the mixture was heated to boiling with magnetic stirring for 5 min;

[0082] (3) Stop heating, wait until the reactor temperature drops to room temperature, continue to add 10 mL of the green reducing solution in step (1), and continue to stir the reaction to obtain a mixture;

[0083] (4) The mixture in step (3) was centrifuged at 10000 rpm for 10 min, the precipitate was collected, washed with anhydrous ethanol 5 times, and dried in a vacuum dryer for 2 h to obtain bimetallic nanoparticles with antibacterial function.

[0084] Test example

[0085] Antibacterial Experiment of Silver-Copper Bimetallic Nanoparticles

[0086] In this test example, a natural lake water sample at 0°C was used to count the total number of bacteria using a coliform test piece (produced by 3M Petrifilm). The total number of bacteria in the water sample was compared between the water sample with the silver-copper bimetallic nanoparticles prepared in Example 1 of the present invention and the water sample without the addition of nanoparticles. The results are as follows: Figure 3 , 4 shown. Figure 3 The test sample with 30 ppm of the prepared Ag-Cu nanoparticles added did not show any presence of E. coli, while the control group ( Figure 4 ) The total number of bacteria was about 225 / ml, and the antibacterial rate of the green synthesized Ag-Cu bimetallic nanoparticles reached 100%.

[0087] Bacterial removal comparison experiment of silver-copper bimetallic nanoparticles, silver nanoparticles and copper nanoparticles

[0088] Take a fresh natural water sample, dilute it five times, add 30 mg / L of copper nanoparticles (Comparative Example 2), silver nanoparticles (Comparative Example 1), and copper-silver bimetallic nanoparticles (Example 1), respectively, mix them thoroughly, and then use a sterile cotton swab to evenly apply the mixture on Petrifilm bacteria counting test paper. After culturing in a dry incubator for 48 hours, count the bacteria and calculate the removal rate.

[0089] Figure 5 This is a comparison chart of the sterilization efficiency of the silver-copper bimetallic nanoparticles prepared in Example 1, the silver nanoparticles prepared in Comparative Example 1, and the copper nanoparticles prepared in Comparative Example 2. According to the antibacterial performance, the antibacterial performance of the copper-silver bimetallic nanoparticles is stronger than the other two.

[0090] Comparative experiment on sterilization of silver-copper bimetallic nanoparticles with different concentrations

[0091] Take a fresh natural water sample, dilute it five times, add 5ppm, 10ppm, 15ppm copper-silver bimetallic nanoparticles (Example 1) respectively, mix them thoroughly, and then use a sterile cotton swab to evenly apply the mixture on Petrifilm bacteria counting test paper. After incubating in a dry incubator for 24 hours, count the bacteria and calculate the removal rate.

[0092] Figure 6 The antibacterial performance of total bacteria in natural lake water sources was analyzed, and the results showed the antibacterial test results of Ag / Cu nanoparticles at different doses (5ppm, 10ppm, 15ppm) after 24 hours. All the above tests were repeated three times. As can be seen from the figure, the antibacterial efficiency of all samples with Ag / Cu nanoparticles is as high as nearly 70%, and the antibacterial efficiency increases with the increase of Ag / Cu nanoparticle dosage. Among them, the total bacterial inhibition rate is as high as 100% when 15ppm of Ag / CuNP is added.

[0093] Finally, it should be noted that the above-mentioned embodiments only express several implementation methods of the present invention and are not intended to limit the invention. For those skilled in the art, any modification, equivalent replacement, improvement, etc. made without departing from the concept of the present invention should be included in the protection scope of the invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing bimetallic nanoparticles with antibacterial function, characterized in that: The following steps are involved: (1) preparing a green reducing solution; (2) transferring the green reducing solution in step (1) to a reactor, immediately adding silver and copper metal salt stock solutions, stirring with a magnetic stirrer and heating to boiling; (3) stopping heating, and waiting for the reactor temperature to drop to room temperature, continuing to add the green reducing solution in step (1), and continuing to stir the reaction to obtain a mixture; (4) Centrifuging the mixture in step (3) at high speed, collecting the precipitate, washing and drying to obtain the bimetallic nanoparticles with antibacterial function.

2. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 1, characterized in that: The preparation method of the green reducing liquid in step (1) is specifically as follows: wash and dry the plant to be extracted, add deionized water to squeeze the juice, place the obtained juice in a magnetic stirrer and stir and heat to boil, keep it for 5-20 minutes, wait until the temperature drops to room temperature, centrifuge to remove the precipitate, collect the supernatant, and obtain the green reducing liquid.

3. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 2, characterized in that: The plant to be extracted is any one or more of lemon peel, lemon seed, lemon pulp, orange peel and orange pulp.

4. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 2, characterized in that: The mass ratio of the plant to be extracted to deionized water is (5-30):

100.

5. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 1, characterized in that: In step (2), the silver and copper metal salt solutions are both water-soluble salt solutions, and the total concentration of the silver and copper metal ions is 10-40 mM.

6. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 5, characterized in that: The molar ratio of silver to copper elements in the silver and copper metal salt stock solutions is (1-10): (1-10).

7. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 1, characterized in that: In step (2), the volume ratio of the reducing solution to the stock solutions of the two metal salts of silver and copper is (50-200):(1-20).

8. The method for preparing bimetallic nanoparticles with antibacterial function according to claim 1, characterized in that: The volume ratio of the green reducing solution added in step (3) to the green reducing solution in step (2) is (0.05-0.2):

1.

9. A bimetallic nanoparticle with antibacterial function prepared by the method for preparing bimetallic nanoparticle with antibacterial function as claimed in any one of claims 1 to 8, characterized in that: The bimetallic nanoparticles with antibacterial function are of a core-shell structure, and the particle size of the bimetallic nanoparticles with antibacterial function is 10-100 nm.

10. An application of the bimetallic nanoparticles with antibacterial function as claimed in claim 9, characterized in that: The bimetallic nanoparticles with antibacterial function are directly used as antibacterial materials to kill bacteria or fungi.

Citation Information

Cited By

  • Cu-Ag / SiO2-coated PDMS composite antibacterial osseointegration promoting coating as well as preparation method and application thereof

    CN121648352A