Synthesis method of Fe3O4 / SiO2 / Ag magnetic nano composite material and application of Fe3O4 / SiO2 / Ag magnetic nano composite material as SERS substrate for detecting loramine

By using Fe3O4/SiO4/Ag magnetic nanocomposite as SERS substrate, the problem of complex and insufficient sensitivity of traditional detection methods is solved, and high sensitivity detection of chloramphenicol is achieved, which is suitable for multi-field applications.

CN119035545APending Publication Date: 2024-11-29SHAANXI SCI TECH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411152718.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the traditional method is complex and time-consuming when detecting chloramphenicol. The SERS method has high sensitivity but is difficult to achieve low concentration analysis, and the single nano silver has limited effect as a Raman substrate.

Method used

Using Fe3O4/SiO2/Ag magnetic nanocomposite as SERS substrate, magnetic iron tetroxide nanoparticles were synthesized by co-precipitation method, loading mesoporous silica and nanosilver to form Fe3O4/SiO2/Ag magnetic nanocomposite for use in High sensitivity detection of chloramphenicol.

Benefits of technology

The detection of chloramphenicol in the concentration range of 1.0×10-3~1.0×10-10mol/L was achieved. The linear relationship was good, the detection limit was 0.6×10-11mol/L, and the correlation coefficient R2 was 0.9758, and the reproducibility was Good, suitable for agriculture, industry, environment and food fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035545A_ABST
    Figure CN119035545A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of antibiotic detection, in particular to a synthesis method of a Fe3O4 / SiO2 / Ag magnetic nano composite material and application of the Fe3O4 / SiO2 / Ag magnetic nano composite material as an SERS (Surface Enhanced Raman Scattering) substrate for detecting loramine. The invention provides a synthesis method of a Fe3O4 / SiO2 / Ag magnetic nano composite material, which comprises the following steps: synthesizing magnetic Fe3O4 nano particles by a coprecipitation method, loading SiO2 on the surfaces of the magnetic Fe3O4 nano particles to form Fe3O4 / SiO2, and loading nano silver on the Fe3O4 / SiO2 by taking a silane coupling agent KH-550 as a bridge to form the Fe3O4 / SiO2 / Ag composite nano material. The material can be used as an SERS (Surface Enhanced Raman Scattering) substrate for detecting loramine, the prepared Fe3O4 / SiO2 / Ag magnetic composite nano material is used as the SERS substrate for analyzing and detecting chloramphenicol in a concentration range of 1.0 * 10 <-3 > to 1.0 * 10 <-10 > mol / L, a standard curve equation is y = 48199-4386x, a correlation coefficient R2 is 0.9758, a detection limit is 0.6 * 10 <-11 > mol / L, RSD (Relative Standard Deviation) is 7.2%, and the SERS substrate can be used for analyzing and detecting chloramphenicol. The material can be applied to the fields of agriculture, industry, environment, food, medicine and sanitation, and high-sensitivity detection of analytes is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of antibiotic detection, and in particular to a method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nanocomposite material and an application of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material as a SERS substrate for detecting chloranabine. Background Art

[0002] Antibiotics are a class of drugs used to treat bacterial infections. These drugs work by inhibiting and killing bacteria. In recent years, the production technology of antibiotics has experienced significant progress, and the rapid development of this field has promoted the continuous renewal of antibiotic products. With the continuous emergence of new antibiotics, their antibacterial activity has been significantly improved, which directly promotes the increasing scope of their application in clinical treatment. The high antibacterial properties of antibiotics make them an important weapon against bacterial infections, indicating that in future medical practice, antibiotics will play a more critical role, providing patients with a wider range of treatment options and better health protection. However, the abuse and illegal use of antibiotics leave residues in animal and human tissues. Since antibiotics are not easy to decompose, they will not only remain in animals and humans, but also in nature through food, excretion and other pathways. Long-term residues and irrational use of antibiotics will cause greater harm to human life and health, and this harm is irreversible.

[0003] Chloramphenicol is a broad-spectrum antibiotic that was once widely used in aquaculture. Although it is now included in China's banned list of fishery drugs, it is still frequently detected in the aquatic environment. The presence of chloramphenicol poses a threat to aquatic ecosystems because it can destroy the microecological balance, inhibit the growth of beneficial microorganisms, and promote the reproduction of drug-resistant bacteria, thereby affecting the decomposition and transformation process of organic matter in the water body. In addition, chloramphenicol may also have similar negative effects on other aquatic organisms, thereby changing the population structure and balance of the ecosystem. Commonly used traditional detection methods include chromatography. Although they have high sensitivity, they have the disadvantages of complex processing methods, long detection time, and high detection costs. They are not suitable for field analysis and detection with many and complex samples. SERS is an analytical method that can detect to the molecular level. It is relatively simple to process samples, and it has high sensitivity and good accuracy. It can be used for field analysis and detection. Raman spectroscopy is a molecular vibration spectrum based on the Raman scattering effect, which realizes the identification of molecular vibration states through inelastic scattering spectra. The conventional Raman scattering intensity is weak, resulting in poor sensitivity of Raman spectroscopy, making it difficult to achieve analytical detection of low-concentration target molecules. Surface-enhanced Raman spectroscopy is a new type of molecular spectroscopy technology that is based on the Raman scattering effect and uses a special substrate to generate surface plasmons when excited by light, thereby enhancing the Raman scattering signal of the adsorbed substance by tens of millions of times. It has high sensitivity, strong specificity, and short detection time. The detection process is less affected by the solution.

[0004] With the rapid development of nanomaterials, nano-magnetic composites, as an important functional material, have become a research hotspot in related fields due to their many excellent properties. Magnetic ferroferric oxide nanoparticles, as typical magnetic nanoparticles, have attracted much attention due to their special magnetic properties, good biocompatibility, and low toxicity and side effects. They are often used as magnetic cores to prepare magnetic composites and are used in many fields. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nanocomposite material in view of the deficiencies of the above-mentioned prior art.

[0006] In order to solve the above technical problems, the present invention provides a method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nanocomposite material, comprising the following steps:

[0007] S1. Preparation of Fe3O4 magnetic nanoparticles: nitrogen is introduced into deionized water 1 and mechanically stirred, ferrous sulfate and ferric chloride are added and the rotation speed is increased to dissolve to obtain a mixed solution, NaOH solution is added dropwise to the mixed solution after heating at 60°C in a water bath to adjust the pH value, stirring is stopped after sufficient reaction, the water bath temperature is increased to 80°C and fully aged, the entire reaction process is completed under nitrogen protection, after the reaction is completed, the product is cooled to room temperature, separated using a magnet and fully washed, washing is stopped when the supernatant in the product is neutral, and Fe3O4 magnetic nanoparticles are obtained after drying;

[0008] S2, preparation of Fe3O4 / SiO2: fully dissolve the CTAB added to deionized water 2, then add the Fe3O4 magnetic nanoparticles prepared in S1, add NaOH solution and deionized water 3 after ultrasonic dispersion, heat to 60°C in a water bath and stir thoroughly, then add a mixed solution of ethyl orthosilicate and methanol to obtain a reaction solution, stir thoroughly again in a 60°C water bath, separate using a magnet, wash thoroughly and dry for the first time, reflux the powder obtained by the first drying three times, and dry for the second time to obtain Fe3O4 / SiO2 magnetic nanoparticles

[0009] S3. Preparation of Fe3O4 / SiO2 / Ag: Add Fe3O4 / SiO2 prepared in S2 to deionized water 4, add KH-550 after ultrasonic dispersion and stir evenly, take AgNO3 and dissolve it in deionized water 5 to obtain AgNO3 solution, take sodium citrate and dissolve it in deionized water 6 to obtain sodium citrate solution, add the AgNO3 solution into a conical flask, heat it in a water bath, add the sodium citrate solution, stir evenly again, then stop the water bath and cool to room temperature, wash thoroughly, separate by magnetic separation and dry, to obtain Fe3O4 / SiO2 / Ag magnetic nanocomposite material.

[0010] According to the synthesis method of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material provided by the present invention: the mass volume ratio of the deionized water 1, ferrous sulfate, ferric chloride and NaOH solution in S1 is 75.0mL:0.5563g:0.7201g:10.0mL, and the concentration of the NaOH solution is 2mol / L.

[0011] According to the synthesis method of Fe3O4 / SiO2 / Ag magnetic nanocomposite material provided by the present invention: the time for introducing nitrogen in S1 is 30 minutes, the stirring speed is 200r / min, the increased speed is 1000r / min, the pH value is 9.0-10.0, the time for sufficient reaction is 30 minutes, the time for sufficient aging is 60 minutes, the detergent used for washing is deionized water, and the drying temperature is 60°C.

[0012] According to the synthesis method of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material provided by the present invention: the mass volume ratio of the deionized water 2, CTBA, Fe3O4 magnetic nanoparticles, NaOH solution, deionized water 3, tetraethyl orthosilicate and methanol in S2 is 50.0mL: 0.5001g: 0.0503g: 10.0mL: 400.0mL: 0.5mL: 2.0mL, and the concentration of the NaOH solution is 50mmoL / L.

[0013] According to the synthesis method of Fe3O4 / SiO2 / Ag magnetic nanocomposite material provided by the present invention: the ultrasonic dispersion time in S2 is 15 minutes, the sufficient stirring time is 60 minutes, the sufficient stirring time again is 10 hours, the detergent used for the washing is deionized water and anhydrous ethanol alternately, the first drying temperature is 50°C, the first drying time is 6 hours, the reflux temperature is 80°C, the reflux time is 4 hours, the solvent used for the reflux is acetone, the second drying temperature is 60°C, and the second drying time is 6 hours.

[0014] According to the synthesis method of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material provided by the present invention: the mass volume ratio of the deionized water 4, Fe3O4 / SiO2, KH-550, AgNO3, deionized water 5, sodium citrate and deionized water 6 in S3 is 15.0mL: 0.1023g: 1.00mL: 0.0506g: 75.0mL: 0.0915g: 10.0mL.

[0015] According to the synthesis method of Fe3O4 / SiO2 / Ag magnetic nanocomposite material provided by the present invention: the stirring time in S3 is 6 hours, the water bath heating temperature is 100°C, the re-stirring time is 0.5 hours, the detergent used for the washing is deionized water, the drying temperature is 60°C, and the drying time is 6 hours.

[0016] The present invention also provides an application of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material: the Fe3O4 / SiO2 / Ag magnetic nanocomposite material can be used as a substrate for surface enhanced Raman spectroscopy to detect chlorrelin.

[0017] Due to the large surface energy of magnetic nanoparticles and their own magnetic dipole moment, they are very easy to agglomerate and oxidize, thus losing the excellent performance of magnetic nanoparticles. Therefore, it is necessary to modify the surface of magnetic nanoparticles. Among them, surface loading silica is an ideal material for modification. Nanosilver has the characteristics of nanomaterials, with the advantages of large specific surface area, strong permeability, high safety and oxidation resistance. However, single nanosilver as a Raman substrate has limited enhancement effect. Nanosilver particles are evenly loaded onto inorganic nanocarriers with more stable structures to give them better properties. By loading mesoporous silica and nanosilver on magnetic ferroferric oxide particles, the excellent properties of each particle are combined to synthesize Fe3O4 / SiO2 / Ag magnetic nanocomposite materials, and high-sensitivity detection of chloramphenicol is achieved using SERS technology.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] The invention provides a method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nano-composite material. Magnetic Fe3O4 nano-particles are synthesized by a coprecipitation method, SiO2 is loaded on the surface of the Fe3O4 / SiO2 to form Fe3O4 / SiO2, and nano-silver is loaded on the Fe3O4 / SiO2 using a silane coupling agent KH-550 as a bridge to form a Fe3O4 / SiO2 / Ag composite nano-material.

[0020] The Fe3O4 / SiO2 / Ag magnetic nanocomposite prepared by the present invention can be used as a SERS substrate to detect chloramphenicol. The prepared Fe3O4 / SiO2 / Ag magnetic composite nanocomposite is used as a SERS substrate for the analysis and detection of chloramphenicol at 1.0×10 -3 ~1.0×10 -10 The standard curve equation is y=48199-4386x, and the correlation coefficient is R 2 is 0.9758, and the detection limit is 0.6×10 -11 mol / L, RSD is 7.2%. This material can be used in agriculture, industry, environment, food, medicine and health fields to achieve high-sensitivity detection of analytes. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is the XRD pattern of Fe3O4 prepared in Example 1;

[0022] Figure 2 is the XRD pattern of Fe3O4 prepared in Comparative Example 1;

[0023] Figure 3 is the XRD pattern of Fe3O4 / SiO2 / Ag prepared in Example 1;

[0024] Figure 4 is the XRD pattern of Fe3O4 / SiO2 / Ag prepared in Comparative Example 2;

[0025] Figure 5 is the XRD pattern of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag prepared in Example 1;

[0026] Figure 6 is the infrared spectra of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag prepared in Example 1;

[0027] Figure 7 This is the UV-visible spectrum of Fe3O4 / SiO2 / Ag prepared in Comparative Example 2;

[0028] Figure 8 is a TEM image of Fe3O4 / SiO2 / Ag prepared in Example 1;

[0029] Fig. 9 is the energy spectrum of Fe3O4 / SiO2 / Ag prepared in Example 1;

[0030] Fig.10 This is the Raman spectrum of chloramphenicol solid sample;

[0031] Fig.11 Fe3O4 / SiO2 / Ag-chloramphenicol (10 -5 mol / L)(a), chloramphenicol solution(b), Fe3O4 / SiO2 / Ag(c), Fe3O4 / SiO2(d) and Fe3O4(e) SERS images;

[0032] Fig.12 a~h are concentrations of 1.0×10 -3 ~1.0×10 -10 mol / L SERS image of chloramphenicol on Fe3O4 / SiO2 / Ag substrate;

[0033] Fig.13 It is the negative logarithmic relationship between Raman intensity peak and concentration;

[0034] Fig.14 A is eight parts of chloramphenicol (10 -4 mol / L); B is the SERS image of eight portions of chloramphenicol (10 -4 mol / L) solution at 1590cm -1 RSD of the Raman peak intensity at . DETAILED DESCRIPTION

[0035] Example 1

[0036] This embodiment provides a method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nanocomposite material, comprising the following steps:

[0037] S1. Preparation of Fe3O4 magnetic nanoparticles: 75.0 mL of deionized water was added to a 250.0 mL three-necked flask, and the flask was placed in a water bath and mechanically stirred at a stirring speed of 200 r / min. Nitrogen was introduced for deoxygenation for 30 min, 0.5563 g of ferrous sulfate and 0.7201 g of ferric chloride were added, and the speed was adjusted to 1000 r / min. The solution was stirred until the solid was completely dissolved and the solution was orange-yellow. After the water bath temperature was raised to 60 °C, 10.0 mL of 2 mol / L Na OH solution, during the dropwise addition process, the color of the solution gradually changes from orange-yellow to black, the pH value of the solution is adjusted to between 9.0 and 10.0, and the reaction is carried out for 30 minutes, and the stirring is stopped. Then the water bath temperature is raised to 80°C and aged for 60 minutes. The entire reaction process must be completed under nitrogen protection. After the reaction is completed, the solution is cooled to room temperature, separated by a magnet, and washed with deionized water for more than three times. When the supernatant in the product is neutral, the washing is stopped, and the product is placed in a 60°C oven for drying to obtain Fe3O4 magnetic nanoparticles;

[0038] S2. Preparation of Fe3O4 / SiO2: Add 50.0 mL of deionized water to a 500.0 mL beaker, add 0.5001 g of CTAB (hexadecyl ammonium bromide) to fully dissolve, then add 0.0503 g of Fe3O4 magnetic nanoparticles prepared in S1, and after ultrasonic dispersion for 15 min, add 10.0 mL of 50 mmol / L NaOH solution and 400.0 mL of deionized water, heat in a water bath to 60 °C, and stir thoroughly for 60 min. in, and then add a mixed solution of 0.5mL of ethyl orthosilicate and 2.0mL of methanol to obtain a reaction solution, which is mechanically stirred in a water bath at 60°C for 10 hours, separated by a magnet, washed three times with deionized water and anhydrous ethanol alternately, and dried in an oven at 50°C for 6 hours. The dried powder is refluxed in acetone at 80°C for 4 hours, and the surfactant (CTAB) is removed after reflux three times. Then, it is placed in an oven at 60°C and dried for 6 hours to obtain Fe3O4 / SiO2 magnetic nanoparticles.

[0039] S3, preparation of Fe3O4 / SiO2 / Ag: add 15.0mL of deionized water to a 250.0mL conical flask, add 0.1023g of Fe3O4 / SiO2 prepared in S2, add 1.00mL of silane coupling agent KH-550 after ultrasonic dispersion, stir for 6h to mix well, take 0.0506g of AgNO3 and dissolve it in 75.0mL of deionized water to obtain AgNO3 solution, 0.0915g Dissolve sodium citrate in 10.0 mL of deionized water to obtain a sodium citrate solution, add the AgNO3 solution into a conical flask, heat it in a water bath to 100°C, then add the sodium citrate solution, maintain the water bath temperature at 100°C, stir again for 0.5 h, stop the water bath after stirring and cool to room temperature, wash with deionized water 3 times, and after magnetic separation, put it in an oven at 60°C and dry it for 6 h to obtain a Fe3O4 / SiO2 / Ag magnetic nanocomposite material.

[0040] Comparative Example 1

[0041] This comparative example provides a method for preparing Fe3O4 magnetic nanoparticles, comprising the following steps:

[0042] Preparation of Fe3O4 magnetic nanoparticles: 75.0 mL of deionized water was added to a 250.0 mL three-necked flask, and the mixture was placed in a water bath and mechanically stirred at a speed of 200 r / min. Nitrogen was introduced for deoxygenation for 30 min, 0.2788 g of ferrous sulfate and 0.5415 g of ferric chloride were added, and the speed was adjusted to 1000 r / min. The mixture was stirred until the solid was completely dissolved and the solution was orange-yellow. After the water bath temperature was raised to 60 °C, 8.0 mL of 2 mol / L NaOH was added dropwise. The solution, during the dropwise addition process, the color of the solution gradually changes from orange-yellow to black. After adjusting the pH value of the solution between 9.0 and 10.0, react for 30 minutes, stop stirring, then raise the water bath temperature to 80°C and age for 60 minutes. The entire reaction process must be completed under nitrogen protection. After the reaction is completed, the solution is cooled to room temperature, separated by a magnet, and washed with deionized water for more than three times. When the supernatant in the product is neutral, stop washing, put it in a 60°C oven to dry, and obtain Fe3O4 magnetic nanoparticles.

[0043] Comparative Example 2

[0044] This comparative example provides a method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nanocomposite material, comprising the following steps:

[0045] S1. Preparation of Fe3O4 magnetic nanoparticles: 75.0 mL of deionized water was added to a 250.0 mL three-necked flask, and the flask was placed in a water bath and mechanically stirred at a stirring speed of 200 r / min. Nitrogen was introduced for deoxygenation for 30 min, 0.5563 g of ferrous sulfate and 0.7201 g of ferric chloride were added, and the speed was adjusted to 1000 r / min. The solution was stirred until the solid was completely dissolved and the solution was orange-yellow. After the water bath temperature was raised to 60 °C, 10.0 mL of 2 mol / L Na OH solution, during the dropwise addition process, the color of the solution gradually changes from orange-yellow to black, the pH value of the solution is adjusted to between 9.0 and 10.0, and the reaction is carried out for 30 minutes, and the stirring is stopped. Then the water bath temperature is raised to 80°C and aged for 60 minutes. The entire reaction process must be completed under nitrogen protection. After the reaction is completed, the solution is cooled to room temperature, separated by a magnet, and washed with deionized water for more than three times. When the supernatant in the product is neutral, the washing is stopped, and the product is placed in a 60°C oven for drying to obtain Fe3O4 magnetic nanoparticles;

[0046] S2. Preparation of Fe3O4 / SiO2: Add 50.0 mL of deionized water to a 500.0 mL beaker, add 0.5001 g of CTAB (hexadecyl ammonium bromide) to fully dissolve, then add 0.0503 g of Fe3O4 magnetic nanoparticles prepared in S1, and after ultrasonic dispersion for 15 min, add 10.0 mL of 50 mmol / L NaOH solution and 400.0 mL of deionized water, heat in a water bath to 60 °C, and stir for 60 min. n, then add 0.5mL of a mixed solution of ethyl orthosilicate and 2.0mL of methanol to obtain a reaction solution, stir mechanically in a water bath at 60°C for 10h, separate using a magnet, wash three times with deionized water and anhydrous ethanol alternately, dry in an oven at 50°C for 6h, reflux the dried powder in acetone at 80°C for 4h, remove the surfactant (CTAB) after reflux three times, and then dry in an oven at 60°C for 6h to obtain Fe3O4 / SiO2 magnetic nanoparticles.

[0047] S3. Preparation of Fe3O4 / SiO2 / Ag magnetic nanocomposite materials: 165.0 mL of deionized water was added to a 250.0 mL beaker, which was placed on an asbestos net and heated to boiling. 1.00 mL of 30 mg / mL AgNO3 solution was added dropwise, and then 3.0 mL of 1% sodium citrate solution was added dropwise after boiling. After boiling for 3 to 5 minutes, the color of the solution changed from colorless to light yellow, and then to orange after 5 minutes. Then the temperature was lowered to 92°C and heated for 1 hour to obtain Nanosilver particle solution, add 0.0107g of Fe3O4 / SiO2 prepared in S2 into a 100mL beaker and ultrasonically disperse for 10 minutes, then add the nanosilver particle solution step by step, add 10.0mL each time and stir thoroughly, add 10 times in total, let stand for half an hour after the reaction is completed, separate with a magnet, wash three times with anhydrous ethanol and deionized water, put into a 60°C oven and dry for *h to obtain Fe3O4 / SiO2 / Ag magnetic nanocomposite material.

[0048] Example 2

[0049] In this example, the intermediate products and final products prepared in Example 1, Comparative Example 1 and Comparative Example 2 are characterized.

[0050] (1) XRD characterization of Fe3O4 / SiO2 / Ag magnetic nanocomposites.

[0051] ① Figure 1 is the XRD pattern of Fe3O4 magnetic nanoparticles prepared by S1 in Example 1, Figure 2 This is the XRD diagram of the Fe3O4 magnetic nanoparticles prepared in Comparative Example 1.

[0052] By comparing the two figures, we can see Figure 1 Compare Figure 2 The characteristic peak of Fe3O4 in the sample is stronger and has a better peak shape, indicating that the Fe3O4 magnetic nanoparticles prepared by the method provided in Example 1 are better. 2+ with Fe 3+ The effect will be better when the amount ratio of the substance is about 3:4.

[0053] This is because Fe 2+ Easily oxidized to Fe 3+ , which makes the ratio of the amount of substances required for the theoretical reaction inconsistent with 1:2, so during the reaction process, Fe 2+ The amount should be appropriately excessive.

[0054] ②After preparing Fe3O4 / SiO2, Figure 3 The XRD pattern of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material prepared by the method provided in Example 1 is shown in FIG. Figure 4 This is the XRD diagram of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material prepared by the method provided in Comparative Example 2.

[0055] By comparing the two figures, Figure 3 It has characteristic peaks of nanosilver, and the peak shape is also good, and the effect is better; Figure 4 There are characteristic peaks of nanosilver, but the peak shape is weak.

[0056] This indicates that the effect of the silver loading method provided in Comparative Example 2 is not ideal, while the effect of the silver loading method provided in Example 1 is better.

[0057] ③ XDR was used to characterize the three materials Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag prepared in Example 1. The results are as follows: Figure 5 shown.

[0058] Figure 5 The three lines a, b and c are the XRD diffraction peaks of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag respectively. The sample contains the characteristic peaks of Fe3O4, SiO2 and Ag, and no other impurity peaks are detected.

[0059] It can be seen from the XRD diagram that the magnetic nanoparticles Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag all have diffraction peaks at 2θ of 30.1°, 35.4°, 43.1°, 56.9° and 62.5°, which are the characteristic peaks of Fe3O4 and correspond to its standard magnetic ferroferric oxide crystal structure data (220), (311), (400), (511) and (440).

[0060] Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag have a wider peak at around 2θ 20°, which is the characteristic peak of SiO2 and is consistent with its standard diffraction peak of SiO2.

[0061] Compared with the Fe3O4 / SiO2 spectrum, the Fe3O4 / SiO2 / Ag has new diffraction peaks at 2θ of 38.2°, 44.3°, 64.5° and 77.4°, which correspond to the (111), (200), (220) and (311) crystal planes of Ag, respectively.

[0062] From the above characterization results, it can be seen that the product Fe3O4 / SiO2 / Ag in Example 1 was successfully prepared.

[0063] (2) IR characterization of Fe3O4 / SiO2 / Ag magnetic nanocomposites.

[0064] Figure 6 It is the IR (infrared spectrum) analysis diagram of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag, showing the characteristic peaks of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag.

[0065] from Figure 6 It can be clearly seen that the -1 The absorption peak near is the characteristic absorption peak of Fe-O bond in Fe3O4, indicating the presence of Fe3O4 magnetic nanoparticles in this nanomaterial.

[0066] Figure 6 The comparison between Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag and Fe3O4 shows that at 1150cm -1 An obvious characteristic peak appears near the absorption peak, which is caused by the bending vibration of the Si-O-Si bond, indicating the presence of mesoporous silica in the nanomaterial.

[0067] pass Figure 6 It was found that the absorption peak intensity of the Si-O bond in Fe3O4 / SiO2 / Ag was weakened after further loading of nanosilver. This is because the nanosilver was well loaded on the Fe3O4 / SiO2 surface and the coverage was uniform.

[0068] from Figure 6 It can be seen that nanosilver and silicon dioxide are successfully loaded on Fe3O4 magnetic nanoparticles.

[0069] (3) UV-Vis image of nanosilver.

[0070] Figure 7The UV-Vis (ultraviolet visible spectrum) of the Fe3O4 / SiO2 / Ag magnetic composite nanoparticle solution in Comparative Example 2 shows that the -1 The absorption peaks on the left and right are characteristic absorption peaks of nanosilver particle solution.

[0071] (4) TEM and EDX characterization of Fe3O4 / SiO2 / Ag magnetic nanocomposites.

[0072] Figure 8 and Fig. 9 TEM (transmission electron microscopy) and EDX (energy spectrum) characterizations of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material prepared in Example 1.

[0073] from Figure 8 It can be seen that the dark gray particles are Fe3O4 nanoparticles, the thin layer of gray is SiO2, and the dark black is nano-Ag. Due to the magnetism of Fe3O4, the nanoparticles are in a clustered state.

[0074] from Fig. 9 It can be seen that there are elements such as Fe, O, Si and Ag, indicating that Example 1 successfully prepared the Fe3O4 / SiO2 / Ag magnetic nanocomposite material.

[0075] Example 3

[0076] This embodiment provides an application method of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material prepared in Example 1, and the specific steps are as follows.

[0077] S1. Dissolve 0.0323 g of chloramphenicol powder in 10.0 mL of anhydrous ethanol to obtain a concentration of 1.0 × 10 -2 mol / L chloramphenicol ethanol solution, and then, a stepwise dilution method was used to prepare a concentration range of 1.0×10 -3 ~1.0×10 -10 mol / L chloramphenicol solution, place in a cool, dry place until use;

[0078] S2, take 0.0123g of the Fe3O4 / SiO2 / Ag magnetic nanocomposite powder prepared in Example 1 and dissolve it in 5.0mL of anhydrous ethanol, ultrasonically disperse it for 15min, and evenly drip it on a glass slide with a pipette, put it in a 50°C oven to dry, and after the glass slide is dried, a glass slide containing a Fe3O4 / SiO2 / Ag substrate is obtained, and it is cooled to room temperature and set aside;

[0079] S3, pipette the 1.0×10 -3 ~1.0×10 -1020.0 μL of chloramphenicol solutions of various concentrations within the mol / L range were dropped onto the glass slide containing the Fe3O4 / SiO2 / Ag substrate prepared in S2, and then Raman detection was performed.

[0080] Fig.10 The Raman spectrum of chloramphenicol solid is used as a reference for the characteristic peak. It can be seen from the figure that the Raman characteristic peak of chloramphenicol is 1109cm -1 is the asymmetric stretching vibration of the ring, 1347 cm -1 The characteristic peak is C 14 -H 20 Out-of-plane rocking vibration, 1590 cm -1 The characteristic peak is C 17 -N 18 Ring asymmetric stretching vibration

[0081] Fig.11 Figures e, d and c are the Raman spectra of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag respectively. It can be seen from the figure that the three blank substrates of Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag have no SRES signal, indicating that there is no interference with the SRES signal of chloramphenicol; Fig.11 (b) is the SERS image of pure chloramphenicol solution; Fig.11 (a) Fe3O4 / SiO2 / Ag-chloramphenicol (10 -5 mol / L) Raman spectrum.

[0082] The Fe3O4 / SiO2 / Ag prepared in Example 1 was used as the substrate, and the concentration was 1.0×10 -3 ~1.0×10 - 10 mol / L chloramphenicol solution for Raman analysis, such as Fig.12 As shown, Fig.12 a~h are concentrations of 1.0×10 -3 ~1.0×10 -10 mol / L SERS image of chloramphenicol on Fe3O4 / SiO2 / Ag substrate. It can be seen from the figure that as the CAP concentration gradually decreases, the intensity of the SERS signal also shows a downward trend.

[0083] The SERS signal intensity is used as the ordinate and the negative logarithm of the chloramphenicol concentration is plotted, such as Fig.13 As shown in the figure, a standard curve of the Raman peak intensity of CAP at 1590 cm-1 and the negative logarithm of the concentration was plotted. Through linear regression analysis, the standard curve equation was obtained as follows: y = 48199-4386x, and its correlation coefficient R 2=0.9758, showing a good linear relationship.

[0084] This equation not only confirms the correlation between SERS signal intensity and CAP concentration, but also provides a reliable mathematical model for accurately quantifying CAP concentration.

[0085] Spectral reproducibility is one of the important bases to prove the stability and reproducibility of this method. -4 mol / L chloramphenicol solution was subjected to Raman detection, such as Fig.14 (A) Eight parts of chloramphenicol (10 -4 mol / L) and 14 (B) eight portions of chloramphenicol (10 -4 mol / L) solution at 1590cm -1 The RSD of the Raman peak intensity at is shown.

[0086] The reproducibility of chloramphenicol on Fe3O4 / SiO2 / Ag substrate was tested and it was found that the -1 The reproducibility of the Raman signal intensity was good, and its relative standard deviation (RSD) was 7.2%, indicating that the method had good reproducibility.

[0087] Through the detection of chloramphenicol, when the concentration of CAP has dropped to 1.0×10 -10 mol / L, although the peak intensity is very weak, we can still see the Raman characteristic peak of CAP, which shows that this method has high sensitivity. In addition, by routinely measuring eight groups of samples, the results show that the synthesized material has good stability and the established method has good reproducibility.

[0088] The above results fully demonstrate that this embodiment has established a new method for detecting chloramphenicol with high sensitivity and reproducibility, and the synthesized Fe3O4 / SiO2 / Ag magnetic nanocomposite material exhibits good SERS activity, making it an ideal SERS substrate. The high efficiency of this material enables it to sensitively detect extremely low concentrations of analytes, thus showing great application potential in the field of trace analysis. Its magnetic properties also facilitate the separation and collection of samples, further enhancing its convenience and practicality in practical applications.

[0089] Example 4

[0090] This example tested chloramphenicol in domestic water. The results showed that chloramphenicol was not detected in the water. A spike recovery experiment was also conducted. The results are shown in Table 1.

[0091] Table 1 Spiked recovery

[0092]

[0093] In summary, in the present invention, magnetic ferroferric oxide nanoparticles are synthesized by a coprecipitation method, and then silicon dioxide is effectively loaded on the magnetic nanoparticles, and then nanosilver is loaded by in-situ reduction to form a Fe3O4 / SiO2 / Ag magnetic nanocomposite material.

[0094] The characterization by X-ray powder diffractometer, infrared spectrometer, transmission electron microscope and ultraviolet absorption spectrometer confirmed that the present invention has successfully synthesized a new type of magnetic nanocomposite material Fe3O4 / SiO2 / Ag. The prepared Fe3O4, Fe3O4 / SiO2 and Fe3O4 / SiO2 / Ag materials were used as substrates for comparison and used for the detection of chloramphenicol. The results showed that Fe3O4 / SiO2 / Ag had the best enhancement effect.

[0095] Fe3O4 / SiO2 / Ag was selected as the surface enhanced Raman substrate and used for the quantitative detection of chloramphenicol by the standard curve method. -3 ~1.0×10 -10 mol / L concentration range, it showed a good linear relationship, and a reproducibility experiment was conducted. The results showed that the material was relatively stable and the established method had good reproducibility.

[0096] The present invention not only synthesizes a nanocomposite material with a three-layer structure, but also establishes a new method for detecting antibiotic drugs such as chloramphenicol, and the method has high sensitivity and reproducibility. The new method established is not only used for the detection of antibiotic drugs, but also can be used for the quantitative detection of pollutants such as pesticide residues, food additives, preservatives, organic dyes, etc. This method is expected to be used in future food safety, medical and health, and environmental protection, and provide certain social application value in the protection of human health and ecological environment. .

[0097] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for synthesizing a Fe3O4 / SiO2 / Ag magnetic nanocomposite material, characterized in that: The following steps are involved: S1. Preparation of Fe3O4 magnetic nanoparticles: nitrogen is introduced into deionized water 1 and mechanically stirred, ferrous sulfate and ferric chloride are added and the rotation speed is increased to dissolve to obtain a mixed solution, NaOH solution is added dropwise to the mixed solution after heating at 60°C in a water bath to adjust the pH value, stirring is stopped after sufficient reaction, the water bath temperature is increased to 80°C and fully aged, the entire reaction process is completed under nitrogen protection, after the reaction is completed, the product is cooled to room temperature, separated using a magnet and fully washed, washing is stopped when the supernatant in the product is neutral, and Fe3O4 magnetic nanoparticles are obtained after drying; S2, preparation of Fe3O4 / SiO2: fully dissolve the CTAB added to deionized water 2, then add the Fe3O4 magnetic nanoparticles prepared in S1, add NaOH solution and deionized water 3 after ultrasonic dispersion, heat to 60°C in a water bath and stir thoroughly, then add a mixed solution of ethyl orthosilicate and methanol to obtain a reaction solution, stir thoroughly again in a 60°C water bath, separate using a magnet, wash thoroughly and dry for the first time, reflux the powder obtained by the first drying three times, and dry for the second time to obtain Fe3O4 / SiO2 magnetic nanoparticles S3. Preparation of Fe3O4 / SiO2 / Ag: Add Fe3O4 / SiO2 prepared in S2 to deionized water 4, add KH-550 after ultrasonic dispersion and stir evenly, take AgNO3 and dissolve it in deionized water 5 to obtain AgNO3 solution, take sodium citrate and dissolve it in deionized water 6 to obtain sodium citrate solution, add the AgNO3 solution into a conical flask, heat it in a water bath, add the sodium citrate solution, stir evenly again, then stop the water bath and cool to room temperature, wash thoroughly, separate by magnetic separation and dry, to obtain Fe3O4 / SiO2 / Ag magnetic nanocomposite material.

2. The method for synthesizing the Fe3O4 / SiO2 / Ag magnetic nanocomposite material according to claim 1, characterized in that: The mass volume ratio of the deionized water 1, ferrous sulfate, ferric chloride and NaOH solution in S1 is 75.0 mL: 0.5563 g: 0.7201 g: 10.0 mL, and the concentration of the NaOH solution is 2 mol / L.

3. The method for synthesizing the Fe3O4 / SiO2 / Ag magnetic nanocomposite material according to claim 1, characterized in that: In S1, the time for introducing nitrogen is 30 minutes, the stirring speed is 200 r / min, the increased speed is 1000 r / min, the pH value is 9.0-10.0, the time for sufficient reaction is 30 minutes, the time for sufficient aging is 60 minutes, the detergent used for the washing is deionized water, and the drying temperature is 60°C.

4. The method for synthesizing the Fe3O4 / SiO2 / Ag magnetic nanocomposite material according to claim 1, characterized in that: The mass volume ratio of deionized water 2, CTBA, Fe3O4 magnetic nanoparticles, NaOH solution, deionized water 3, tetraethyl orthosilicate and methanol in S2 is 50.0mL: 0.5001g: 0.0503g: 10.0mL: 400.0mL: 0.5mL: 2.0mL, and the concentration of the NaOH solution is 50mmoL / L.

5. The method for synthesizing the Fe3O4 / SiO2 / Ag magnetic nanocomposite material according to claim 1, characterized in that: The ultrasonic dispersion time in S2 is 15 minutes, the sufficient stirring time is 60 minutes, the sufficient stirring time again is 10 hours, the detergent used for the washing is deionized water and anhydrous ethanol alternately, the first drying temperature is 50°C, the first drying time is 6 hours, the reflux temperature is 80°C, the reflux time is 4 hours, the solvent used for the reflux is acetone, the second drying temperature is 60°C, and the second drying time is 6 hours.

6. The method for synthesizing the Fe3O4 / SiO2 / Ag magnetic nanocomposite material according to claim 1, characterized in that: The mass volume ratio of the deionized water 4, Fe3O4 / SiO2, KH-550, AgNO3, deionized water 5, sodium citrate and deionized water 6 in S3 is 15.0 mL: 0.1023 g: 1.00 mL: 0.0506 g: 75.0 mL: 0.0915 g: 10.0 mL.

7. The method for synthesizing the Fe3O4 / SiO2 / Ag magnetic nanocomposite material according to claim 1, characterized in that: The stirring time in S3 is 6 hours, the water bath heating temperature is 100° C., the re-stirring time is 0.5 hours, the detergent used for the washing is deionized water, the drying temperature is 60° C., and the drying time is 6 hours.

8. An application of the Fe3O4 / SiO2 / Ag magnetic nanocomposite material as claimed in claims 1-7, characterized in that: The Fe3O4 / SiO2 / Ag magnetic nanocomposite material can be used as a substrate for surface enhanced Raman spectroscopy to detect chlorrelin.

Citation Information

Cited By

  • Preparation method and application of Ag / MnFe2O4 composite SERS (Surface Enhanced Raman Scattering) substrate