Injectable hydrogel rapidly prepared at normal temperature based on binary assembly of lipoic acid as well as preparation method and application of injectable hydrogel
By using the combination of lipoic acid, polyhydroxyalcoamine and metal ions in bioadhesives, a rapid gelation hydrogel is formed, which solves the problem of long preparation time of existing lipoic acid and achieves anti-inflammatory and anti-inflammatory and sterilization. The effect has enhanced the application value of bioadhesives.
Patent Information
- Application Number
- CN202410933831.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-29
AI Technical Summary
The existing lipoic acid has a long preparation time and complicated steps when preparing bioadhesives, which limits its application in the field of bioadhesives.
Using a rapid preparation method for binary assembly based on lipoic acid, the gelation time is shortened by adding ferrous ions or magnesium ions to the gel system, and the three-dimensional effect is formed by carboxyl and hydrogen bonding of lipoic acid and polyhydroxy alcoholamine. The network structure, combined with the anti-inflammatory and bactericidal effect of metal ions, prepares an injectable hydrogel.
It has achieved rapid preparation of lipoic acid in the field of bioadhesives, has the functions of anti-inflammatory and scavenging reactive oxygen radicals, promotes tissue healing and repair, simplifies the preparation process, and has significant medical application value.
Smart Images

Figure CN119033990A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bioadhesives, and in particular to an injectable hydrogel rapidly prepared at room temperature by binary assembly based on lipoic acid, and a preparation method and application thereof. Background Art
[0002] The development of human society is inseparable from human activities. Many activities that humans engage in are prone to cause body dysfunction. The most common is physical injury, such as skin trauma, tissue contusion, bone fracture, etc. In the field of biomedicine, the treatment of physical injuries mainly includes hemostasis, wound closure, surgical repair, and reconstruction of damaged or degenerated soft tissue. The treatment of hemostasis and wound healing can be traced back to ancient times, when humans knew to use leaves of natural plants as dressings to treat wounds. With the progress of human civilization and the development of science and technology, bioadhesives have come into everyone's field of vision as a kind of material with excellent biocompatibility and will not cause secondary trauma to the wound to avoid wound infection. Bioadhesives have an extremely broad range of applications in wound healing tissue trauma.
[0003] Lipoic acid (LA) is a natural disulfide compound that exists in mitochondria. It is similar to vitamins and is a growth factor for some microorganisms. It can eliminate free radicals that accelerate aging and cause disease. Lipoic acid is the most effective known natural antioxidant and can regenerate endogenous antioxidants. Lipoic acid enters cells after being absorbed through the intestines. It has both fat-soluble and water-soluble properties, so it can pass through the body unimpeded and reach any cell part, providing comprehensive effectiveness to the human body. It is a "universal antioxidant" that is both fat-soluble and water-soluble. Lipoic acid has been used clinically for more than 30 years. It was first used as a prescription drug in Germany and has been widely used in the fields of diabetes, neurology, and cardiology. At the same time, lipoic acid is also a therapeutic drug for burning mouth syndrome and has a significant therapeutic effect on it.
[0004] As a clinical drug, lipoic acid can eliminate oxygen free radicals (ROS) and has anti-inflammatory effects. Using it as an adhesive can effectively protect tissue wounds and prevent infection. Lipoic acid itself also has anti-inflammatory effects and is widely used in the preparation of bioadhesives. At present, there are extensive reports on lipoic acid, mainly based on the fact that the disulfide bond of lipoic acid is a dynamic chemical bond with chemical response, thermal response and light response to form polylipoic acid. However, these steps take a long time to prepare and the preparation method is cumbersome, which to some extent limits the application of lipoic acid in the field of bioadhesives.
[0005] Therefore, there is an urgent need to develop a simple, efficient, and biochemically functional lipoic acid-based bioadhesive, so that lipoic acid has a greater application prospect in the field of bioadhesives. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide an injectable hydrogel based on lipoic acid that is rapidly prepared at room temperature by binary assembly and a preparation method and application thereof. By adding a certain amount of ferrous ions or magnesium ions to the gel system, the occurrence time of the gelation phenomenon is shortened. At the same time, trace amounts of metal ions have a certain anti-inflammatory and bactericidal effect on wounds, and can work synergistically with lipoic acid to jointly promote tissue healing and repair.
[0007] The purpose of the present invention can be achieved by the following technical solutions: The present invention provides an injectable hydrogel that is rapidly prepared at room temperature based on binary assembly of lipoic acid, wherein the injectable hydrogel comprises lipoic acid and polyhydroxy alcohol amine molecules; The polyhydroxy alcohol amine molecule is tromethamine, and the molar ratio of lipoic acid to tromethamine is (1.6-1.2):1.
[0008] Furthermore, the polyhydroxy alcohol amine molecules also include one of triethanolamine and triisopropanolamine.
[0009] Furthermore, the mass concentration of the lipoic acid is 50%.
[0010] Furthermore, the deprotonated carboxyl group of the lipoic acid interacts with the protonated amino group and the adjacent hydroxyl group of the polyhydroxylamine molecule simultaneously, and through the hydrogen bonding with the carboxyl group, one end of multiple lipoic acid molecules are connected, and the dithiolane ring at the other end forms a physical cross-linking point through hydrophobic aggregation, thereby synergistically constructing a three-dimensional network structure with the polyhydroxylamine molecules to form a hydrogel structure.
[0011] The present invention also provides a method for preparing an injectable hydrogel that is rapidly prepared at room temperature based on binary assembly of lipoic acid. At room temperature, polyhydroxy alcohol amine molecules and metal ions are sequentially added to deionized water, and then lipoic acid is added and shaken to obtain a mixed solution, which is allowed to stand to obtain the injectable hydrogel.
[0012] Furthermore, the metal ions are reducing metal ions, and the reducing metal ions include Fe 2+ Mg 2+ .
[0013] Furthermore, the added amount of the metal ions is 0.1%-1% by mass concentration.
[0014] Furthermore, the standing time is 20-40s.
[0015] Furthermore, the thiol group in the lipoic acid can chelate metal ions to form a complex.
[0016] The present invention also provides an application of an injectable hydrogel rapidly prepared at room temperature based on binary assembly of lipoic acid, wherein the injectable hydrogel is used for wound repair.
[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The present invention can shorten the occurrence time of gelation by adding a certain amount of ferrous ions or magnesium ions into the gel system, and the ferrous ions or magnesium ions have a certain bactericidal effect.
[0018] 2. The preparation process of the present invention is simple, and the prepared injectable hydrogel has the functions of anti-inflammatory and scavenging active oxygen free radicals. Trace amounts of metal ions have certain anti-inflammatory and bactericidal effects on wounds, and can work synergistically with lipoic acid to jointly promote tissue healing and repair, and has great medical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a schematic diagram of the gelation state in Comparative Example 3; Figure 2 This is a schematic diagram of the gelation state in Example 1; Figure 3 This is a schematic diagram of the gelation state in Comparative Example 1; Figure 4 For example 3 without Fe 2+ After standing for 40 seconds, invert and add Fe 2+ Schematic diagram of the inverted flow state after standing for 40 seconds; Figure 5 Schematic diagram of the extrusion of the injectable hydrogel in Example 1 and Example 3; Figure 6 The relationship between modulus and time in the system of 20% tromethamine and 50% 1a in Example 1; Figure 7 Whether Mg 2+ Relationship between frequency of content and storage modulus and loss modulus; Figure 8 For different Mg 2+ Relationship between frequency of content and storage modulus and loss modulus; Fig. 9 For different Mg 2+ Oscillatory strain scan of content; Fig.10 For different Mg 2+ Viscosity-shear rate relationship diagram of the content. DETAILED DESCRIPTION
[0020] The specific implementation methods of the present invention are described in detail below through examples. These examples are implemented on the premise of the scheme described in the present invention, and provide detailed implementation methods and specific operating processes, but the protection scope of the present invention is not limited to the following examples.
[0021] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. Any features such as component models, material names, connection structures, preparation methods, materials, structures or composition ratios not clearly described in this technical solution are deemed to be common technical features disclosed in the prior art. Example 1
[0022] This embodiment provides an injectable hydrogel rapidly prepared at room temperature by binary assembly based on lipoic acid, wherein the injectable hydrogel comprises lipoic acid and polyhydroxy alcohol amine molecules. The polyhydroxy alcohol amine molecules comprise one of tromethamine, triethanolamine, and triisopropanolamine, and the mass concentration of lipoic acid is 50%.
[0023] The carboxyl group of lipoic acid interacts with the amino group and the hydroxyl group of the alkaline polyhydroxylamine molecule through hydrogen bonding, and the hydrophobic aggregation of the dithiolane ring of lipoic acid, and together they form a binary assembly. Lipoic acid has carboxyl and dithiolane functional groups, and its deprotonated carboxyl group interacts with the protonated amino group and the adjacent hydroxyl group of the alkaline polyhydroxylamine molecule, such as tromethamine, at the same time. When the content of tromethamine is low, tromethamine with multiple hydrogen bond donor functional groups acts as a small molecule cross-linking agent, and connects with multiple lipoic acid molecules through hydrogen bonding with the carboxyl group. At the same time, the dithiolane ring at the other end of the lipoic acid molecule forms a physical cross-linking point through hydrophobic aggregation, thereby synergistically constructing a three-dimensional network structure with tromethamine. Due to the hydrophobic aggregation of the dithiolane ring, the local dithiolane concentration is high, which is accompanied by a disulfide bond exchange reaction. When the content of tromethamine is high, the tromethamine molecule can achieve the dispersion of lipoic acid in water by interacting with multiple sites of lipoic acid (including the dithiolane ring). The thiol group in lipoic acid can chelate metal ions to form complexes, which improves the mechanical properties of hydrogels. Adding strong reducing metal ions to the system can accelerate gelation, and the metal ions give the system biochemical activity, which can effectively kill bacteria and promote wound repair.
[0024] This embodiment also provides an application of an injectable hydrogel that is rapidly prepared at room temperature based on binary assembly of lipoic acid. The injectable hydrogel is used in the preparation process of bioadhesives and in wound repair.
[0025] This embodiment also provides a method for preparing an injectable hydrogel based on lipoic acid binary assembly and rapid preparation at room temperature, comprising the following steps: Add 0.2g tromethamine (Tris base) and 50mg magnesium sulfate to 1ml deionized water and shake until completely dissolved. Add 0.5g lipoic acid to the prepared tromethamine solution and shake to dissolve. Pour the prepared lipoic acid and tromethamine solution into a syringe and let it stand for 20-40s to gel, thereby obtaining an injectable hydrogel.
[0026] like Figure 2 As shown by Figure 2 As shown in (c) and (d), in the system with the addition of magnesium ions, most of the lipoic acid particles were dissolved and showed a good gelation state after one minute. Figure 5 (a) is a diagram of the extrusion state of the configured injectable hydrogel. It can be seen from the figure that the injectable hydrogel prepared in this embodiment has good extrudability.
[0027] Figure 6 20wt.% tromethamine and 50wt.% lipoic acid modulus versus time, G' is the storage modulus, G" is the loss modulus. As can be seen from the figure, the storage modulus of 20wt.% tromethamine and 50wt.% lipoic acid gradually increases with the passage of time, indicating that the injectable hydrogel prepared in this example can exhibit rapid gelation in a short time.
[0028] Figure 7 Whether Mg 2+ The relationship between the frequency of the content and the storage modulus and loss modulus is shown in FIG. The red curve is the injectable hydrogel prepared in this embodiment, and the black curve is the hydrogel prepared in Comparative Example 4. As can be seen from the figure, the storage modulus of the hydrogel prepared by adding magnesium ions to 20 wt.% of tromethamine and 50 wt.% of lipoic acid is significantly higher than that prepared in Comparative Example 4, which shows that the participation of surface metal ions is conducive to the binary assembly of lipoic acid.
[0029] Figure 8 For different Mg 2+ The relationship between the frequency of the content and the storage modulus and loss modulus is shown in FIG. 1 , wherein the blue curve is the injectable hydrogel prepared in this example, the black curve is the injectable hydrogel prepared in Example 8, and the red curve is the injectable hydrogel prepared in Example 9. Figure 8 It can be seen that with the increase of Mg 2+ The storage modulus of the hydrogel increased with the increase of 1% Mg 2 + The storage modulus of the hydrogel was the highest, which was mainly due to the fact that lipoic acid could chelate metal ions to form complexes, thus improving the mechanical properties of the hydrogel. In addition, all groups showed the rheological properties of solid hydrogels, with storage moduli greater than the corresponding loss modulus (i.e., G′>G′′), showing elastic solidity.
[0030] Fig. 9For different Mg 2+ The blue curve is the injectable hydrogel prepared in this example, the black curve is the injectable hydrogel prepared in Example 9, and the red curve is the injectable hydrogel prepared in Example 8. Fig. 9 It can be seen that in the strain scan with a frequency of 1 Hz, when the shear strain increases from 0.01% to 1050%, the sample changes from a more elastic solid state to a more viscous flow state as the shear strain increases; Fig.10 For different Mg 2+ The viscosity-shear rate relationship diagram of different Mg contents at 1% strain is compared. 2+ The viscosity-shear rate relationship of the hydrogel material with the content of 1.5 wt %. The blue curve is the injectable hydrogel prepared in Example 8, the black curve is the injectable hydrogel prepared in Example 9, and the red curve is the injectable hydrogel prepared in this example. As the shear rate increases from 0.001 s -1 Gradually increase to 100 s -1 , the viscosity of the samples showed a downward trend, showing shear thinning. Stable and continuous shear destroyed the interaction inside the hydrogel, allowing it to flow. In addition, the hydrogel has thixotropic properties and typical shear-induced gel-fluid transition behavior, which is crucial for injectable hydrogels. Example 2
[0031] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: Add 0.2g triethanolamine and 50mg magnesium sulfate to 1ml deionized water and shake until completely dissolved. Add 0.5g lipoic acid (la) to the prepared triethanolamine solution and shake to dissolve. Pour the prepared lipoic acid and triethanolamine solution into a syringe and let it stand for 20-40s to gel, and then squeeze out the gelled hydrogel. Example 3
[0032] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: Add 0.2g tromethamine and 50mg ferrous chloride to 1ml deionized water and shake until completely dissolved to prepare a 20% tromethamine solution. Add 0.5g lipoic acid to the prepared tromethamine solution and shake to dissolve. Pour the prepared lipoic acid and triethanolamine solution into a syringe and let it stand for 20-40s to gel, and then squeeze out the gelled hydrogel. Figure 4 As shown, Figure 4 (a) is the flow state diagram of the inverted state after the ferrous ion is shaken evenly and then left to stand for 40 seconds. Figure 4(b) is the flow state diagram of the inverted solution after adding ferrous ions and shaking and standing for 40 seconds. It can be seen from the figure that the solution shows gelation after adding ferrous ions. Figure 5 (b) is a diagram of the extrusion state of the configured injectable hydrogel. It can be seen from the figure that the injectable hydrogel prepared in this example has good extrudability. Example 4
[0033] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.2g triisopropanolamine and 50mg magnesium sulfate are added to 1ml deionized water and shaken until completely dissolved, and 0.5g lipoic acid is added to the prepared triisopropanolamine solution and shaken to dissolve. The prepared lipoic acid and triisopropanolamine solution is poured into a syringe and allowed to stand for one minute to gel, and the gelled hydrogel can be squeezed out. Example 5
[0034] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.18g tromethamine and 50mg magnesium sulfate in 1ml deionized water were shaken until completely dissolved, and 0.5g lipoic acid was added to the prepared triethanolamine solution and shaken to dissolve. The prepared lipoic acid and tromethamine solution was poured into a syringe and allowed to stand for 20-40s to gel, thereby obtaining an extrudable gelled hydrogel. Example 6
[0035] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.2g triethanolamine and 50mg ferrous chloride were added to 1ml deionized water and shaken until completely dissolved, and 0.5g lipoic acid was added to the prepared triethanolamine solution and shaken to dissolve. The prepared lipoic acid and triethanolamine solution was poured into a syringe and allowed to stand for 20-40s to gel, thereby obtaining an extrudable gelled hydrogel. Example 7
[0036] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.25 g of tromethamine and 100 mg of magnesium sulfate were added to 1 ml of deionized water and shaken until completely dissolved, and 0.5 g of lipoic acid was added to the prepared triethanolamine solution and shaken to dissolve. The prepared lipoic acid and tromethamine solution was poured into a syringe and allowed to stand for 20-40 seconds to gel, thereby obtaining an extrudable gelled hydrogel. Example 8
[0037] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.2g tromethamine and 100mg magnesium sulfate were added to 1ml deionized water and shaken until completely dissolved, and 0.5g lipoic acid was added to the prepared triethanolamine solution and shaken to dissolve. The prepared lipoic acid and tromethamine solution was poured into a syringe and allowed to stand for 20-40s to gel, thereby obtaining an extrudable gelled hydrogel. Example 9
[0038] This embodiment provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.2g tromethamine and 10mg magnesium sulfate were added to 1ml deionized water and shaken until completely dissolved, and 0.5g lipoic acid was added to the prepared triethanolamine solution and shaken to dissolve. The prepared lipoic acid and tromethamine solution was poured into a syringe and allowed to stand for 20-40s to gel, thereby obtaining an extrudable gelled hydrogel.
[0039] Comparative Example 1 This comparative example provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.3g of tromethamine and 50mg of magnesium sulfate were dissolved in 1ml of deionized water and shaken until completely dissolved. 0.5g of lipoic acid was added to the prepared tromethamine solution and shaken to dissolve. It was found that in this system, lipoic acid could not be completely dissolved in the system and could not gel. Figure 3 As shown by Figure 3 As shown in (e) and (f), when the content of tromethamine was increased to 30%, lipoic acid was completely dissolved, but no rapid gelation occurred after five minutes.
[0040] Comparative Example 2 This comparative example provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: 0.16 g of tromethamine and 50 mg of magnesium sulfate were dissolved in 1 ml of deionized water and shaken until completely dissolved, and 0.5 g of lipoic acid was added to the prepared tromethamine solution and shaken to dissolve. It was found that the system was filled with a large number of lipoic acid particles that could not be dissolved.
[0041] Comparative Example 3 This comparative example provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: Dissolve 0.16g of tromethamine and 50mg of magnesium sulfate in 1ml of deionized water and shake until completely dissolved. Add 0.25g of lipoic acid to the prepared tromethamine solution and shake until dissolved. After the lipoic acid in this system is dissolved, due to the low concentration of lipoic acid, no rapid gelation phenomenon occurs. Figure 1 As shown by Figure 1 (a) and (b) show that 16% tromethamine can also gel after one minute, but there are many undissolved lipoic acid particles.
[0042] Comparative Example 4 This comparative example provides a method for preparing an injectable hydrogel based on binary assembly of lipoic acid, comprising the following steps: Dissolve 0.2g of tromethamine in 1ml of deionized water and shake until completely dissolved, add 0.5g of lipoic acid to the prepared tromethamine solution and shake to dissolve. In this system, lipoic acid dissolves and gelation occurs after 5-10 minutes.
[0043] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. An injectable hydrogel based on lipoic acid binary assembly and rapidly prepared at room temperature, characterized in that: The injectable hydrogel includes lipoic acid and polyhydroxylamine molecules; The polyhydroxy alcohol amine molecule is tromethamine, and the molar ratio of lipoic acid to tromethamine is (1.6-1.2):
1.
2. The injectable hydrogel prepared rapidly at room temperature by binary assembly based on lipoic acid according to claim 1, characterized in that: The polyhydroxy alcohol amine molecules also include one of triethanolamine and triisopropanolamine.
3. The injectable hydrogel based on lipoic acid binary assembly and rapid preparation at room temperature according to claim 1, characterized in that: The mass concentration of the lipoic acid is 50%.
4. The injectable hydrogel based on lipoic acid binary assembly and rapid preparation at room temperature according to claim 1, characterized in that: The deprotonated carboxyl group of the lipoic acid interacts with the protonated amino group and the adjacent hydroxyl group of the polyhydroxy alcohol amine molecule simultaneously, and through the hydrogen bonding with the carboxyl group, one end of multiple lipoic acid molecules are connected, and the dithiolane ring at the other end forms a physical cross-linking point through hydrophobic aggregation, thereby synergistically constructing a three-dimensional network structure with the polyhydroxy alcohol amine molecules to form a hydrogel structure.
5. A method for preparing an injectable hydrogel rapidly prepared at room temperature based on binary assembly of lipoic acid as claimed in any one of claims 1 to 4, characterized in that: At room temperature, polyhydroxy alcohol amine molecules and metal ions are added to deionized water in sequence, and then lipoic acid is added and shaken to obtain a mixed solution, which is allowed to stand to obtain an injectable hydrogel.
6. The method for preparing an injectable hydrogel based on binary assembly of lipoic acid at room temperature and rapidly prepared according to claim 5, characterized in that: The metal ions are reducing metal ions, including Fe 2+ Mg 2+ .
7. The method for preparing an injectable hydrogel based on binary assembly of lipoic acid at room temperature and rapidly prepared according to claim 5, characterized in that: The added amount of the metal ions is 0.1%-1% by mass concentration.
8. The method for preparing an injectable hydrogel based on binary assembly of lipoic acid at room temperature and rapidly prepared according to claim 5, characterized in that: The standing time is 20-40s.
9. The method for preparing an injectable hydrogel based on binary assembly of lipoic acid at room temperature and rapidly prepared according to claim 5, characterized in that: The thiol group in the lipoic acid can chelate metal ions to form a complex.
10. An application of an injectable hydrogel rapidly prepared at room temperature by binary assembly based on lipoic acid as claimed in any one of claims 1 to 4, characterized in that: The injectable hydrogel is used for wound repair.
Citation Information
Cited By
Preparation method and application of organic-inorganic composite hydrogel with high mechanical adaptability and wet adhesion stability
CN121360278A
Method for preparing and application of organic-inorganic composite hydrogel with high mechanical adaptability and stable adhesion in wet state
CN121360278B
Long-acting injection preparation based on alpha-lipoic acid derivative as well as preparation method and application of long-acting injection preparation
CN121971369A