Method for investment casting of D5S high-nickel austenite nodular cast iron

By optimizing the process and raw material ratio, the problems of poor fluidity and easy suction of high-nickel ductile iron are solved, and the stable production of D5S high-nickel austenite ductile iron is achieved, which avoids defects such as shrinkage and pores, and meets high performance Require.

CN119035449APending Publication Date: 2024-11-29BINZHOU ZHENGDAO MASCH MFG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411064723.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When the prior art produces ductile iron with high nickel, high silicon and low carbon content, problems such as poor fluidity and easy suction lead to the production of conventional processes that easily lead to defects such as shrinkage, pores, and cold separation, and high waste rate.

Method used

The wax type is made of medium-temperature wax, using a mixture of silicon sol and zircon powder as the shell surface material, and the mixture of silicon sol and mull powder as the transition layer and back layer material. The shell is roasted by natural gas, and pig iron and furnace refrigeration material are selected. , scrap steel, electrolytic nickel, high-carbon ferrochromium, and ferrosilicon are melted, and the casting temperature and incubation of the melted model shell are controlled, and the process conditions are optimized to produce D5S high Nickel austenite ductile iron.

Benefits of technology

Through process optimization and precise control of raw material ratio, defects such as shrinkage, pores, and cold separation are solved, spheroidization rate and mechanical properties are improved, and performance requirements of ASTM A439/A439M-18 standard are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035449A_ABST
    Figure CN119035449A_ABST
Patent Text Reader

Abstract

The invention relates to the field of casting of nodular cast iron made of special materials, and particularly discloses a method for investment casting of D5S high-nickel austenite nodular cast iron. The method comprises the following steps: (1) preparing a wax pattern by adopting medium-temperature wax, adopting a mixture of silica sol and zircon powder as a surface layer material of a shell, adopting a mixture of silica sol, mullite powder and fused quartz powder as a transition layer and back layer material of the shell, and drying and dewaxing to obtain a final shell; (2) roasting the shell by adopting a natural gas roasting furnace; (3) pig iron, foundry returns, waste steel, electrolytic nickel, high-carbon ferrochrome and ferrosilicon are selected as halogen materials and added into a smelting furnace to be smelted, and molten iron is obtained; (4) carrying out spheroidizing treatment on the molten iron by adopting a pouring-in method; (5) casting by adopting a secondary inoculation mode; and (6) during spheroidizing, the investment shell is taken out of the roasting furnace to be cast, and a product is obtained. According to the invention, through process optimization and accurate control of the raw material ratio, under the condition that the product spheroidization rate, the matrix structure stability and the mechanical property standard reaching are ensured, the problems of shrinkage porosity, air holes, cold shut and the like which are extremely easy to form in the conventional process production are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of special material ductile iron casting, and in particular to a method for investment casting of D5S high-nickel austenitic ductile iron. Background Art

[0002] D5S is a special ductile iron with high nickel, high silicon and low carbon content. This material has particularly high heat resistance, corrosion resistance and a small linear expansion coefficient. It is a key material for the production of turbine housings, exhaust pipes, turbocharger housings, high-precision parts, etc.; the nickel content is the highest among the known ductile iron materials, reaching 34-37%. At the same time, the high silicon and low carbon are exactly the opposite of the high carbon and low silicon of existing ductile iron. The requirements for element content cause the material to have extremely poor fluidity and easy air absorption. Conventional production processes are very likely to form defects such as shrinkage, pores, cold shut, and the scrap rate remains high. Summary of the invention

[0003] In order to make up for the deficiencies of the prior art, the present invention provides a method for investment casting D5S high-nickel austenitic ductile iron with optimized process, precise control of raw material ratio and stable product performance.

[0004] The present invention is achieved through the following technical solutions: A method for investment casting D5S high-nickel austenitic ductile iron comprises the following steps: (1) A wax mold is made using medium-temperature wax, a mixture of silica sol and zircon powder is used as the surface layer material of the mold shell, and zircon sand is used as the sanding material; a mixture of silica sol and mullite powder is used as the transition layer and back layer material of the mold shell, and mullite sand is used as the sanding material, and the final mold shell is obtained after drying and dewaxing; (2) Use a natural gas roasting furnace to roast the shell, cool it down in the furnace before spheroidization and then keep it warm; (3) Pig iron, recycled materials, scrap steel, electrolytic nickel, high carbon ferrochrome and ferrosilicon are selected as halogen materials and added into a smelting furnace for smelting to obtain molten iron; (4) Spheroidizing the molten iron by flushing method; (5) Adopting the secondary inoculation method, adding inoculant when tapping iron, and using secondary inoculation during casting; (6) During the spheroidization treatment, the molten model shell is taken out of the roasting furnace for casting to obtain the product.

[0005] The present invention optimizes the process conditions and treatment methods of each step through the steps of investment casting shell making, shell roasting, molten iron smelting, spheroidizing inoculation treatment, shell pouring, heat treatment, etc., and produces high-nickel austenitic ductile iron of special material by combining with investment casting.

[0006] A better technical solution of the present invention is: In step (1), the specific process of investment casting shell making is as follows: a) Add distilled water / purified water to the silica sol to adjust the mass concentration of silica to 27-28%, then slowly add the wetting agent and defoamer to the silica sol solution in sequence, then add zircon powder in batches, and continue stirring until uniform. The viscosity of the final silica sol slurry is measured with a No. 4 James cup to measure 30-45s; b) Soak the wax model in wax model cleaning agent and silica sol in sequence, then immerse it in silica sol slurry, take it out after it is completely immersed, blow the bubbles on the surface with compressed air, immerse it in silica sol slurry again, take it out after it is completely immersed, and then send it to the sand spraying machine to be covered with zircon sand. Hang the wax model covered with sand and dry it for 3-8 hours at a temperature of 23±3℃ and a breeze of 0.5-1m / s to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of silica sol and 180-250 mesh mullite powder to prepare the slurry. In the transition layer slurry, the weight ratio of mullite powder to silica sol is 1.2-2:1, and the drying time is 8-12h; in the back layer slurry, the weight ratio of mullite powder to silica sol is 1-1.5:1, and the drying time is 10-24h; in the sealing layer slurry, the weight ratio of mullite powder to silica sol is 0.8-1.2:1, and the drying time is 10-14h; the transition layer, back layer and sealing layer are all dried at a temperature of 23±3℃ and a breeze of 3-5m / s; d) In steps b)-c), the surface layer is made 1-2 times, the transition layer is made 1-2 times, the backing layer is made 2-8 times, the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 15-30 minutes, the dewaxing temperature is 150-170°C, the dewaxing pressure is 0.6-0.7MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds.

[0007] Further preferably, the silica sol is 830 type silica sol, the mass concentration of silicon dioxide is 30%, in step a), the volume ratio of distilled water / pure water to silica sol is 72-111:1000; the volume ratio of wetting agent, defoaming agent to silica sol is 1.2-1.7:0.7-1:1000; the mass ratio of zircon powder to silica sol is 3.2-4.5:1.

[0008] Further preferably, in step b), the wax mold is soaked in wax mold cleaning agent for 5-15s, hung up to drip off the liquid and then soaked in silica sol for 3-5s, hung up to drip off the liquid and then immersed in silica sol slurry until it is completely immersed and then taken out, 0.1-0.3MPa compressed gas is used to blow up the surface bubbles, immersed in silica sol slurry again until it is completely immersed and then taken out to control the slurry for 5-10s, and then sent to a sand spraying machine to be covered with 80-120 mesh zircon sand.

[0009] In step (2), the natural gas roasting temperature is 1050-1150°C, the roasting time is greater than 45 minutes, and the temperature is reduced to 850-950°C after roasting, and the temperature is kept constant for more than 10 minutes before casting.

[0010] In step (3), the pig iron is high-purity pig iron. Some impurity elements in the pig iron, such as lead, tin, tellurium, etc., have a strong interference effect on the formation of high-nickel austenitic ductile iron graphite, which will affect the spheroidization of the product. Therefore, high-purity pig iron is selected; the recycled materials are die heads or scrap materials made of high-nickel materials such as D5S. In order to reduce impurity interference and ensure spheroidization, other materials are not used. The recycled steel is high-quality carbon steel, containing only carbon, silicon, manganese and trace amounts of sulfur and phosphorus, and the rest is iron, without other elements, to avoid affecting spheroidization; the electrolytic nickel is NI99.99 high-purity electrolytic nickel; the high-carbon ferrochrome is FECr55; the ferrosilicon is FeSi75; the above-mentioned purchased raw materials are prohibited from having oil stains, mud blocks, plastics and other debris on the surface, and they are all shot blasted, derusted, dehydrated and dried before use; The weight ratio of the above raw materials is 20-30% of pig iron, 20-35% of recycled materials, 10-15% of scrap steel, 20-30% of electrolytic nickel, 1.8-3% of high carbon ferrochrome, and 4-6% of ferrosilicon.

[0011] Further preferably, pig iron is placed in a furnace body, scrap steel and recycled materials are added in sequence, and when the molten iron is melted to 60-80% of the capacity of the furnace and the temperature reaches 1450-1520°C, electrolytic nickel, high carbon ferrochrome and ferrosilicon are added to melt and samples are taken for component detection. Since D5S has a high melting point and the fluidity of the molten iron is very poor, the smelting temperature should be 100-150°C higher than that of normal ductile iron. When the temperature of the molten iron reaches 1600-1650°C, it is allowed to stand for slag removal for 3-5 minutes. After the standing period is over, the molten iron is discharged from the furnace at 1550-1600°C.

[0012] In step (4), the spheroidization is carried out by the flushing method. First, a nickel-magnesium spheroidizer is placed on the bottom of the inner side of the dam. The amount of nickel-magnesium spheroidizer added is 0.5-0.8% of the weight of the molten iron. The nickel-magnesium spheroidizer is covered with an inoculant, and then covered with D5S ductile iron filings, and finally covered with a layer of slag cleaning agent. Each layer of covering material is compacted.

[0013] Due to the particularity of D5S high nickel ductile iron, the product produced by ordinary spheroidizer does not meet the standards. Therefore, nickel-magnesium spheroidizer is used. The model of nickel-magnesium spheroidizer is Ni80Mg20. When the addition amount is 0.5-0.8%, the residual Mg in the casting can be guaranteed to be 0.08-0.12%.

[0014] In step (5), the ladle inoculation uses a silicon strontium inoculant with a specification of 2-10 mm and an inoculation amount of 1.0-1.2%; the in-stream inoculation uses a silicon strontium inoculant with a specification of 0.2-0.7 mm and an inoculation amount of 0.1-0.2%. In order to prevent the spheroidization inoculation decay of the molten iron after the spheroidization inoculation treatment from causing waste, the molten iron is cast within 10 minutes, and the casting temperature is 1500-1550°C.

[0015] In step (6), the final casting temperature of the molten model shell is controlled at 850-950°C. During casting, a layer of slag cleaning agent is sprinkled on the surface of the molten iron in the spheroidizing ladle for slag cleaning and heat preservation. At the same time, slag blocking cotton is placed on the surface of the slag cleaning agent to intercept slag. During the casting process, a 15-30 mesh ceramic filter is placed at the gate position of the molten model shell to filter and block slag, thereby reducing the entry of impurities into the product.

[0016] The patented technology of the present invention utilizes the investment casting process to produce D5S high nickel austenitic ductile iron. Through the optimization of the preparation process and the control of the raw material ratio, the element content (%) of the obtained product D5S ductile iron is as follows: C≤2.3, Si: 4.9-5.5, Mn≤1.0, P≤0.08, Ni: 34-37, Cr: 1.75-2.25.

[0017] The present invention solves the problem of shrinkage, pores, cold shut and other defects that are easily formed in conventional production processes by optimizing the process and accurately controlling the raw material ratio, while ensuring the product spheroidization rate, matrix structure stability and mechanical properties reaching the standards. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention will be further described below in conjunction with the accompanying drawings.

[0019] Figure 1 This is a schematic diagram of metallographic detection of ductile iron in Example 1; Figure 2 This is a schematic diagram of metallographic detection of ductile iron in Example 2; Figure 3 Schematic diagram of metallographic detection of ductile iron in Example 3. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1: A method for investment casting D5S high-nickel austenitic ductile iron, comprising the following steps: (1) Investment casting shell making: using medium temperature wax to make wax pattern, using a mixture of silica sol and zircon powder as the surface material of the shell, and using zircon sand as the sanding material; using a mixture of silica sol, mullite powder and fused quartz powder as the transition layer and back layer material of the shell, and using mullite sand as the sanding material, and obtaining the final shell after drying and dewaxing, wherein the silica sol is 830 type silica sol, and the mass concentration of silicon dioxide is 30%. The specific process is as follows: a) Add 30L of distilled water to 270L of silica sol to adjust the mass concentration of silica to 27%, then slowly add 324mL of wetting agent (purchased finished product, main components are polyether sensitive siloxane copolymer mixture and modifier) ​​and 270mL of defoamer (purchased finished product, main components are dimethyl silicone oil and modifier) ​​to the silica sol solution, then add 972kg of zircon powder in batches, continue stirring until uniform, and measure the viscosity of the final prepared silica sol slurry with a No. 4 James cup for 30s; b) Soak the wax model in wax model cleaning agent for 5 seconds, hang it up to drip off the liquid and soak it in silica sol for 5 seconds, hang it up to drip off the liquid and then immerse it in silica sol slurry until it is completely immersed and then take it out, blow the bubbles on the surface with 0.1MPa compressed air, immerse it in silica sol slurry again until it is completely immersed and then take it out to control the slurry for 5 seconds, then send it to the sand spraying machine to be covered with 80-120 mesh zircon sand, hang up the wax model covered with sand, dry it at 26℃ and 0.5m / s breeze for 3 hours to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of silica sol and 180-250 mesh mullite powder. In the transition layer slurry, the mullite powder is 480kg and the silica sol is 400kg, and the drying time is 8h; in the back layer slurry, the mullite powder is 400kg and the silica sol is 400kg, and the drying time is 10h; in the sealing layer slurry, the mullite powder is 200kg and the silica sol is 250kg, and the drying time is 10h; the transition layer, back layer and sealing layer are all dried at a temperature of 26℃ and a wind speed of 3m / s; d) In steps b) to c), the surface layer is made once, the transition layer is made once, the backing layer is made twice, and the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 15 minutes, the dewaxing temperature is 170°C, the dewaxing pressure is 0.6 MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds; (2) Shell roasting: natural gas is used for roasting, the roasting temperature is 1050℃, the time is 50min, after roasting, the temperature is reduced to 850℃, and the temperature is kept for 15min before casting; (3) Hot metal smelting: Place pig iron at the bottom of the furnace, add scrap steel and recycled materials in turn, and when the hot metal melts to 60% of the furnace capacity and the temperature reaches 1520°C, add electrolytic nickel, high carbon ferrochrome and ferrosilicon to melt and take samples for component testing. When the hot metal temperature reaches 1600°C, let it stand for 3 minutes to remove slag. After the standing time is over, the hot metal is discharged from the furnace at 1550°C. Among them, the pig iron is high-purity pig iron imported from South Africa, brand SORELMETAL RF-10; the recycled materials are die heads or scrap materials of high-nickel materials such as D5S; the scrap steel is high-quality carbon steel; the electrolytic nickel is NI99.99 high-purity electrolytic nickel; the high-carbon ferrochrome is FECr55; the ferrosilicon is FeSi75; the above-mentioned raw materials are prohibited from adhering to the surface of oil stains, mud blocks, plastics and other debris, and they can only be used after shot blasting, rust removal, dehydration and drying; the weight ratio of the above raw materials is 23.2% pig iron, 35% recycled materials, 15% scrap steel, 21% electrolytic nickel, 1.8% high-carbon ferrochrome, and 4% ferrosilicon; (4) Spheroidizing treatment: Spheroidizing is carried out by flushing method. First, a nickel-magnesium spheroidizing agent of model Ni80Mg20 is placed on the bottom of the inner side of the dam. The addition amount of the nickel-magnesium spheroidizing agent is 0.5% of the weight of the molten iron. The nickel-magnesium spheroidizing agent is covered with an inoculant, and then covered with D5S ductile iron filings, and finally covered with a layer of slag cleaning agent. Each layer of covering material is compacted; (5) Inoculation treatment: The secondary inoculation method is adopted. The ladle inoculation uses a silicon strontium inoculant with a specification of 2-10mm and an inoculation amount of 1.2%; the flow inoculation uses a silicon strontium inoculant with a specification of 0.2-0.7mm and an inoculation amount of 0.1%. In order to prevent the spheroidization inoculation decline of the molten iron after the spheroidization inoculation treatment and cause waste, the molten iron is cast within 10 minutes, and the casting temperature is 1500℃; (6) Mold shell pouring: During the spheroidizing treatment, the final casting temperature of the molten mold shell is controlled at 850°C. During casting, a layer of slag remover is sprinkled on the surface of the molten iron in the spheroidizing ladle for slag removal and heat preservation. At the same time, slag blocking cotton is placed on the surface of the slag remover to intercept slag. During the casting process, a 15-mesh ceramic filter is placed at the gate of the molten mold shell to filter and block slag to reduce the entry of impurities into the product.

[0022] Example 2: A method for investment casting D5S high-nickel austenitic ductile iron, the specific steps are the same as those in Example 1, and the parameters different from those in Example 1 are: (1) The specific process of investment casting shell making is as follows: a) Add 15L of pure water to 209L of silica sol to adjust the mass concentration of silica to 28%, then slowly add 314mL of wetting agent and 146mL of defoamer to the silica sol solution, then add 1045kg of zircon powder in batches, continue stirring until uniform, and measure the viscosity of the final silica sol slurry with a No. 4 James cup for 45s; b) Soak the wax model in wax model cleaning agent for 15 seconds, hang it up to drip off the liquid and soak it in silica sol for 5 seconds, hang it up to drip off the liquid and then immerse it in silica sol slurry until it is completely immersed and then take it out, blow the bubbles on the surface with 0.3MPa compressed air, immerse it in silica sol slurry again until it is completely immersed and then take it out to control the slurry for 10 seconds, then send it to the sand spraying machine to be covered with 80-120 mesh zircon sand, hang up the wax model covered with sand, dry it at 20℃ and 1m / s breeze for 8 hours to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of silica sol and 180-250 mesh mullite powder. In the transition layer slurry, the mullite powder is 800kg and the silica sol is 400kg, and the drying time is 12h; in the back layer slurry, the mullite powder is 600kg and the silica sol is 400kg, and the drying time is 24h; in the sealing layer slurry, the mullite powder is 300kg and the silica sol is 250kg, and the drying time is 14h; the transition layer, back layer and sealing layer are all dried at a temperature of 20℃ and a wind speed of 5m / s; d) In steps b) to c), the surface layer is made twice, the transition layer is made twice, the back layer is made 8 times, and the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 30 minutes, the dewaxing temperature is 150°C, the dewaxing pressure is 0.7 MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds; (2) Shell roasting: natural gas is used for roasting, the roasting temperature is 1150℃, the time is 50min, after roasting, the temperature is reduced to 950℃, and the temperature is kept at this temperature for 12min before casting; (3) Hot metal smelting: Pig iron is placed at the bottom of the furnace, and scrap steel and recycled materials are added in sequence. When the hot metal is melted to 80% of the furnace capacity and the temperature reaches 1520°C, electrolytic nickel, high carbon ferrochrome and ferrosilicon are added to melt and samples are taken for component testing. When the hot metal temperature reaches 1650°C, the hot metal is allowed to stand for 5 minutes to remove slag. After the standing time is over, the hot metal is discharged from the furnace at 1600°C. The weight ratio of the above raw materials is 30% pig iron, 20% recycled materials, 12% scrap steel, 30% electrolytic nickel, 3% high carbon ferrochrome, and 6% ferrosilicon. (4) Spheroidizing treatment: The amount of nickel-magnesium spheroidizing agent added is 0.8% of the weight of molten iron; (5) Inoculation treatment: For ladle inoculation, a silicon-strontium inoculant with a size of 2-10 mm and an inoculation amount of 1.2% is used; for in-stream inoculation, a silicon-strontium inoculant with a size of 0.2-0.7 mm and an inoculation amount of 0.2% is used. The molten iron is cast within 10 minutes at a casting temperature of 1550°C. (6) Mold shell casting: During the spheroidization process, the final casting temperature of the molten mold shell is controlled at 950°C. During the casting process, a 30-mesh ceramic filter is placed at the gate of the molten mold shell to filter out slag and reduce the entry of impurities into the product.

[0023] Example 3: A method for investment casting D5S high-nickel austenitic ductile iron, the specific steps are the same as those in Example 1, and the parameters different from those in Example 1 are: (1) Investment casting shell making: The specific process is as follows: a) Add 21.6L of pure water to 240L of silica sol to adjust the mass concentration of silica to 27.5%, then slowly add 408mL of wetting agent and 192mL of defoaming agent to the silica sol solution, then add 1008g of zircon powder in batches, continue stirring until uniform, and finally measure the viscosity of the prepared silica sol slurry with a No. 4 James cup for 38s; b) Soak the wax model in wax model cleaning agent for 10 seconds, hang it up to drip off the liquid and soak it in silica sol for 4 seconds, hang it up to drip off the liquid and then immerse it in silica sol slurry until it is completely immersed and then take it out, blow the bubbles on the surface with 0.2MPa compressed air, immerse it in silica sol slurry again until it is completely immersed and then take it out to control the slurry for 8 seconds, then send it to the sand spraying machine to be covered with 80-120 mesh zircon sand, hang up the wax model covered with sand, dry it at 23℃ and 0.8m / s breeze for 5 hours to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of silica sol and 180-250 mesh mullite powder. In the transition layer slurry, the mullite powder is 640kg and the silica sol is 400kg, and the drying time is 10h; in the back layer slurry, the mullite powder is 520kg and the silica sol is 400kg, and the drying time is 17h; in the sealing layer slurry, the mullite powder is 250kg and the silica sol is 250kg, and the drying time is 12h; the transition layer, back layer and sealing layer are all dried at a temperature of 23℃ and a wind speed of 4m / s; d) In steps b) to c), the surface layer is made twice, the transition layer is made once, the back layer is made five times, and the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 22 minutes, the dewaxing temperature is 160°C, the dewaxing pressure is 0.65 MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds; (2) Shell roasting: natural gas is used for roasting, the roasting temperature is 1100℃, the time is 48min, after roasting, the temperature is reduced to 900℃, and the temperature is kept for 12min before casting; (3) Hot metal smelting: Pig iron is placed at the bottom of the furnace, and scrap steel and recycled materials are added in sequence. When the hot metal is melted to 70% of the furnace capacity and the temperature reaches 1490°C, electrolytic nickel, high carbon ferrochrome and ferrosilicon are added to melt and samples are taken for component testing. When the hot metal temperature reaches 1620°C, the hot metal is allowed to stand for 4 minutes to remove slag. After the standing period is over, the hot metal is discharged from the furnace at 1580°C. The weight ratio of the above raw materials is 25% pig iron, 30% recycled materials, 12.5% ​​scrap steel, 25% electrolytic nickel, 2.5% high carbon ferrochrome, and 5% ferrosilicon. (4) Spheroidizing treatment: The amount of nickel-magnesium spheroidizing agent added is 0.6% of the weight of molten iron; (5) Inoculation treatment: For ladle inoculation, a silicon-strontium inoculant with a size of 2-10 mm and an inoculation amount of 1.1% is used; for in-stream inoculation, a silicon-strontium inoculant with a size of 0.2-0.7 mm and an inoculation amount of 0.15% is used. The molten iron is cast within 10 minutes at a casting temperature of 1520°C. (6) Mold shell casting: During the spheroidization process, the final casting temperature of the molten mold shell is controlled at 900°C. During the casting process, a 25-mesh ceramic filter is placed at the gate of the molten mold shell to filter out slag and reduce the entry of impurities into the product.

[0024] The composition of the D5S high-nickel austenitic ductile iron obtained in Examples 1-3 was tested, and the results were as follows: It can be seen from the above test results that the nickel content in the austenitic ductile iron prepared by the method of the present invention is more than 34%, the product is non-magnetic, has extremely strong corrosion resistance, and excellent high temperature resistance, low temperature resistance and wear resistance.

[0025] The performance parameters of the D5S high nickel austenitic ductile iron obtained in Examples 1-3 were tested, and the results are as follows: It can be seen from the above test results that the D5S austenitic ductile iron prepared by the method of the present invention fully meets the performance requirements of the ASTM A439 / A439M-18 standard, and the specific requirements are as follows: Tensile strength>380Mpa, yield strength>210Mpa, elongation>10%, hardness 131-193HB.

[0026] Combined with Figure 1-3 The metallographic test results of the austenitic ductile iron obtained in Examples 1-3 show that the ductile iron prepared by the present invention has spherical graphite, a small amount of flocculent graphite, a spheroidization rate of 1-3, a graphite ball size of 5-8, an austenite matrix and a small amount of carbide, which fully meets the requirements of ASTM A439 / A439M-18 standards.

[0027] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for investment casting D5S high nickel austenitic ductile iron, characterized by: The steps include: (1) A wax mold is made using medium-temperature wax, a mixture of silica sol and zircon powder is used as the surface layer material of the mold shell, and zircon sand is used as the sanding material; a mixture of silica sol and mullite powder is used as the transition layer and back layer material of the mold shell, and mullite sand is used as the sanding material, and the final mold shell is obtained after drying and dewaxing; (2) Use a natural gas roasting furnace to roast the shell, cool it down in the furnace before spheroidization and then keep it warm; (3) Pig iron, recycled materials, scrap steel, electrolytic nickel, high carbon ferrochrome and ferrosilicon are selected as halogen materials and added into a smelting furnace for smelting to obtain molten iron; (4) Spheroidizing the molten iron by flushing method; (5) Adopting the secondary inoculation method, adding inoculant when tapping iron, and using secondary inoculation during casting; (6) During the spheroidization treatment, the molten model shell is taken out of the roasting furnace for casting to obtain the product.

2. The method for investment casting D5S high nickel austenitic ductile iron according to claim 1, characterized in that: In step (1), the specific process of investment casting shell making is as follows: a) Add distilled water / purified water to the silica sol to adjust the mass concentration of silica to 27-28%, then slowly add the wetting agent and defoamer to the silica sol solution in sequence, then add zircon powder in batches, and continue stirring until uniform. The viscosity of the final silica sol slurry is measured with a No. 4 James cup to measure 30-45s; b) Soak the wax model in wax model cleaning agent and silica sol in sequence, then immerse it in silica sol slurry, take it out after it is completely immersed, blow the bubbles on the surface with compressed air, immerse it in silica sol slurry again, take it out after it is completely immersed, and then send it to the sand spraying machine to be covered with zircon sand. Hang the wax model covered with sand and dry it for 3-8 hours at a temperature of 23±3℃ and a breeze of 0.5-1m / s to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of silica sol and 180-250 mesh mullite powder to prepare the slurry. In the transition layer slurry, the weight ratio of mullite powder to silica sol is 1.2-2:1, and the drying time is 8-12h; in the back layer slurry, the weight ratio of mullite powder to silica sol is 1-1.5:1, and the drying time is 10-24h; in the sealing layer slurry, the weight ratio of mullite powder to silica sol is 0.8-1.2:1, and the drying time is 10-14h; the transition layer, back layer and sealing layer are all dried at a temperature of 23±3℃ and a breeze of 3-5m / s; d) In steps b)-c), the surface layer is made 1-2 times, the transition layer is made 1-2 times, the back layer is made 2-8 times, the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 15-30 minutes, the dewaxing temperature is 150-170°C, the dewaxing pressure is 0.6-0.7MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds.

3. The method for investment casting D5S high nickel austenitic ductile iron according to claim 2, characterized in that: The silica sol is 830 type silica sol, and the mass concentration of silicon dioxide is 30%. In step a), the volume ratio of distilled water / pure water to silica sol is 72-111:1000; the volume ratio of wetting agent, defoaming agent to silica sol is 1.2-1.7:0.7-1:1000; the mass ratio of zircon powder to silica sol is 3.2-4.5:

1.

4. The method for investment casting D5S high nickel austenitic ductile iron according to claim 2, characterized in that: In step b), the wax mold is immersed in wax mold cleaning agent for 5-15s, hung up to drip off the liquid and then immersed in silica sol for 3-5s, hung up to drip off the liquid and then immersed in silica sol slurry until it is completely immersed and then taken out, 0.1-0.3MPa compressed gas is used to blow the surface bubbles, immersed in silica sol slurry again until it is completely immersed and then taken out to control the slurry for 5-10s, and then sent to the sand spraying machine to be covered with 80-120 mesh zircon sand.

5. The method for investment casting D5S high nickel austenitic ductile iron according to claim 1, characterized in that: In step (2), the natural gas roasting temperature is 1050-1150°C, the roasting time is greater than 45 minutes, and the temperature is reduced to 850-950°C after roasting, and the temperature is kept constant for more than 10 minutes before casting.

6. The method for investment casting D5S high nickel austenitic ductile iron according to claim 1, characterized in that: In step (3), the pig iron is high-purity pig iron, the recycled material is a die head or scrap material of the same material as D5S, the scrap steel is high-quality carbon steel, the electrolytic nickel is NI99.99 high-purity electrolytic nickel, the high-carbon ferrochrome is FECr55, and the ferrosilicon is FeSi75. The weight ratio of the above raw materials is 20-30% of pig iron, 20-35% of recycled material, 10-15% of scrap steel, 20-30% of electrolytic nickel, 1.8-3% of high-carbon ferrochrome, and 4-6% of ferrosilicon.

7. The method for investment casting D5S high nickel austenitic ductile iron according to claim 1 or 6, characterized in that: In step (3), pig iron is placed in a furnace body, and scrap steel and recycled materials are added in sequence. When the molten iron is melted to 60-80% of the capacity in the furnace and the temperature reaches 1450-1520°C, electrolytic nickel, high carbon ferrochrome and ferrosilicon are added to melt and samples are taken for component detection. When the temperature of the molten iron reaches 1600-1650°C, the molten iron is allowed to stand for 3-5 minutes to remove slag. After the standing period is completed, the molten iron is discharged from the furnace at 1550-1600°C.

8. The method for investment casting D5S high nickel austenitic ductile iron according to claim 1, characterized in that: In step (4), the spheroidization is carried out by the flushing method. First, a nickel-magnesium spheroidizer is placed on the bottom of the inner side of the dam. The amount of nickel-magnesium spheroidizer added is 0.5-0.8% of the weight of the molten iron. The nickel-magnesium spheroidizer is covered with an inoculant, and then covered with D5S ductile iron filings, and finally covered with a layer of slag cleaning agent. Each layer of covering material is compacted.

9. The method for investment casting D5S high nickel austenitic ductile iron according to claim 1, characterized in that: In step (5), the inoculation in the bag uses a silicon strontium inoculant with a specification of 2-10 mm and an inoculation amount of 1.0-1.2%; The flow inoculation uses a silicon strontium inoculant with a specification of 0.2-0.7mm and an inoculation amount of 0.1-0.2%. The molten iron is cast within 10 minutes and the casting temperature is 1500-1550℃.

10. The method for investment casting D5S high internal austenite ductile iron according to claim 1, characterized in that: In step (6), the final casting temperature of the molten model shell is controlled at 850-950°C. During casting, a layer of slag cleaning agent is sprinkled on the surface of the molten iron in the spheroidizing ladle, and slag blocking cotton is placed on the surface of the slag cleaning agent to intercept slag. During the casting process, a 15-30 mesh ceramic filter is placed at the gate position of the molten model shell to filter and block the slag.

Citation Information

Cited By

  • Conductivity sensor packaging method, conductivity sensor and temperature-salinity-depth measuring instrument

    CN119555754A