Method for producing steel bonded body

By configuring carbonaceous material at the steel joint surface and heating it at a specific temperature to generate a liquid phase, a carbon concentration inclined layer is formed, which solves the problem of insufficient joint strength and wear resistance of steel joints and achieves high strength and high wear resistance of steel joints.

CN119035739APending Publication Date: 2024-11-29NETUREN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411380095.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-12
Filing Date
2022-09-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In existing technologies, the joint strength and wear resistance of steel joints are insufficient and difficult to improve effectively.

Method used

By placing carbonaceous material on the steel joint surface and heating it at a temperature of 1150℃ to 1500℃ after overlapping, a liquid phase is generated at the joint surface, forming a concentration-sloping layer with the carbon concentration gradually decreasing from the joint interface. This inhibits the precipitation of hard and brittle solidification structure and cementite, thereby improving the joint strength and wear resistance.

Benefits of technology

It significantly improves the joint strength of steel joints and the wear resistance near the joint, and enhances the ductility and toughness of steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035739A_ABST
    Figure CN119035739A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a steel material assembly and a method for manufacturing a steel material assembly, whereby the joint strength between steel materials can be effectively improved, and the wear resistance of the outer peripheral surface in the vicinity of the joint can also be improved. In order to solve the above-mentioned problem, a steel material bonded body is used which is obtained by bonding a plurality of steel materials to each other, the carbon concentration at the bonding interface between the steel materials being 0.20 mass% or more and 2.10 mass% or less, and the steel material bonded body having a concentration gradient layer in which the carbon concentration decreases as the distance from the bonding interface increases.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with the application date of September 6, 2022, application number 202211098897.7, and invention name “Steel joint and its manufacturing method”. Technical Field

[0002] The present invention relates to a steel material joint body and a method for manufacturing the same. Background Art

[0003] In the past, a method for hot joining of steel materials has been disclosed in which a carbonaceous material is applied or dispersed on the joining surfaces, the hot steel materials are overlapped or butted, and then heated and press-joined in a reducing atmosphere, with the aim of developing a technology that can simply and efficiently join hot steel materials in an actual factory and can obtain a high joining strength to the extent that it does not hinder the subsequent rolling process (see Patent Document 1).

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 6-7970 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, the steel joint obtained by the technology described in Patent Document 1 cannot be said to be a steel joint in which the joint strength between steels is effectively improved. Therefore, an object of the present invention is to provide a steel joint that can effectively improve the joint strength between steels and can also improve the wear resistance of the outer peripheral surface near the joint. In addition, an object of the present invention is to provide a method for manufacturing a steel joint that can effectively improve the joint strength between steels.

[0009] Solutions to Solve Problems

[0010] The steel material joint body of the present invention is obtained by joining a plurality of steel materials together, wherein the carbon concentration at the joining interface between the steel materials is 0.20 mass% or more and 2.10 mass% or less, and the steel material joint body has a concentration gradient layer in which the carbon concentration decreases as the distance from the joining interface increases.

[0011] The steel joint body of the present invention is obtained by joining a plurality of medium carbon steels to each other, and is characterized in that the carbon concentration at the joining interface between the steels is greater than 0.50 mass% and less than 2.10 mass%, and the steel joint body has a concentration gradient layer in which the carbon concentration decreases as it moves away from the joining interface.

[0012] The method for manufacturing a steel joint of the present invention is a method for manufacturing a steel joint obtained by joining a plurality of steels to each other, and is characterized in that it comprises: a configuration step of configuring a carbonaceous substance on a joining surface of at least one of the steels to be joined; an overlapping step of overlapping the joining surfaces of the steels to be joined via the carbonaceous substance; and a heating step of heating the steels after the joining surfaces are overlapped to a maximum reaching temperature of not less than 1150°C and not more than 1500°C, wherein the carbonaceous substance is configured to generate a liquid phase at the joining surface under the condition of the maximum reaching temperature.

[0013] The manufacturing method of the steel joint body of the present invention is a manufacturing method of the steel joint body obtained by joining a plurality of steel materials to each other, wherein the manufacturing method of the steel joint body comprises: a configuration step of configuring a carbonaceous substance on the joint surface of at least one of the steel materials to be joined; a superposition step of making the joint surfaces of the steel materials to be joined overlap by their own weight only by pressing against each other via the carbonaceous substance, or overlapping while applying a pressing load; a heating step of making the steel materials after the joint surfaces overlap each other heat by their own weight only by pressing against each other, or heating by applying a pressing load and heating to the maximum temperature reaching the liquid phase of the carbonaceous substance; and a cooling step of cooling the heated steel materials.

[0014] Effects of the Invention

[0015] According to the present invention, a steel material joint body can be provided which can effectively improve the joint strength between steel materials and can also improve the wear resistance of the outer peripheral surface near the joint portion. In addition, according to the present invention, a method for manufacturing a steel material joint body which can effectively improve the joint strength between steel materials can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a conceptual diagram for explaining a steel material joined product according to an embodiment of the present invention.

[0017] Figure 2 This is a state diagram of an iron-carburizing system for explaining the effect of the present invention.

[0018] Figure 3 This is a conceptual diagram for explaining the effects of the present invention.

[0019] Figure 4 This is a conceptual diagram for explaining the location where the metal (metallographic) structure of a steel material joint is confirmed.

[0020] Figure 5 The test body (steel joint body) prepared in Example 3 Figure 4 (b) shows the metal structure images at the respective locations A, B, and C on the L cross section.

[0021] Figure 6 This is a process flow chart for explaining the method for producing a steel material joined body according to the embodiment of the present invention.

[0022] Figure 7 For more specific description Figure 6 FIG. 1 is a process flow chart of a method for producing a steel material joined body according to an embodiment of the present invention.

[0023] Figure 8 This is a conceptual diagram for explaining a method for producing a steel material joined product according to a specific first embodiment of the present invention.

[0024] Fig. 9 This is a conceptual diagram for explaining a method for producing a steel material joined product according to a specific second embodiment of the present invention.

[0025] Fig.10 This is a state diagram of an iron-carburizing system for explaining the effect of the present invention.

[0026] Fig.11 This is a conceptual diagram for explaining the effects of the present invention.

[0027] Fig.12 This is a photograph of the appearance of the steel material joined body obtained in Example 7.

[0028] Fig.13 This is a diagram for explaining the observation position when confirming the bonding rate and the method of calculating the bonding rate.

[0029] Fig.14 It is a figure explaining the part where the metal structure was confirmed about the steel material joined bodies obtained in Example 7 and Example 8, and the metal structure photograph of the part.

[0030] Fig.15 These are diagrams for explaining the locations where the metal structures of the steel material joined bodies obtained in Examples 9 to 11 were confirmed, and metal structure photographs of the locations.

[0031] Description of reference numerals:

[0032] 1. 1A steel joint

[0033] 10Steel (raw materials)

[0034] 10a Joint surface

[0035] 15 Concentration Tilt Layers

[0036] 20Steel

[0037] 20a joint surface

[0038] 25 concentration tilted layers

[0039] 30 Carbonaceous substances

[0040] 30a bonding interface

[0041] 31Joint

[0042] 40 Carbonaceous substances

[0043] 50Joint interface

[0044] 100 high frequency induction heating

[0045] S100 configuration process

[0046] S 1 10 Overlapping process

[0047] S120 Heating Process

[0048] A Carbon concentration (joining interface)

[0049] B Carbon concentration (concentration gradient layer on the opposite side of the bonding interface)

[0050] X length (steel)

[0051] φ Diameter (Steel)

[0052] γ Austenite phase

[0053] L liquid phase. DETAILED DESCRIPTION

[0054] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0055] (Embodiment of Steel Material Joining Body)

[0056] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0057] Figure 1 This is a conceptual diagram for explaining the steel material joined product according to the present embodiment.

[0058] like Figure 1 As shown in FIG. 1 , the plurality of steel materials 10 and 20 of the steel material joint body 1 of the present embodiment are joined to each other. In addition, the joint interface 30a ( Figure 1 The carbon concentration of the slashed part) Figure 1 The carbon concentration A) shown is 0.20 mass% or more and 2.10 mass% or less. Furthermore, there are concentration gradient layers 15 and 25 in which the carbon concentration decreases as the distance from the bonding interface 30a increases.

[0059] In the steel joint 1 of this embodiment, the carbon concentration of the joint interface 30a is greater than 0.20 mass% and less than 2.10 mass%, so the joint strength between the steels 10 and 20 can be effectively improved, and the wear resistance of the outer peripheral surface near the joint 31 (within the range where the concentration gradient layers 15 and 25 are formed) can also be improved.

[0060] In detail, since the carbon concentration of the joint interface 30a is 2.10 mass% or less, the crystallization of the solidification structure at the joint interface 30a is suppressed. Therefore, the crystallization of the hard and brittle solidification structure can be suppressed in the joint interface 30a, so the joint strength between the steel materials 10 and 20 can be effectively improved. In addition, since the carbon concentration of the joint interface 30a is 0.20 mass% or more, the hardness of the joint interface 30a can be improved. Therefore, the wear resistance of the outer peripheral surface near the joint portion 31 can also be improved.

[0061] The carbon concentration is preferably 0.20 mass% or more and 0.90 mass% or less. By setting the carbon concentration of the joint interface 30a to 0.20 mass% or more and 0.90 mass% or less, the joint strength between the steel materials 10 and 20 can be more effectively improved.

[0062] Specifically, by setting the carbon concentration of the joint interface 30a to 0.90 mass% or less, the precipitation of cementite at the austenite grain boundary is suppressed. Therefore, the precipitation of cementite at the hard and brittle austenite grain boundary can be suppressed at the joint interface 30a, thereby more effectively improving the joint strength between the steel materials 10 and 20.

[0063] The carbon concentration of the joint interface 30a in the steel joint 1 of the present embodiment can be measured by cutting the steel joint 1 along the joint interface 30a, grinding the cross section, and measuring it using an element distribution measuring device such as an electron beam microanalyzer (EPMA) or an energy dispersive X-ray analyzer (EDX). In the present invention, the carbon concentration of the joint interface 30a is a value calculated by measuring five arbitrary locations of the cross section after grinding and using the average value thereof.

[0064] The steel material joint 1 of the present embodiment has the concentration gradient layers 15 and 25 in which the carbon concentration decreases as the distance from the joint interface 30a increases. Therefore, the carbon concentration is high in the joint interface 30a (see Figure 1 The carbon concentration A shown in FIG. 1 is the carbon concentration of the steel materials 10 and 20, thereby effectively improving the bonding strength between the steel materials 10 and 20. In addition, the carbon concentration ( Figure 1Since the carbon concentration B) is lower than that of the joint interface 30a, the raw materials 10 and 20 can be "stretched". Therefore, the steel material joint 1 of the present embodiment can be suitably used for applications requiring "stretching" on the raw materials 10 and 20 sides.

[0065] The concentration gradient layers 15 and 25 are preferably as follows Figure 1 As shown, the carbon concentration continuously decreases as the distance from the bonding interface 30a increases.

[0066] The term "continuously reducing" as used herein refers to Figure 1 As shown, the carbon concentration decreases in proportion from the joint interface 30 a toward the plurality of steel materials (raw materials) 10 , 20 .

[0067] Since the concentration gradient layers 15 and 25 have such a decreasing tendency, in addition to the above-mentioned effects, the ductility and toughness at the bonding interface 30 a are also improved.

[0068] The carbon concentration of the concentration gradient layers 15 and 25 in the steel joint 1 of the present embodiment can be measured by cutting the steel joint 1 along the joint interface 30a, further cutting it along the direction of separation from the surface of the cut joint interface 30a (the direction of the raw materials 10 and 20 side), and then grinding the cross-section cut along the separation direction, and measuring it using an element distribution measuring device such as an electron beam microanalyzer (EPMA) and an energy dispersive X-ray analyzer (EDX).

[0069] In the present invention, in the measurement of the decreasing tendency of the concentration gradient layers 15, 25, the carbon concentrations of any five locations (a total of 10 locations) on the straight line from the carbon concentration of the bonding interface 30a to the carbon concentration of the raw materials 10, 20 in the direction from the bonding interface 30a to the respective sides of the raw materials 10, 20 may be measured using the above-mentioned element distribution measuring device with respect to the cross section in the direction of separation after grinding, and a carbon concentration with respect to the distance may be patterned by taking the distance from the bonding interface 30a as the horizontal axis and the carbon concentration as the vertical axis. Figure 1 This is confirmed by looking at the graph shown.

[0070] In addition, the structural morphology of the joint interface 30a of the steel joint body 1 of the present embodiment can be arbitrary, but the joint interface 30a is preferably composed of pearlite. The pearlite can be obtained by air cooling or slow cooling the steel joint body 1 in the austenite state. The joint interface 30a is composed of pearlite, so the tensile strength and bending strength become higher, so the joint strength of the joint interface 30a can be more effectively improved. It should be noted that the structural morphology of the joint interface 30a can be confirmed by cutting the steel joint body 1 along the joint interface 30a, grinding the cut section, and confirming it using an optical microscope in a state where the ground section is etched with nitric acid.

[0071] The joint interface 30a preferably does not have cementite at the austenite grain boundary. If there is cementite at the grain boundary, cracks may be easily generated during tension and bending starting from the cementite at the grain boundary.

[0072] It should be noted that the above-mentioned "not having" does not mean that there is no grain boundary cementite at all, but that the existence ratio of the grain boundary cementite at the joint interface 30a is less than 10%. Here, the confirmation of the existence ratio of the grain boundary cementite at the joint interface 30a is performed by applying nitric acid to the cross section and then using the point method based on JIS G0555 to the cross section.

[0073] In addition, in the steel material joint 1 of the present embodiment, the material of the joined steel materials (raw materials) 10, 20 is any steel material, and is not particularly limited as long as it is a metal that can be integrated with each other. In addition, the alloy elements other than carbon of the joint interface 30a and the plurality of steel materials (raw materials) 10, 20 before joining are not particularly limited, and for example, they have a composition that generally includes Si: 1.50 mass% or less, Mn: 1.00 mass% or less, and the remainder is composed of Fe and inevitable impurities as specified in JIS G 4051. The shapes of the plurality of steel materials (raw materials) 10, 20 before joining are not particularly limited as long as they each have a joint surface and the joint surfaces overlap each other so as to be integrated with each other. The steel materials (raw materials) 10, 20 can be, for example, cylindrical, prism, threaded, concave and convex, etc.

[0074] Another steel material joined body 1A according to the present embodiment is as follows Figure 1 As shown in FIG. 1 , a plurality of steel materials 10 and 20 made of medium carbon steel are joined to each other. In addition, a joint interface 30a ( Figure 1 The carbon concentration of the slashed part) Figure 1The carbon concentration A) shown is 0.50 mass% or more and 2.10 mass% or less. Furthermore, there are concentration gradient layers 15 and 25 in which the carbon concentration decreases as the distance from the bonding interface 30a increases.

[0075] That is, the steel material joined body 1A has a different range of carbon concentration from that of the steel material joined body 1.

[0076] Thus, when medium carbon steel is used as a plurality of steel materials (raw materials) before joining, it is advantageous to achieve the subject of the present invention by making the carbon concentration 0.50 mass% or more and 2.10 mass% or less. Specifically, since the carbon concentration of the joint interface 30a is 2.10 mass% or less, the crystallization of the solidification structure at the joint interface 30a is suppressed. Therefore, in the joint interface 30a, the crystallization of the hard and brittle solidification structure can be suppressed, so the joint strength between the steel materials 10 and 20 can be effectively improved.

[0077] In addition, since the carbon concentration of the joint interface 30a is 0.50 mass% or more, the hardness of the joint interface 30a can be increased. Therefore, the wear resistance of the peripheral surface near the joint portion 31 can be improved.

[0078] The carbon concentration in the other steel joint 1A of the present embodiment is preferably 0.50 mass% to 0.90 mass%. By setting the carbon concentration of the joint interface 30a to 0.50 mass% to 0.90 mass%, the joint strength between the steels 10 and 20 can be more effectively improved.

[0079] Specifically, by setting the carbon concentration of the joint interface 30a to 0.90 mass% or less, the precipitation of cementite at the austenite grain boundary is suppressed. Therefore, at the joint interface 30a, the precipitation of cementite at the hard and brittle austenite grain boundary can be suppressed, thereby more effectively improving the joint strength between the steel materials 10 and 20.

[0080] In addition, the other steel material joint body 1A of the present embodiment has the concentration gradient layers 15 and 25 in which the carbon concentration decreases as the distance from the joint interface 30a increases. Therefore, the carbon concentration is high at the joint interface 30a (see Figure 1 The carbon concentration A shown in FIG. 1 is the carbon concentration of the steel materials 10 and 20 before joining. Figure 1 Since the carbon concentration B) in the joint interface 30a is lower than that in the joint interface 30a, the raw materials 10 and 20 can be "stretched". Therefore, the steel material joint 1A of the present embodiment can be suitably used for applications requiring "stretching" on the raw materials 10 and 20 sides.

[0081] Preferably, the concentration gradient layers 15 and 25 are similarly formed as in the other steel material joint bodies 1A of the present embodiment. Figure 1 As shown, the carbon concentration continuously decreases as the distance from the bonding interface 30a increases.

[0082] Since the concentration gradient layers 15 and 25 have such a decreasing tendency, in addition to the above-mentioned effects, the ductility and toughness at the bonding interface 30 a are also improved.

[0083] In addition, the carbon concentrations of the joint interface 30a and the concentration gradient layers 15 and 25 can be measured under the same conditions and method as those of the steel joint 1 of the present embodiment described above.

[0084] It should be noted that the medium carbon steel referred to in the present invention refers to a steel material having a carbon concentration of 0.30 mass% or more and 0.50 mass% or less. For reference, low carbon steel refers to a steel material having a carbon concentration of less than 0.30 mass%, and high carbon steel refers to a steel material having a carbon concentration of more than 0.50 mass%. In addition, the metal structure of the joint interface 30a of the other steel joint body 1A of the present embodiment is the same as that of the steel joint body 1 of the present embodiment described above, so the description here is omitted.

[0085] Hereinafter, a mechanism by which the joining force between steel materials is improved in the steel material joined bodies 1 and 1A according to the present embodiment will be described using the drawings.

[0086] Figure 2 This is a state diagram of an iron-carburizing system for explaining the effect of the present invention. Figure 3 This is a conceptual diagram for explaining the effect of the present invention, and more specifically, it is a conceptual diagram showing the reaction occurring at the joint interface. As a method for manufacturing the steel joint body 1, 1A of the present embodiment, carbon powder (carbonaceous material) is arranged on the joint surface of at least one of the steels to be joined, and the steels after the joint surfaces of the steels to be joined are overlapped with each other through the carbonaceous material are heated in a predetermined atmosphere (for example, in an atmospheric atmosphere) at a maximum reaching temperature of 1150°C or higher and 1500°C or lower (preferably, 1150°C or higher and 1300°C or lower) (refer to Figure 3 (a)).

[0087] When the temperature of the joint surface between the steel materials reaches, for example, 1250°C, a liquid phase L having a carbon concentration of 3.5 mass% is generated at the interface between the steel material and the carbonaceous material (see Figure 2 The liquid phase L increases until the carbonaceous material is exhausted (refer to Figure 3 (b)).

[0088] It should be noted that the interface between the "austenite γ phase" region and the "austenite γ phase + liquid phase L" region under the condition of 1250°C (refer to Figure 2 The carbon concentration of the portion indicated by ○ in the figure is 1.6 mass% (refer to Figure 2 ). Carbon diffusion is extremely fast under 1250℃. When this temperature is maintained, carbon diffuses rapidly from the joint surface of the steel to the austenite γ phase inside. As a result, at the interface between the liquid phase L and the austenite γ phase, the austenite γ phase side maintains the carbon concentration at 1.6 mass% and takes carbon from the liquid phase L side. On the other hand, the liquid phase L decreases because the carbon concentration of the liquid phase L is maintained at 3.5 mass% (refer to Figure 3 Finally, the liquid phase L disappears and the joining of the steel materials is completed (refer to Figure 3 (d)).

[0089] It should be noted that there is a case where the carbon concentration of the joint surface is high just after the liquid phase L disappears. In addition, in the case of suppressing the precipitation of the above-mentioned grain boundary cementite, in the steel joint 1, the carbon concentration of the joint interface needs to be reduced to 0.20 mass% or more and 0.90 mass% or less. In addition, in the steel joint 1A, the carbon concentration needs to be reduced to 0.50 mass% or more and 0.90 mass% or less. The reduction of the carbon concentration at the joint interface can be controlled by lengthening the heating maintenance time under the condition of the maximum reached temperature.

[0090] It should be noted that the carbonaceous material mentioned here is not particularly limited in material and shape as long as it is disposed on at least one of the joining surfaces of the joined steel materials and the joining surfaces can be integrated with each other. The carbonaceous material can be, for example, graphite particle powder (carbon powder) with an average particle size of 1 μm.

[0091] (Embodiment of the method for producing a steel material joint)

[0092] Figure 6 This is a process flow chart for explaining the method for producing a steel material joined body according to the embodiment of the present invention.

[0093] The method for manufacturing the steel material joint body according to the present embodiment is as follows Figure 6 A method for manufacturing a steel material joint body obtained by joining a plurality of steel materials to each other as shown in the figure, wherein the method for manufacturing a steel material joint body comprises: a configuration step of configuring a carbonaceous material on a joining surface of at least one of the steel materials to be joined ( Figure 6 step S100 shown); a superposition process ( Figure 6and heating the steel material having the joint surfaces overlapped with each other to a maximum reaching temperature of 1150°C or more and 1500°C or less ( Figure 6 Step S120 shown).

[0094] Furthermore, in the method for producing a steel material joined body of the present embodiment, in the arrangement step (step S100 ), the carbonaceous material is arranged so that a liquid phase is generated at the joining surface under the condition of the highest reaching temperature.

[0095] The method for producing a steel material joined body of the present invention can effectively improve the joining strength between steel materials by including the above-mentioned process flow.

[0096] Figure 7 For more specific description Figure 6 FIG. 1 is a process flow chart of a method for producing a steel material joined body according to an embodiment of the present invention.

[0097] The method for manufacturing the steel material joint body according to the present embodiment is as follows Figure 7 A method for manufacturing a steel material joint body obtained by joining a plurality of steel materials to each other as shown in the figure, wherein the method for manufacturing a steel material joint body comprises: a configuration step of configuring a carbonaceous material on a joining surface of at least one of the steel materials to be joined ( Figure 7 step S100 shown); a superposition process ( Figure 7 Step S110 shown); a heating step (a) of pressing the steel materials whose joint surfaces overlap each other and heating them by their own weight to the maximum temperature at which the liquid phase of the carbonaceous material is generated, or heating them to the maximum temperature at which the liquid phase of the carbonaceous material is generated while applying a pressing load. Figure 7 Step S120 shown); and a cooling step ( Figure 7 Step S130 shown).

[0098] The method for producing a steel material joint of the present invention can easily and effectively improve the joining strength between steel materials by including the above-mentioned process flow.

[0099] Hereinafter, each of the above steps will be described in detail.

[0100] Figure 8 This is a conceptual diagram for explaining a method for producing a steel material joined product according to a specific first embodiment of the present invention. Fig. 9 This is a conceptual diagram for explaining a method for manufacturing a steel material joint according to a specific second embodiment of the present invention. Figure 8 The first embodiment shown is Fig. 9In the second embodiment shown, only the form of the carbonaceous material disposed on the joining surface of the steel material is made different.

[0101] <About the Arrangement Process (Step S100)>

[0102] In the method for manufacturing the steel material joint 1 of the first and second embodiments, in the arrangement step (step S100), as shown in FIG. Figure 8 (a) and Fig. 9 As shown in (a) of FIG. 1 , at least one of the joining surfaces (10a and / or 20a: at least one of the steel materials (10, 20) to be joined has a Figure 8 (a) and Fig. 9 In addition, at this time, the carbonaceous material is configured to generate a liquid phase L (refer to Fig.10 : described later).

[0103] By arranging in this way, the joining strength between the steel materials can be more effectively improved.

[0104] Here, the material of the steel materials (10, 20) to be joined may be any steel material as long as they are metals that can be integrated with each other, and is not particularly limited. For example, low carbon steel, medium carbon steel, high carbon steel, etc. can be used.

[0105] It should be noted that the medium carbon steel mentioned in the present invention refers to a steel material having a carbon concentration of 0.30 mass% or more and 0.50 mass% or less. In addition, low carbon steel refers to a steel material having a carbon concentration of less than 0.30 mass%, and high carbon steel refers to a steel material having a carbon concentration of more than 0.50 mass%. In addition, when low carbon steel, medium carbon steel and high carbon steel are used, the alloy elements other than the carbon are not particularly limited. For example, a composition as specified in JIS G 4051 can be adopted, which generally includes Si: less than 1.5 mass%, Mn: less than 1.0 mass%, and the remainder is composed of Fe and inevitable impurities.

[0106] The shape of the steel materials (10, 20) is not particularly limited as long as they have joint surfaces (10a, 20a) respectively and the joint surfaces (10a and 20a) overlap and can be integrated with each other. For example, a cylindrical shape, a prism shape, a threaded shape, a concave-convex shape, etc. can be used.

[0107] In addition, the carbonaceous material (30, 40) is not particularly limited in material and shape as long as it can be arranged on the joint surface (10a and / or 20a) of at least one of the steel materials (10, 20) to be joined and the joint surfaces (10a and 20a) can be integrated. Figure 8 The powdered carbonaceous material (30) shown, Fig. 9 The flaky carbonaceous material (40) shown. Here, when a powdered carbonaceous material (30) is used, it can be configured by applying it to the joint surface (10a and / or 20a). When a flaky carbonaceous material (40) is used, it can be directly configured on the joint surface (10a and / or 20a).

[0108] <About Overlapping Process (Step S110)>

[0109] In the method for manufacturing the steel material joint 1 of the first and second embodiments, in the overlapping step (step S110), as shown in FIG. Figure 8 (b) and Fig. 9 As shown in (b), the joining surfaces (10a and 20a) of the steel materials (10, 20) to be joined are overlapped with each other via the carbonaceous material (30 or 40) arranged by the "arrangement step (step S100)". In the overlapping step (step S110), when the joining surfaces (10a and 20a) of the steel materials (10, 20) are overlapped with each other, it is preferred to apply a load to fix the joining surfaces to each other. In the overlapping step of the present embodiment, by applying a load to fix the joining surfaces (10a and 20a) of the steel materials (10, 20) to each other, the joining force between the steel materials (10 and 20) can be improved.

[0110] More specifically, in the method for manufacturing the steel material joint 1 of the first and second embodiments, in the overlapping step (step S110), Figure 8 (b) and Fig. 9 As shown in (b), the carbonaceous material (30 or 40) arranged in the "arrangement step (step S100)" causes the joining surfaces (10a and 20a) of the steel materials (10, 20) to be joined to overlap by simply pressing against each other.

[0111] In the overlapping step (step S110), when the joining surfaces (10a and 20a) of the steel materials (10, 20) are overlapped only by pressing against each other, it is preferred that the joining surfaces are fixed by their own weight. In the overlapping step of the present embodiment, by fixing the joining surfaces (10a and 20a) of the steel materials (10, 20) by their own weight, the joining force between the steel materials (10 and 20) can be improved.

[0112] In addition, in the overlapping process (step S110), when the joining surfaces (10a and 20a) of the steel materials (10, 20) are overlapped only by pressing each other, it is preferable to apply a load (pressing load) to fix the joining surfaces to each other. In the overlapping process of the present embodiment, by applying a load to fix the joining surfaces (10a and 20a) of the steel materials (10, 20) to each other, the joining force of the steel materials (10 and 20) can be improved. In addition, when such a pressing load is applied, the overlapping of the joining surfaces (10a and 20a) of the steel materials (10, 20) can be performed without being performed at the same time. Figure 8 , Fig. 9 It is preferably performed in the horizontal direction (not shown) rather than in the vertical direction as shown.

[0113] Furthermore, in the superposition process of this embodiment, it is preferable to adjust the inclination of the joining surface of the steel materials to be joined during the pressing. By adjusting the inclination of the joining surface in this way, the joining strength between the steel materials can be more effectively improved.

[0114] <About the heating process (step S120)>

[0115] In the method for manufacturing the steel material joint 1 of the first and second embodiments, in the heating step (step S120), Figure 8 (c) and Fig. 9 As shown in (c) of FIG. 1 , the steel materials (10, 20) whose joint surfaces (10a and 20a) are overlapped by the "overlapping step (step S110)" are heated. Here, the maximum temperature reached by heating the steel materials (10, 20) is within the range where the liquid phase L is generated at the joint surface 50 (refer to Fig.10 , see below).

[0116] More specifically, in the method for manufacturing the steel material joint 1 of the first and second embodiments, in the heating step (step S120), Figure 8 (c) and Fig. 9 As shown in (c) of FIG. 1 , the steel materials (10, 20) whose joint surfaces (10a and 20a) are overlapped in the "overlapping process (step S110)" are simply pressed against each other and heated while the joint surfaces are fixed to each other by their own weight. Here, the maximum temperature reached by heating the steel materials (10, 20) is within the range where the liquid phase L is generated at the joint surface 50 (refer to Fig.10 , see below).

[0117] In the heating, it is preferred that the steel materials (10, 20) whose joint surfaces (10a and 20a) overlap each other are simply pressed against each other and heated while applying a load (pressing load) to fix the joint surfaces against each other.

[0118] By applying a load to fix the steel materials (10, 20) whose joint surfaces (10a and 20a) overlap each other and heating them in this way, the joining force between the steel materials (10 and 20) can be improved. In addition, when such a pressing load is applied, the heating of the joint surfaces (10a and 20a) of the steel materials (10, 20) can be performed without being too long. Figure 8 , Fig. 9 It is preferably performed in the horizontal direction (not shown) rather than in the vertical direction as shown.

[0119] As described above, in the arrangement step (step S100 ), the carbonaceous material is arranged by adjusting the mass of the carbonaceous material so that the liquid phase L is generated on the joint surface 50 under the condition of the highest reaching temperature during heating in the heating step (step S120 ).

[0120] Therefore, since such a carbonaceous material is arranged on the joint surface, the carbon concentration of the joint surface 50 becomes high. Therefore, the tensile strength and bending strength of the joint surface 50 become high, and thus the joint surface 50, that is, the joint strength between the steel materials can be effectively improved.

[0121] It should be noted that, in order to adjust the mass of the carbonaceous material, the joint surface 50 is configured so as to generate a liquid phase L under the condition of the highest reaching temperature when the carbonaceous material is heated (see Fig.10 ), for example, the mass of the carbonaceous material can be determined by using a raw material, i.e., steel (10, 20), having the same shape and carbon concentration as the steel joint body to be the product, and changing the mass of the carbonaceous material arranged on the joint surface 50 and performing heating joint tests on them at the same maximum reaching temperature, and evaluating the joint rate described later, thereby determining the appropriate mass of the carbonaceous material for generating the liquid phase L.

[0122] The carbonaceous material is preferably arranged so as to generate a liquid phase over the entire joint surface under the condition of the maximum reaching temperature.

[0123] By arranging the carbonaceous material so as to generate a liquid phase over the entire joining surface, the entire joining surface can be joined, thereby more effectively improving the joining strength between the steel materials.

[0124] The heating mechanism in the heating process (step S120) is not particularly limited as long as it does not impair the effect of the present invention. Various heating methods such as high-frequency induction heating (100) using a heating coil 60, a heating furnace other than high-frequency induction heating, laser heating, etc. can be used.

[0125] In addition, the atmosphere during heating in the heating step (step S120 ) is not particularly limited.

[0126] The atmosphere includes, for example, an oxidizing atmosphere (oxygen, air, etc.) and a non-oxidizing atmosphere (nitrogen, argon, etc.).

[0127] The heating step (step S120) of the present invention is preferably performed by high-frequency induction heating (100). High-frequency induction heating (100) can accurately and rapidly heat to a desired temperature, and thus can manufacture the above-mentioned steel material joint (1).

[0128] Furthermore, in the heating step (step S120) of the present invention, at the stage where the liquid phase L generated at the joint surface 50 of the steel materials (10, 20) disappears, the steel materials (10 and 20) are joined ( Figure 8 (d) and Fig. 9 (d)). The cooling mechanism after the heating in the heating step (step S120) of the present invention is not particularly limited, and conventionally known gas cooling, spray cooling using a coolant such as a polymer, etc., can be used.

[0129] More specifically, the heated Figure 7 The cooling process (step S130 ) shown is not particularly limited, and conventionally known natural cooling, gas cooling, spray cooling using a quenching coolant such as a polymer, or the like can be employed.

[0130] The above has described each process included in the present invention. Next, a specific example of the mechanism by which the joining force of steel materials can be improved by performing each process described above will be described using the drawings.

[0131] Fig.10 This is a state diagram of an iron-carburizing system for explaining the effect of the present invention. Fig.11 1 is a conceptual diagram for explaining the effect of the present invention, and more specifically, is a conceptual diagram showing the reaction occurring at the joint interface. As a method for manufacturing a steel joint body 1 of the present embodiment, a carbon powder (carbonaceous material) whose mass is adjusted to generate a liquid phase L under the condition of the highest reaching temperature during heating is arranged on the joint surface of at least one of the steel materials to be joined, and the steel materials after the joint surfaces of the steel materials to be joined are overlapped with each other via the carbonaceous material are heated at a predetermined maximum reaching temperature under a predetermined atmosphere (for example, in an atmospheric atmosphere) (refer to Fig.11 (a)).

[0132] according to Fig.10 The temperature at which the liquid phase L is generated at the joint interface between the steel material and the carbonaceous material is 1150° C. or higher and 1500° C. or lower.

[0133] Specifically, when the maximum temperature near the joint surface of the steel materials reaches 1250°C, for example, a liquid phase L having a carbon concentration of 3.5 mass% is generated at the interface between the steel material and the carbonaceous material (see Fig.10 The liquid phase L increases until the carbonaceous material disappears (refer to Fig.11 (b)).

[0134] The interface between the "austenite γ" region and the "austenite γ + liquid L" region at 1250°C (refer to Fig.10 The carbon concentration of the steel (indicated by ○ in the figure) is 1.6 mass%. Therefore, under the condition of 1250°C, the steel almost becomes a single phase of austenite γ. In addition, when the carbon content exceeds 1.6 mass%, two phases of austenite γ and liquid phase L coexist. The diffusion of carbon under the condition of 1250°C is extremely fast. When this temperature is maintained, carbon diffuses rapidly from the joint surface of the steel to the austenite γ inside. As a result, at the interface between the liquid phase L and the austenite phase γ, the austenite phase γ side maintains the carbon concentration at 1.6 mass% and takes carbon from the liquid phase L side. In addition, since the liquid phase L maintains the carbon concentration at 3.5 mass%, the liquid phase L decreases (refer to Fig.11 (c)). The liquid phase L eventually disappears and the joining of the steel materials is completed (refer to Fig.11 (d).

[0135] The effect of the present invention in the heating step (step S120) of the present invention is described with the maximum reaching temperature of 1250°C. Fig.10 According to the state diagram of the iron-carburizing system and the embodiments described later, the above-mentioned effect of the present invention is obtained within the temperature range of forming the "austenite phase γ" region and the "austenite phase γ+liquid phase L" region (the highest reached temperature is above 1150°C and below 1500°C).

[0136] As described above, the mass of the carbonaceous material is adjusted and arranged so that the liquid phase L is generated at the joining surface, and the steel materials whose joining surfaces are overlapped are heated under the condition of a maximum reaching temperature of 1150° C. to 1500° C., thereby enabling the above-mentioned joining to be performed.

[0137] The maximum temperature reached is preferably above 1150°C and below 1300°C. By setting the maximum temperature reached below 1300°C, the heating member (coil, etc.) used to heat the steel can be efficiently cooled, and deformation caused by the heat of the steel joint itself can also be suppressed. It should be noted that the maximum temperature reached in the heating step (S120) can be measured by a platinum-rhodium thermocouple welded on the outer peripheral surface of the steel (raw material) side within 2 mm from the joining surface 50 of the steel to be joined.

[0138] Next, the present invention will be described in more detail by way of Examples and Comparative Examples. However, the present invention is not limited to these Examples at all.

[0139] [Example]

[0140] (Examples (1 to 6) and Comparative Examples (1 to 2) of Steel Material Joining Body)

[0141] [Example 1]

[0142] In Example 1, Figure 1 Two steel materials (low carbon steel) with a carbon concentration of 0.045 mass% were prepared in the shape of a cylinder (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown in the figure. Then, the two steel materials were joined together to produce a test body. Figure 1 The steel joint body is as shown in the figure 1. At this time, carbon powder (carbonaceous material) is arranged on the joint surface of each of the two steels, and the joint surfaces of the steels to be joined are overlapped with each other through the carbonaceous material. Next, high-frequency induction heating is performed at a maximum reaching temperature of 1250°C in an air atmosphere, and then slow cooling is performed. Here, the mass of the carbon powder arranged on the joint surface of each of the two steels is adjusted to be able to produce Figure 2 and Figure 3 The carbon concentration of the bonding interface after high-frequency induction heating was adjusted to 0.20 mass % by controlling the heating maintenance time under the condition of the highest reached temperature.

[0143] In Example 1, the following “confirmation of joining strength and wear resistance” was performed on the test body (steel material joined body) produced.

[0144] (Confirmation of the presence or absence of a concentration gradient layer, the main structure of the bonding interface, and the bonding strength and wear resistance)

[0145] The presence or absence of a concentration gradient layer (a concentration gradient layer in which the carbon concentration decreases as the distance from the bonding interface is increased) and the main microstructure of the bonding interface, bonding strength (○ high, Δ low), and wear resistance (○ high, Δ low) were confirmed for the prepared test bodies (steel joints). Figure 1 Based on the graph shown, the determination was made by whether there was a decreasing trend in carbon concentration. The main organizational structure (metal structure) of the joint interface was confirmed by observing the predetermined parts of the joint interface of the produced steel joint body with an optical microscope while etching with nitric acid. Figure 4 A diagram is shown to illustrate the location where the metal structure is confirmed. Figure 4 The steel material joint shown in (b) is as follows Figure 4As shown in (a), the steel joint body is cut in an L-section, and the metal structure images at the respective positions A, B, and C on the L-section are image processed, thereby confirming the presence or absence of metal structures (pearlite, etc.) in each image. Regarding the joint strength, it was measured and evaluated as tensile strength. The tensile strength was tested using JIS 9 No. A (G.L100mm). In addition, regarding wear resistance, a wear tester was used to adjust the speed and final load in a dry environment. The target material used a grinding wheel made of cubic silicon nitride with a grain size number of 400, and the relative wear amount of the outer peripheral surface of the joint was evaluated. The results of the confirmation of the above-mentioned confirmation items are shown in Table 1 shown below.

[0146] [Example 2]

[0147] In Example 2, Figure 1 Two steel materials (medium carbon steel) with a carbon concentration of 0.450 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 0.50 mass%. Otherwise, a test body (steel joint body) was produced under the same conditions and methods as Example 1.

[0148] In Example 2, similarly to Example 1, "confirmation of the presence or absence of a concentration gradient layer, the main organizational structure of the bonding interface, bonding strength, and wear resistance" was performed. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description related to the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Example 2 are shown together with the confirmation results of Example 1.

[0149] [Example 3]

[0150] In Example 3, Figure 1 Two steel materials (medium carbon steel) with a carbon concentration of 0.450 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown in the figure. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 0.90 mass%. Otherwise, the test body (steel joint body) was produced under the same conditions and method as Example 1.

[0151] In Example 3, similarly to Example 1, "confirmation of the presence or absence of a concentration gradient layer, the main organizational structure of the bonding interface, bonding strength, and wear resistance" was performed. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description related to the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Example 3 are shown together with the confirmation results of Example 1.

[0152] It should be noted that, for reference, the test body (steel joint body) prepared in Example 3 Figure 4 The metal structure images at the A, B, and C positions on the L section shown in (b) are shown in FIG. Figure 5 middle.

[0153] [Example 4]

[0154] In Example 4, Figure 1 Two steel materials (medium carbon steel) with a carbon concentration of 0.450 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown in the figure. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 1.30 mass%. Otherwise, the test body (steel joint body) was produced under the same conditions and method as Example 1.

[0155] In Example 4, similarly to Example 1, "confirmation of the presence or absence of a concentration gradient layer, the main organizational structure of the bonding interface, bonding strength, and wear resistance" was performed. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description related to the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Example 4 are shown together with the confirmation results of Example 1.

[0156] [Example 5]

[0157] In Example 5, Figure 1 Two steel materials (medium carbon steel) with a carbon concentration of 0.450 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 1.70 mass%. Otherwise, a test body (steel joint body) was produced under the same conditions and method as Example 1.

[0158] In Example 5, similarly to Example 1, "confirmation of the presence or absence of a concentration gradient layer, the main organizational structure of the bonding interface, bonding strength, and wear resistance" was performed. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description related to the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Example 5 are shown together with the confirmation results of Example 1.

[0159] [Example 6]

[0160] In Example 6, Figure 1 Two steel materials (medium carbon steel) with a carbon concentration of 0.450 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 2.10 mass%. Otherwise, a test body (steel joint body) was produced under the same conditions and method as Example 1.

[0161] In Example 6, similarly to Example 1, "confirmation of the presence or absence of a concentration gradient layer, the main organizational structure of the bonding interface, bonding strength, and wear resistance" was performed. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description related to the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Example 6 are shown together with the confirmation results of Example 1.

[0162] [Comparative Example]

[0163] [Comparative Example 1]

[0164] In Comparative Example 1, Figure 1 Two steel materials (low carbon steel) with a carbon concentration of 0.045 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 0.10 mass%. Otherwise, a test body (steel joint body) was produced under the same conditions and method as Example 1.

[0165] In Comparative Example 1, the "confirmation of the presence or absence of the concentration gradient layer, the main organizational structure of the bonding interface, the bonding strength and the wear resistance" was performed in the same manner as in Example 1. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description related to the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Comparative Example 1 are shown together with the confirmation results of Example 1.

[0166] [Comparative Example 2]

[0167] In Comparative Example 2, Figure 1 Two steel materials (medium carbon steel) with a carbon concentration of 0.450 mass% were prepared in a cylindrical shape (length X: 150 mm, diameter φ: 15 mm (diameter of the joint surface)) as shown. In addition, by controlling the heating maintenance time under the condition of the highest reached temperature, the carbon concentration of the joint interface after high-frequency induction heating was adjusted to 2.30 mass%. Otherwise, a test body (steel joint body) was produced under the same conditions and method as Example 1.

[0168] In Comparative Example 2, similarly to Example 1, "confirmation of the presence or absence of a concentration gradient layer, the main organizational structure of the bonding interface, bonding strength, and wear resistance" was performed. Here, when performing this confirmation, the same conditions and methods as in Example 1 were used. Therefore, the description of the conditions and methods is omitted. In Table 1 shown below, the confirmation results of Comparative Example 2 are shown together with the confirmation results of Example 1.

[0169]

Table 1

[0170]

[0171] (Results and Investigation)

[0172] From the results in Table 1, it can be seen that when the carbon concentration of the joint interface of the test body (steel joint body) is 0.20 mass% or more and 2.10 mass% or less (Examples 1 to 6), it is confirmed that the joint strength and wear resistance are high. On the other hand, in Comparative Example 1, since the carbon concentration of the joint interface is low, it is confirmed that the wear resistance is reduced. In addition, in Comparative Example 2, crystallization of the solidified structure is confirmed as the structure of the joint interface, so it is confirmed that the joint strength is reduced.

[0173] In addition, in the steel joints of Examples 4 to 6, in addition to pearlite, cementite (including cementite at the austenite grain boundary) was also confirmed as the main structure of the joint interface. On the other hand, in the steel joints of Examples 1 to 3, pearlite was confirmed as the main structure of the joint interface, and cementite was not confirmed. Therefore, it is believed that the steel joints of Examples 1 to 3 in which hard and brittle cementite is not confirmed (the case where the carbon concentration of the joint interface is 0.20 mass% or more and 0.90 mass% or less) have higher joint strength and wear resistance. Moreover, based on the confirmation results, it is believed that in the case where the steel to be joined uses medium carbon steel, the carbon concentration of the joint interface is 0.50 mass% or more and 0.90 mass% or less in terms of achieving the subject of the present invention.

[0174] (Examples (7 to 11) and Comparative Examples (3 and 4) of the Method for Producing Steel Joined Products)

[0175] [Example 7]

[0176] In Example 7, two S45C steel materials (medium carbon steel) were prepared with round bars of a size of φ14.7 mm in diameter of the joint surface and L47 mm in length in the axial direction. Furthermore, the joint surfaces of the S45C steel materials were overlapped and heatedly joined via a carbonaceous material (PGS graphite sheet manufactured by Panasonic Corporation) of a size of 20 mm in length, 20 mm in width, and 16 μm in thickness. The mass (gram weight) of the graphite sheet was adjusted to a carbon concentration that generates a liquid phase L at the joint surface of the steel materials under the condition of the following maximum reaching temperature (1250° C.).

[0177] The maximum temperature described below was measured by welding a platinum-rhodium thermocouple to the outer peripheral surface of the S45C steel material within 2 mm from the position to be the joining surface of the steel material.

[0178] In summary, if Figure 6 As shown in the process flow, the configuration process (step S100), the overlapping process (step S110), and the heating process (step S120) are performed in sequence.

[0179] More specifically, if Figure 7 As shown in the process flow, the cooling process (step S130) is performed after the heating process (step S120). In the overlapping process, the joining surfaces of the steel materials to be joined are only pressed against each other through the carbonaceous material and overlapped under the condition of a pressure of 7.0 MPa, that is, while applying a pressing load.

[0180] In the heating process, the S45C steel materials were heated to a maximum temperature of 1250°C in 20 seconds by high-frequency induction heating at a frequency of 10 kHz in an atmospheric atmosphere, and the temperature was maintained for 20 seconds before air cooling to room temperature. The heating in the atmospheric atmosphere caused the joint surfaces of the S45C steel materials separated by the carbonaceous material to be heat-joined while being pressurized at a pressure of 7.2 MPa (a load for fixing the joint interface).

[0181] More specifically, in the heating process, the S45C steel materials were heated to a maximum temperature of 1250°C in 20 seconds by high-frequency induction heating at a frequency of 10 kHz in an air atmosphere, and the temperature was maintained for 20 seconds before air cooling to room temperature. During the heating in the air atmosphere, the joint surfaces of the S45C steel materials separated by the carbonaceous material were only pressed against each other and heated and joined under a pressure of 7.2 MPa (a load for fixing the joint interface), that is, while applying a pressing load. In the cooling process, at least the joint surface of the heated steel material was cooled by natural cooling.

[0182] In Example 7, the steel material joined body obtained through the above-mentioned steps was used as a test body.

[0183] The appearance of the steel material joined product obtained in Example 7 was observed using a camera. Fig.12 The following is a photograph of the appearance of the steel material joint obtained in Example 7. In Example 7, the joining rate of the obtained steel material joint was confirmed. Here, the joining rate was confirmed by observing the joining interface of the obtained steel material joint in a non-etched state using an optical microscope. Fig.13 2 shows a diagram for explaining the observation position when confirming the bonding rate and the method of calculating the bonding rate.

[0184] like Fig.13 As shown in (a), the observation position for confirming the bonding rate is as follows Fig.13 As shown in (a) of FIG. 1 , the steel material joint body is cut in an L-section parallel to the central axis α. As for the joining rate, Fig.13 As shown in (b), when d is the diameter of the steel joint body and Lv is the length of the gap, the joining rate is calculated by "(d-∑Lv) / d×100" using these values. In Table 2 shown below, the results after confirming the joining rate are shown together with other results.

[0185] In Example 7, the metal structure of the obtained steel material joint body at the joint interface was confirmed. Here, in the confirmation of the metal structure, the steel material joint body after heat joining was observed with a camera in a non-etched state. Fig.13 A predetermined portion at the bonding interface of the surface after cutting in an L-section as shown in (a). Fig.14 A diagram illustrating a location where metal structure confirmation is performed and a metal structure photograph of the location are shown. Fig.14 The steel material joint shown in (a) is as follows Fig.13The steel joint body is cut at the joint interface as shown in (a) of FIG. 1 , and the metal structure is confirmed at each of the A, B, and C positions on the cross section of the joint interface. Fig.14 In (b), the metal structure photographs of the respective parts A, B, and C are shown together with other metal structure photographs.

[0186] [Example 8]

[0187] In Example 8, the "joining rate" and "metal structure at the joint interface" of the obtained steel material joint were confirmed in the same manner as in Example 7. Here, the same method as in Example 7 was used to confirm these. Therefore, the description of the above methods is omitted.

[0188] In Example 8, as in Example 7, Figure 6 (Specifically, Figure 7 ) are sequentially performed as shown in the process flow of ). In Example 8, the condition different from that in Example 7 is that the heating in the heating process is performed in a nitrogen atmosphere. In the heating in the nitrogen atmosphere, the flow rate of nitrogen is 100 L / min, and the joint surfaces of the S45C steel material separated by the carbonaceous material are pressurized at a pressure of 7.2 MPa (a load for fixing the joint interface) while being heated and joined.

[0189] In Table 2 shown below, the results of confirming the bonding rate are shown together with the results of Example 7. Fig.14 A diagram illustrating a location where metal structure confirmation is performed and a metal structure photograph of the location are shown together with the metal structure photograph of Example 7.

[0190]

Table 2

[0191]

[0192] (Results and Evaluation)

[0193] according to Fig.12 In the steel material joint obtained in Example 7, it can be confirmed that the round bars are joined to each other. In addition, according to Table 2, no significant difference is confirmed between Example 7 and Example 8 regarding the joining rate of the steel material joint. Fig.14 Regarding the metal structure of the joint interface portion of the steel material joint body, it was confirmed that there was no significant difference between Example 7 and Example 8, and that a pearlite phase was formed in both.

[0194] [Example 9 to Example 11]

[0195] The maximum reaching temperature was changed to 1150°C (Example 9), 1200°C (Example 10), and 1300°C (Example 11), and the other heat joining was performed in the same process and conditions as in Example 8. The steel joint bodies obtained by heat joining were used as test bodies under the conditions of the respective maximum reaching temperatures. The "joining rate" and "metal structure at the joint interface" of each obtained steel joint body were confirmed in the same way as in Example 7. Here, the same method as in Example 7 was used to perform these confirmations. Therefore, the description related to the above-mentioned methods is omitted.

[0196] In Table 3 shown below, the results of Examples 9 and 11 after confirming the bonding rates are collectively shown. Fig.15 A diagram illustrating a location where metal structure confirmation is performed and metal structure photographs of each of Examples 9 to 11 at that location are also shown.

[0197]

Table 3

[0198]

[0199] (Results and Evaluation)

[0200] According to Table 3, no significant difference was observed in the joining ratio of the steel material joints between Examples 9 and 11. No significant difference was observed between Examples 9 and 11 and Examples 7 and 8. Fig.15 Regarding the metal structure of the joint interface portion of the steel joint body, it was also confirmed that there was no significant difference in Examples 9 to 11, and between Examples 9 to 11 and Examples 7 and 8, and that pearlite phase was formed in all of them.

[0201] [Comparative Example 3]

[0202] In Comparative Example 3, the maximum reaching temperature was set to 1100° C., and heat bonding was performed in the same process flow and conditions as in Example 8. As a result, bonding as shown in Examples 7 to 11 was not confirmed, and the bonding rate was 0%.

[0203] [Comparative Example 4]

[0204] Heat bonding was performed in the same process flow and conditions as in Example 8 except that the graphite sheet of Example 7 was not used.

[0205] As a result, bonding as shown in Examples 7 to 11 was not confirmed, and the bonding rate was 0%.

[0206] From the above results, it is understood that the method for producing a steel material joined product of the present invention can effectively improve the joining strength between steel materials by preferably setting the maximum reaching temperature to 1150° C. or higher and 1300° C. or lower.

[0207]

Industrial Applicability

[0208] According to the method for manufacturing a steel material joint of the present invention, the joining strength between steel materials can be effectively improved. Specifically, according to the method for manufacturing a steel material joint of the present invention, the joining strength between steel materials can be simply and effectively improved.

[0209] Therefore, the method for producing a steel material joined product of the present invention can be suitably adopted in the production of various structures including a steel material joined product.

Claims

1. A method for producing a steel material joint body, the method comprising: The method for manufacturing a steel material joint body comprises: a step of arranging a carbonaceous material on a joining surface of at least one of the steel materials to be joined; an overlapping step of overlapping the joining surfaces of the steel materials to be joined with each other via the carbonaceous material; as well as a heating step of heating the steel material after the joining surfaces are overlapped with each other to a maximum reaching temperature at which a liquid phase of the carbonaceous material is generated, The carbon concentration at the joint interface between the steel materials is 0.20 mass % or more and 2.10 mass % or less, The bonding interface is composed of pearlite.

2. The method for producing a steel material joined body according to claim 1, wherein: The joint interface does not have cementite at the austenite grain boundary.

3. The method for producing a steel material joined body according to claim 1 or 2, wherein: The carbon concentration of the bonding interface is greater than or equal to 0.50 mass % and less than or equal to 0.90 mass %.