Preparation method of novel silicon-carbon negative electrode material
A novel silicon-carbon anode material was prepared by heating and mixing carbon-containing composite materials with silicon anode materials. This solved the pulverization problem of silicon-based anode materials during charge and discharge, achieving high efficiency and stability, and making it suitable for lithium-ion batteries.
Patent Information
- Application Number
- CN202411164717.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
Existing silicon-based anode materials pulverize due to volume effects during charge and discharge, which affects their commercialization. Furthermore, conventional carbon-coated materials present a contradiction between cycle stability and initial charge and discharge efficiency.
A novel silicon-carbon anode composite material was prepared by heating and mixing carbon-containing composite materials with silicon anode materials in a mixer, gradually increasing the stirring speed to knead and pulverize them.
It improves the initial coulombic efficiency and cycle stability of silicon-based anode materials, and the preparation process is simple, low-cost, and easy to industrialize.
Smart Images

Figure CN119038556A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a nano-silicon negative electrode material, and in particular, to a method for preparing a novel silicon-carbon negative electrode material. Background Art
[0002] Silicon-based negative electrode materials have a theoretical specific capacity of 4200mAh / g, which is 10 times the specific capacity of current commercial graphite negative electrode materials. However, due to the huge volume effect (>300%) generated during the charging and discharging process, the material will pulverize, seriously affecting its commercialization. The commonly used solutions at present are silicon nano-, hollow or porous. Since nano-silicon, nano-hollow silicon and porous silicon all have the disadvantages of small particles, large specific surface area and poor conductivity, carbon coating is required to increase the conductivity of silicon negative electrode materials, adjust the particle size distribution, reduce the specific surface area, and improve the electrochemical performance of the material.
[0003] In the prior art, conventional carbon coatings are either single soft carbon or hard carbon coatings, but these two types of carbon have certain advantages and disadvantages as negative electrode materials for lithium-ion batteries. Comparing these two materials, soft carbon has high initial efficiency but poor cycle stability, while hard carbon has relatively low initial efficiency but good cycle stability. Therefore, it is necessary to synthesize new silicon-carbon composite materials to meet the main performance indicators of lithium-ion battery materials such as initial charge and discharge efficiency, specific capacity, and cycle performance. Therefore, a new method for preparing silicon-carbon negative electrode materials is urgently needed to solve the above-mentioned problems. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of this application is to provide a method for preparing a novel silicon-carbon negative electrode material to solve the problems raised in the above background technology.
[0005] In order to achieve the above object, the present application provides a method for preparing a novel silicon-carbon negative electrode material, comprising the following steps:
[0006] Step (A) adding the carbon-containing composite material into a mixer and introducing an inert gas, stirring and heating to fully mix the mixture to obtain a molten mixture;
[0007] Step (B) adds silicon negative electrode material to the molten mixture obtained in step (A), then gradually increases the stirring speed and continues to heat to mix the silicon negative electrode material and the molten mixture together to obtain a mixed mixture, and the mixed mixture is degummed and pulverized to obtain a silicon-carbon negative electrode composite material.
[0008] Preferably, the heating temperature in step (A) is 60-200° C. and the stirring speed is 50-300 rpm.
[0009] Preferably, the carbon-containing composite material in step (A) is a mixture of petroleum asphalt or coal asphalt and one or more of needle coke, carbon fiber, carbon microspheres, porous carbon, carbon nanotubes and graphite hard carbon materials.
[0010] Preferably, in step (B), the stirring speed is 50-2000 rpm and the heating temperature is 250-600°C.
[0011] Preferably, the silicon negative electrode material in step (B) is one or more of nano-silicon, nano-hollow silicon, and porous silicon with uniform particle size and regular morphology.
[0012] Preferably, the ratio of the amount of silicon negative electrode material added in step (B) to the total weight of the carbon-containing composite material is (0.1-3):1.
[0013] Preferably, the inert gas in step (A) is nitrogen or argon.
[0014] According to the preparation method of a novel silicon-carbon negative electrode material of the present application, both the high first coulombic efficiency of the silicon-based negative electrode material and its cycle stability are guaranteed, and the preparation process has the advantages of simple operation, low cost and easy industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments with reference to the following drawings:
[0016] Figure 1 The present invention is a flow chart of a method for preparing a novel silicon-carbon negative electrode material according to an embodiment of the present application. DETAILED DESCRIPTION
[0017] In order to make the technical means, creative features, objectives and effects achieved by this application easy to understand, this application is further explained below in conjunction with specific implementation methods.
[0018] like Figure 1 As shown, the present application provides a technical solution: a method for preparing a novel silicon-carbon negative electrode material, comprising the following steps:
[0019] Step (A) adding the carbon-containing composite material into a mixer and introducing an inert gas, stirring and heating to fully mix the mixture to obtain a molten mixture;
[0020] Step (B) adds silicon negative electrode material to the molten mixture obtained in step (A), then gradually increases the stirring speed and continues heating to mix the silicon negative electrode material with the molten mixture to obtain a mixed mixture, and the mixed mixture is degummed and pulverized to obtain a silicon-carbon negative electrode composite material. This design gradually increases the stirring speed during the heating process to ensure both the dispersibility of the silicon negative electrode material and its encapsulation by the molten mixture.
[0021] Preferably, the heating temperature in step (A) is 60-200° C. and the stirring speed is 50-300 rpm.
[0022] Preferably, the carbon-containing composite material in step (A) is a carbon-containing composite material in which petroleum asphalt or coal tar is mixed with one or more of needle coke, carbon fiber, carbon microspheres, porous carbon, carbon nanotubes and graphite hard carbon materials in a certain proportion, wherein petroleum asphalt and coal tar are soft carbon materials.
[0023] Preferably, in step (B), the stirring speed is 50-2000 rpm and the heating temperature is 250-600° C. This design ensures sufficient mixing of the carbon-containing composite material by heating.
[0024] Preferably, the silicon negative electrode material in step (B) is one or more of nano-silicon, nano-hollow silicon, and porous silicon with uniform particle size and regular morphology.
[0025] Preferably, the ratio of the amount of silicon negative electrode material added in step (B) to the total weight of the carbon-containing composite material is (0.1-3):1.
[0026] Preferably, the inert gas in step (A) is nitrogen or argon.
[0027] The following is an introduction to a specific embodiment of a method for preparing a novel silicon-carbon negative electrode material according to the present invention.
[0028] Example 1: Step (A1) A carbon-containing composite material in which coal tar powder and carbon fiber powder are mixed in a weight ratio of 1:1 is added into a mixer and nitrogen is introduced. Under the protection of nitrogen, the mixture is stirred at a stirring speed of 50 rpm and heated to 150° C. to uniformly mix the coal tar powder and the carbon fiber powder to obtain a molten mixture;
[0029] Step (B1) Add nano hollow silicon to the molten mixture obtained in step (A1) in a weight ratio of 1:1, then stir at a stirring speed of 50 rpm for 30 minutes, then 200 rpm for 30 minutes, then 500 rpm for 30 minutes, and finally increase the speed to 1000 rpm and continue to heat to 400° C. to blend the nano hollow silicon and the molten mixture together to obtain a blended mixture, degumming and pulverizing the blended mixture, and continue stirring for 2 hours to obtain a new silicon-carbon negative electrode composite material.
[0030] Example 2: Step (A2) A carbon-containing composite material in which petroleum asphalt powder and carbon nanotubes are mixed in a weight ratio of 5:4 is added into a mixer and argon is introduced. Under the protection of argon, the mixture is stirred at a stirring speed of 100 rpm and heated to 190° C. to uniformly mix the carbon-containing composite material to obtain a molten mixture;
[0031] Step (B2) Add nano silicon to the molten mixture obtained in step (A2) in a weight ratio of 1:1, then stir at a stirring speed of 50 rpm for 30 minutes, then 200 rpm for 30 minutes, then 500 rpm for 30 minutes, and finally increase the speed to 1000 rpm and continue to heat to 360°C to blend the nano silicon and the molten mixture together to obtain a blended mixture, degumming and pulverizing the blended mixture, and continue stirring for 2 hours to obtain a new silicon-carbon negative electrode composite material.
[0032] Example 3: Step (A3) A carbon-containing composite material in which petroleum asphalt powder and needle coke are mixed in a weight ratio of 5:3 is added into a mixer and argon is introduced. Under the protection of argon, the mixture is stirred at a stirring speed of 50 rpm and heated to 150° C. to uniformly mix the petroleum asphalt powder and needle coke to obtain a molten mixture;
[0033] Step (B3) Porous silicon is added to the molten mixture obtained in step (A3) in a weight ratio of 1:1.2, and then the stirring speed is increased from 50 rpm to 30 minutes, then 200 rpm to 30 minutes, and then 500 rpm to 30 minutes. Finally, the speed is increased to 1000 rpm and continued to heat to 410°C to mix the porous silicon and the needle coke molten mixture together to obtain a mixed mixture. The mixed mixture is degummed and pulverized, and continued to be stirred for 2 hours to obtain a new silicon-carbon negative electrode composite material.
[0034] Comparative Example 1: Step (A11) adding a certain amount of coal tar pitch soft carbon material into a mixer, stirring at a stirring speed of 50 rpm and heating the material to 150° C. to melt the material to obtain a melt;
[0035] Step (B11) Add nano hollow silicon to the melt obtained in step (A11) in a weight ratio of 1:1, then stir at a stirring speed of 50 rpm for 30 minutes, then 200 rpm for 30 minutes, then 500 rpm for 30 minutes, and finally increase the speed to 1000 rpm and continue to heat to 400°C to mix the nano hollow silicon and the melt together to obtain a mixed mixture, degumming and pulverizing the mixed mixture, and continue stirring for 2 hours to obtain a soft carbon-coated silicon-carbon negative electrode composite material.
[0036] Comparative Example 2: Step (A12) A certain amount of porous carbon hard carbon material is added into a mixer, stirred at a stirring speed of 50 rpm and heated to 190° C. to melt the material to obtain a melt;
[0037] Step (B12) Add nano-silicon to the melt obtained in step (A12) in a weight ratio of 1:1, then increase the stirring speed from 50 rpm to 30 minutes, then to 200 rpm to 30 minutes, then to 500 rpm to 30 minutes, and finally increase the speed to 1000 rpm and continue to heat to 360°C to mix the nano-silicon and the melt together to obtain a mixed mixture, and the mixed mixture is degummed and pulverized, and continued to be stirred for 2 hours to obtain a hard carbon-coated silicon-carbon negative electrode composite material.
[0038] According to the novel silicon-carbon negative electrode composite material prepared by coating the silicon negative electrode material with the carbon-containing composite material in Examples 1-3, the soft carbon-coated silicon-carbon negative electrode composite material prepared in Comparative Example 1, and the hard carbon-coated silicon-carbon negative electrode composite material prepared in Comparative Example 2, negative electrode sheets were prepared respectively, and then assembled into lithium-ion batteries, and the performance of each group of batteries was tested, wherein the preparation method of the negative electrode sheet and the lithium-ion battery comprises the following steps:
[0039] 94-97% of negative electrode material, 0.1-1% of conductive agent (single-walled carbon nanotubes) and 3-5% of binder (PAALi) are evenly mixed in a mass ratio, a certain amount of high-purity water is added to prepare negative electrode slurry, coated on copper foil, dried at 110°C in a vacuum drying oven for 10 h, and the negative electrode sheet is obtained by rolling and punching. A lithium sheet is used as the counter electrode, 1.0 mol / L LiPF6 / EC:DEC=1:1Vol%+5%FEC is used as the electrolyte, and button batteries are assembled in a glove box under an argon atmosphere.
[0040] The prepared battery was subjected to electrochemical testing, and the results are shown in Table 1:
[0041]
[0042]
[0043] Table 1
[0044] According to Table 1, the present application adopts a method for preparing a new silicon-carbon negative electrode material, such as Examples 1-3, to prepare a negative electrode plate from a new silicon-carbon negative electrode composite material prepared by a carbon-containing composite material, and the specific capacity, first coulomb efficiency, and cycle capacity retention rate of the assembled lithium-ion battery are compared with those of the negative electrode plates made of silicon-carbon negative electrode composite materials prepared by using soft carbon materials in Comparative Example 1 and hard carbon materials in Comparative Example 2, respectively. The performance of the assembled lithium-ion battery is as follows: the first coulomb efficiency is increased by 3.7%-10.1%, and the cycle capacity retention rate (cycle stability) is increased by 4.6%-12.1%. Therefore, the method for preparing a new silicon-carbon negative electrode composite material by coating a silicon negative electrode material with a carbon-containing composite material in the present application has the following advantages, which ensures both a high first coulomb efficiency and a cycle stability of the silicon-based negative electrode material, and the preparation method of the present application has a simple preparation process, low cost, and is easy to industrialize.
[0045] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a novel silicon-carbon negative electrode material, characterized in that: The following steps are involved: Step (A) adding the carbon-containing composite material into a mixer and introducing an inert gas, stirring and heating to fully mix the mixture to obtain a molten mixture; Step (B) adds silicon negative electrode material to the molten mixture obtained in step (A), then gradually increases the stirring speed and continues to heat to mix the silicon negative electrode material and the molten mixture together to obtain a mixed mixture, and the mixed mixture is degummed and pulverized to obtain a silicon-carbon negative electrode composite material.
2. The method for preparing a novel silicon-carbon negative electrode material according to claim 1, characterized in that: In the step (A), the heating temperature is 60-200° C. and the stirring speed is 50-300 rpm.
3. The method for preparing a novel silicon-carbon negative electrode material according to claim 1, characterized in that: The carbon-containing composite material in step (A) is a mixture of petroleum asphalt or coal asphalt and one or more of needle coke, carbon fiber, carbon microspheres, porous carbon, carbon nanotubes and graphite hard carbon materials.
4. The method for preparing a novel silicon-carbon negative electrode material according to claim 1, characterized in that: In the step (B), the stirring speed is 50-2000 rpm and the heating temperature is 250-600°C.
5. The method for preparing a novel silicon-carbon negative electrode material according to claim 1, characterized in that: The silicon negative electrode material in step (B) is one or more of nano-silicon, nano-hollow silicon, and porous silicon with uniform particle size and regular morphology.
6. The method for preparing a novel silicon-carbon negative electrode material according to claim 1, characterized in that: The ratio of the amount of silicon negative electrode material added in step (B) to the total weight of the carbon-containing composite material is (0.1-3):
1.
7. The method for preparing a novel silicon-carbon negative electrode material according to claim 1, characterized in that: The inert gas in step (A) is nitrogen or argon.
Citation Information
Patent Citations
Natural graphite-based silicon-carbon composite negative electrode material as well as preparation method and application thereof
CN111333063A
Silicon-based composite negative electrode material and preparation method thereof, and negative electrode of lithium ion battery
US20210399290A1