Preparation method of Fe3O4 / HAP / Ag nano composite material and application of Fe3O4 / HAP / Ag nano composite material in detection of antibiotic residues in aquatic organisms

Through Fe3O4/HAP/Ag nanocomposites as SERS detection substrate, the electromagnetic field and charge transfer mechanisms are used to solve the sensitivity and repetition of antibiotic residue detection in the prior art, and the rapid and accurate antibiotic CIP residues in aquatic organisms are achieved. Test.

CN119038616APending Publication Date: 2024-11-29SHAANXI SCI TECH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411443879.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art methods for detecting antibiotic residues in aquatic organisms, especially ciprofloxacin (CIP), have sensitivity and repetition problems, especially the false positive rate of ultraviolet spectrophotometry and poor repetition of photoelectrochemical adapter method. It is urgently needed. A high sensitivity detection method.

Method used

Fe3O4/HAP/Ag nanocomposites are used as the SERS detection substrate, and the Raman signal is enhanced by preparing magnetic hydroxyapatite (Fe3O4/HAP) and nanosilver (Ag) composites, and the electromagnetic field enhancement and charge transfer mechanisms are used to enhance the Raman signal to achieve rapid detection. Antibiotic residue.

Benefits of technology

It realizes rapid and sensitive detection of antibiotic CIP residues in aquatic organisms, improves the repeatability and stability of the detection, reduces the false positive rate, has good biocompatibility and high surface energy, and can significantly enhance Raman signal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038616A_ABST
    Figure CN119038616A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of antibiotic detection, in particular to a preparation method of a Fe3O4 / HAP / Ag nano composite material and application of the Fe3O4 / HAP / Ag nano composite material to detection of antibiotic residues in aquatic organisms. The invention provides a method for preparing Fe3O4 / HAP / Ag, which comprises the following steps: firstly preparing magnetic hydroxyapatite Fe3O4 / HAP, and then compounding a nano-silver seed solution with the Fe3O4 / HAP to prepare the Fe3O4 / HAP / Ag. As the Fe3O4 / HAP / Ag is used as the Raman substrate, Raman signals can be enhanced and can be explained through electromagnetic field enhancement and charge transfer principles, and therefore, the Fe3O4 / HAP / Ag material is used as the substrate for SERS (Surface Enhanced Raman Scattering) detection, and the aim of rapidly detecting antibiotic CIP residues in aquatic organisms can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of antibiotic detection, and in particular to a method for preparing a Fe3O4 / HAP / Ag nanocomposite material and an application thereof in detecting antibiotic residues in aquatic organisms. Background Art

[0002] With the rapid development of economy, environmental problems have gradually accumulated and emerged. Antibiotics are considered as an emerging pollutant that may have a significant adverse impact on the environment. In recent years, the problem of antibiotic residues in food and natural environment has attracted increasing attention, especially in aquatic ecosystems. The abuse of antibiotics in aquaculture endangers human health and safety. Therefore, the detection of antibiotic residues in aquatic ecosystems, including aquatic products and water bodies, is crucial. Ciprofloxacin (CIP), as a third-generation synthetic fluoroquinolone antibacterial drug, has become one of the most important anti-infective drugs in aquaculture.

[0003] Currently, the standard methods for CIP residue detection include high performance liquid chromatography (HPLC), ultraviolet spectrophotometry (UV-SP) and enzyme immunoassay (ELISA), as well as emerging optical and electrochemical biosensing methods, however, each method has certain limitations. For example, although ultraviolet spectrophotometry is fast and accurate, it has a high false positive rate; the photoelectrochemical adapter method has the characteristics of high sensitivity and poor repeatability; therefore, there is an urgent need to develop a highly sensitive ciprofloxacin detection method.

[0004] SERS is an advanced non-destructive analytical technique that can significantly enhance the Raman signal of molecules, amplifying it by several orders of magnitude. The adaptability of this technology is widely used in various fields, including medical diagnosis, industrial investigation, environmental monitoring and food safety review. SERS has high sensitivity, which is achieved by substrate enhancement of Raman scattering signals. The SERS phenomenon is fundamentally rooted in the enhancement mechanism, including electromagnetic field enhancement and charge transfer mechanism, which are two common and widely recognized theories to explain the effect. The enhancement of SERS through electromagnetic mechanism (EM) is mainly due to the localized surface plasmon resonance (LSPR) effect occurring inside the metal nanostructure, which significantly amplifies the electromagnetic field on the surface of the material. On the other hand, the enhancement of chemical mechanism (CM) originates from the charge transfer (CT) interaction between the adsorbed molecules and the substrate, which plays a vital role in the SERS effect. The SERS substrate is crucial to determine the enhancement mechanism. The rapid development of nanotechnology has made various noble metal nanoparticles the focus of SERS substrate exploration, mainly because they can produce high-density hotspots. In particular, silver nanoparticles (AgNPs) have excellent SERS signal effects. However, the reliance on a single type of substrate brings some challenges, including reduced stability, oxidation tendency and limited reproducibility. The emergence of composite materials has had a huge impact, and the emergence of composite materials has solved this problem well. The magnetic semiconductor Fe3O4 component is often used as a SERS active noble metal support for diagnostic and therapeutic agents due to its potential chemical enhancement and high photothermal conversion effect.

[0005] The electromagnetic enhancement mechanism mainly relies on the localized surface plasmon resonance (LSPR) to amplify the Raman scattering of the target molecule. This resonance is mainly induced by depositing some noble metals (Au, Ag, Cu, etc.) or transition metals (Cu, Ni, Ti, Co, etc.) on the surface of various nanostructures. The electromagnetic field generated by the surface plasmon resonance (SPR) of the metal nanostructure forms a "hot spot" on the nanoscale ("Ag loaded TiO2 nanotube photonic crystals self-doped Ti 3+periodically by anodization process and their performance of surface enhanced Raman scattering”, Zhou et al, Optical Materials, 99, 109567, January 2020), and “hot spots” are where the LSPR field is concentrated at sharp points and gaps in the nanostructure, where the SERS signal is significantly amplified (“Manipulating the surface-enhanced Raman spectroscopy (SERS) activity and plasmon-driven catalytic efficiency by the control of Ag NP / graphene layers under optical excitation”, Xianwu Xiu et al, Nanophotonics, 10 (5), 1529-1540, February 2021).

[0006] CM enhancement is based on the chemical interaction between the analyte and the substrate, such as charge transfer (CT) between various analyte and substrate states (“Switching from electromagnetic to chemical mechanism in quantum plasmonic tip-induced graphene oxide enhanced Raman scattering”, Hana N. Hrimet al, Physical Review, 106(3), 035410, July 2022). Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a method for preparing a Fe3O4 / HAP / Ag nanocomposite material and its application in detecting antibiotic residues in aquatic organisms in view of the deficiencies of the above-mentioned prior art.

[0008] The present invention provides a method for preparing a Fe3O4 / HAP / Ag nanocomposite material, comprising the following steps:

[0009] S1. Preparation of Fe3O4 nanoparticles: Adding double distilled water into a three-necked flask, placing it in a water bath and mechanically stirring it, introducing nitrogen for deoxygenation, adding FeSO4 and FeCl3·6H2O, stirring until the solid is completely dissolved, heating the water bath to 60°C, then adding sodium hydroxide solution dropwise thereto to adjust the pH value and react fully, stopping stirring, raising the water bath temperature to 80°C, and fully aging, then stopping adding nitrogen, washing the solution after cooling it to room temperature, and obtaining Fe3O4 fluid when the pH value of the solution after washing is 7.0, drying it, and grinding and preserving it after cooling it to room temperature to obtain Fe3O4 nanoparticles;

[0010] S2. Preparation of magnetic hydroxyapatite (Fe3O4 / HAP) nanoparticles:

[0011] S201, preparing a hydroxyapatite precursor solution: adding sodium citrate to a calcium nitrate solution, stirring thoroughly, adding a disodium hydrogen phosphate solution dropwise, and then adding a sodium hydroxide solution to adjust the pH value to obtain a mixed solution, and after the reaction is completed, placing the solution under sealing conditions and continuing to stir the reaction to obtain a hydroxyapatite precursor solution;

[0012] S202, preparing dispersed Fe3O4 nanoparticles: taking the Fe3O4 nanoparticles prepared in S1 and dispersing them by ultrasonic to obtain dispersed Fe3O4 nanoparticles;

[0013] S203, preparing Fe3O4 / HAP nanoparticles: putting the dispersed Fe3O4 nanoparticles prepared in S202 into the hydroxyapatite precursor solution prepared in S201 and fully stirring, and continuously reacting at high temperature, after the reaction is completed, washing by centrifugation and drying, and grinding to obtain Fe3O4 / HAP nanoparticles;

[0014] S3, preparing nano silver seed solution: taking silver nitrate solution and sodium citrate solution 1 and mixing them, adding hydrogen peroxide thereto, stirring and mixing them well to obtain a mixed solution, injecting sodium borohydride into the mixed solution with a syringe, and letting it stand at room temperature after sufficient reaction to obtain nano silver seed crystals, taking the nano silver seed crystals and dissolving them in deionized water, adding a mixed solution of sodium citrate solution 2 and ascorbic acid, and then adding silver nitrate solution to continue the reaction to obtain nano silver seed solution;

[0015] S4, preparation of Fe3O4 / HAP / Ag nanocomposite material: the Fe3O4 / HAP nanoparticles prepared in S2 are dissolved in water to obtain a Fe3O4 / HAP solution, and after ultrasonic dispersion, a sodium hydroxide solution is added to adjust the pH value of the Fe3O4 / HAP solution, and then the solution is heated in a water bath while being stirred, and the nanosilver seed solution prepared in S3 is added to the Fe3O4 / HAP solution, and after sufficient reaction and aging, a precipitate is obtained, which is washed and dried, and then ground to obtain a Fe3O4 / HAP / Ag nanocomposite material.

[0016] According to the preparation method of the Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the mass volume ratio of the double distilled water, FeSO4 and FeCl3·6H2O in S1 is 75.0 mL:1.39 g:2.7 g, and the concentration of the sodium hydroxide solution is 3 mol / L.

[0017] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the deoxygenation time in S1 is 30 minutes, the pH value is adjusted to 9.0-10.0, the sufficient reaction time is 30 minutes, the aging time is 60 minutes, the washing detergent is anhydrous ethanol and deionized water, the temperature of the oven is 60°C, and the drying condition is drying in an oven at a temperature of 60°C for 12 hours.

[0018] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the mass volume ratio of the calcium nitrate solution, sodium citrate and disodium hydrogen phosphate solution in S201 is 100mL:2.351g:100mL, the concentration of the calcium nitrate solution is 0.30mol / L, the concentration of the disodium hydrogen phosphate solution is 0.18mol / L, the time for sufficient stirring in S201 is 10min, the pH value is 10.0, and the stirring reaction time is 1 to 2h.

[0019] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the mass of Fe3O4 in S202 is 2.312 g, the temperature of the ultrasonic cleaner is 45° C., and the dispersion time of the ultrasonic cleaner is 20 min.

[0020] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the mass volume ratio of Fe3O4 nanoparticles and hydroxyapatite precursor solution in S203 is 1:40, the temperature of the high temperature continuous reaction is 180°C, the time of the high temperature continuous reaction is 24h, and the drying condition is drying in an oven at 80°C for 12h.

[0021] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the volume ratio of the silver nitrate solution, sodium citrate solution 1, hydrogen peroxide and sodium borohydride in S3 is 0.60mL:23.5mL:0.1mL:0.60mL, the concentration of the silver nitrate solution is 0.01mol / L, the concentration of the sodium citrate solution 1 is 2.5×10 -4 mol / L, the concentration of the hydrogen peroxide is 1.875 mol / L, the concentration of the sodium borohydride is 0.01 mol / L, the time for sufficient reaction is 15 min, and the standing time is 2 h.

[0022] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the volume ratio of the nanosilver seed, deionized water, sodium citrate solution 2, ascorbic acid and silver nitrate solution in S3 is 2mL:16mL:1.0mL:2.0mL:1.0mL, the concentration of the sodium citrate solution 2 is 0.075mol / L, the concentration of the ascorbic acid is 0.1mol / L, and the continued reaction time is 30min.

[0023] According to the preparation method of Fe3O4 / HAP / Ag nanocomposite material provided by the present invention, the mass of Fe3O4 / HAP nanoparticles in S4 is 0.10g, the volume of Fe3O4 / HAP solution is 50mL, the ultrasonic dispersion time is 60min, the concentration of sodium hydroxide solution is 1.0mol / L, the pH value is 10.0, the temperature of the water bath is 70°C, the sufficient reaction time is 1h, the aging time is 24h, the detergent for washing is deionized water, the drying condition is drying in an oven at a temperature of 80°C for 12h, and the method of adding the nanosilver seed solution prepared in S3 to the Fe3O4 / HAP solution in S4 is: adding the nanosilver seed solution prepared in S3 into it in 8 times, each time with an interval of 20min, and adding 20mL of nanosilver seed solution each time.

[0024] The present invention also provides an application of the Fe3O4 / HAP / Ag composite nanomaterial, characterized in that the prepared Fe3O4 / HAP / Ag composite nanomaterial is used as a substrate for SERS detection to detect antibiotic residues in aquatic organisms.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] The present invention provides a method for preparing Fe3O4 / HAP / Ag, wherein magnetic hydroxyapatite Fe3O4 / HAP is first prepared, and then nano silver seed solution is compounded with Fe3O4 / HAP to prepare Fe3O4 / HAP / Ag. Because Fe3O4 / HAP / Ag is used as a Raman substrate, Raman signals can be enhanced, which can be explained by electromagnetic field enhancement and charge transfer principles. Therefore, using Fe3O4 / HAP / Ag material as a substrate for SERS detection can achieve the purpose of rapidly detecting antibiotic CIP residues in aquatic organisms. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is the preparation flow chart of Fe3O4 / HAP / Ag nanocomposite;

[0028] Figure 2 are the XRD patterns of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag;

[0029] Figure 3 It is the infrared characterization diagram of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag;

[0030] Figure 4 This is the UV spectrum of nanosilver;

[0031] Figure 5 are the SEM images of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag and the TEM image of Fe3O4 / HAP / Ag;

[0032] Figure 6 This is the Raman spectrum of R6G;

[0033] Figure 7 Raman spectra of CIP at different concentrations;

[0034] Figure 8 The CIP concentrations at 1382 cm -1 The intensity standard curve at ;

[0035] Fig. 9 This is the stability test result diagram;

[0036] Fig.10 This is a graph showing the results of a reproducibility experiment. DETAILED DESCRIPTION

[0037] Example 1

[0038] This embodiment provides a method for preparing a Fe3O4 / HAP / Ag nanocomposite material, and the specific steps are as follows:

[0039] S1. Preparation of Fe3O4 nanoparticles: 75.0 mL of double distilled water was added to a three-necked flask, and the flask was placed in a water bath for mechanical stirring. Nitrogen was introduced for deoxygenation for 30 min, and 1.39 g of ferrous sulfate (FeSO4) and 2.7 g of ferric chloride (FeCl3·6H2O) were added. The solid was stirred until it was completely dissolved. At this time, the solution was orange-yellow. After the water bath temperature was raised to 60°C, a 3 mol / L sodium hydroxide solution was added dropwise. The color of the solution gradually changed from orange-yellow to black. The solution was adjusted. After the pH value of the solution is between 9.0 and 10.0, the reaction is carried out for 30 minutes, and the stirring is stopped. Then the water bath temperature is raised to 80°C and aged for 60 minutes. The entire reaction process must be completed under nitrogen protection. After the reaction is completed, the solution is cooled to room temperature and washed with anhydrous ethanol and deionized water. When the pH value of the solution after washing is 7.0, Fe3O4 fluid is obtained. The Fe3O4 fluid is placed in an oven at a temperature of 60°C for 12 hours and then taken out. After cooling to room temperature, it is crushed and ground to obtain Fe3O4 nanoparticles.

[0040] S2. Preparation of magnetic hydroxyapatite (Fe3O4 / HAP) nanoparticles:

[0041] S201, prepare a hydroxyapatite precursor solution: take 100 mL of a 0.30 mol / L calcium nitrate solution in a beaker and add 2.351 g of sodium citrate solid, stir thoroughly for 10 min, then slowly add dropwise 100 mL of a 0.18 mol / L disodium hydrogen phosphate solution, then add a 3 mol / L sodium hydroxide solution to adjust the pH value to 10.0 to obtain a mixed solution, which is milky white at this time. After the reaction system is stable, place it under sealing conditions and continue to stir the reaction for 1 to 2 hours to obtain a hydroxyapatite precursor solution;

[0042] S202, preparing dispersed Fe3O4 nanoparticles: taking 2.312 g of the Fe3O4 nanoparticles prepared in S1 and placing them in an ultrasonic cleaner at a temperature of 45° C., dispersing them for 20 minutes, and obtaining dispersed Fe3O4 nanoparticles;

[0043] S203, preparation of Fe3O4 / HAP nanoparticles: according to the mass volume ratio of Fe3O4 nanoparticles to hydroxyapatite precursor solution of 1:40, the dispersed Fe3O4 nanoparticles prepared in S202 are put into the hydroxyapatite precursor solution prepared in S201 and fully stirred to obtain a mixed solution, the mixed solution is transferred into a polytetrafluoroethylene liner with a capacity of 50 mL and then transferred into an autoclave, the temperature of the autoclave is adjusted to 180°C and the reaction is continued for 24 hours, after the reaction is completed, the obtained product is centrifuged and washed, and after the product is neutral after washing, it is dried in an oven at a temperature of 80°C for 12 hours, taken out and ground for use, to obtain Fe3O4 / HAP nanoparticles;

[0044] S3, preparation of nanosilver seed solution: 0.60mL of 0.01mol / L silver nitrate and 23.5mL of 2.5×10 -4 mol / L sodium citrate was mixed evenly, 0.1mL of 1.875mol / L hydrogen peroxide was added dropwise thereto, the mixture was stirred and mixed evenly to obtain a mixed solution, 0.60mL of 0.01mol / L sodium borohydride (NaBH4) was injected into the mixed solution with a syringe, the color of the mixed solution changed to yellow, and the reaction was continued for 15min, and then the mixture was allowed to stand at room temperature for 2h to obtain nanosilver seeds, 2mL of the nanosilver seeds were moved into a beaker, 16mL of deionized water was added, and then 1.0mL of 0.075mol / L sodium citrate and 2.0mL of 0.1mol / L ascorbic acid were mixed and added to the beaker, and 1.0mL of 0.01mol / L silver nitrate solution was injected, and the reaction was continued for 30min to obtain a nanosilver seed solution, which was red;

[0045] S4, preparation of Fe3O4 / HAP / Ag nanocomposite material: 0.10 g of Fe3O4 / HAP nanoparticles prepared in S2 was dissolved in water to obtain a Fe3O4 / HAP solution with a volume of 50 mL. After dispersion in an ultrasonic cleaner for 60 min, a sodium hydroxide solution with a concentration of 1.0 mol / L was added to adjust the pH value of the Fe3O4 / HAP solution to 10.0. The solution was then placed in a constant temperature water bath at a temperature of 70°C and stirred. The nanosilver seed solution prepared in S3 was added thereto in 8 times, each time with an interval of 20 min, and 20 mL of the nanosilver seed solution was added each time. After all the additions were made, the solution was fully reacted for 1 h, and then aged for 24 h to obtain a supernatant liquid and a precipitate of the product. The supernatant liquid was removed, and the precipitate was washed with deionized water for several times, dried in an oven at 80°C for 12 h, ground and preserved to obtain a Fe3O4 / HAP / Ag nanocomposite material.

[0046] The preparation process of the Fe3O4 / HAP / Ag nanocomposite material provided in this embodiment is as follows: Figure 1 shown.

[0047] Comparative Example 1

[0048] This comparative example provides a method for preparing a nano silver seed solution, and the specific steps are as follows:

[0049] Take 0.60mL of 0.01mol / L silver nitrate and 23.5mL of 2.5×10 -40.1 mL of 1.875 mol / L sodium citrate was added dropwise thereto, the mixture was stirred and mixed to obtain a mixed solution, 0.60 mL of 0.01 mol / L sodium borohydride (NaBH4) was injected into the mixed solution with a syringe, the color of the mixed solution changed to yellow, and the reaction was continued for 15 min, and the mixture was allowed to stand at room temperature for 2 h to obtain nanosilver seeds, 4 mL of the nanosilver seeds were moved into a beaker, 16 mL of deionized water was added, and then 1.0 mL of 0.075 mol / L sodium citrate and 2.0 mL of 0.1 mol / L ascorbic acid were mixed and added to the beaker, and 1.0 mL of 0.01 mol / L silver nitrate solution was injected, and the reaction was continued for 30 min to obtain a nanosilver seed solution, which was blue.

[0050] Example 2

[0051] In this example, the Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag samples prepared in Example 1 were characterized.

[0052] ① XRD characterization of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag

[0053] Figure 2 XRD patterns of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag samples.

[0054] It can be seen from the XRD spectrum that the Fe3O4 curve corresponds to (220), (311), (400), (511) and (440) crystal planes at 2θ of 30.1°, 34.2°, 43.8°, 57.2° and 63.3°, respectively, which is consistent with the spinel structure of Fe3O4 (JCPDS No.85-1436) ("Novel phenylalanine-modified magnetic ferroferric oxide nanoparticles for ciprofloxacin removal from aqueous solution", Fu X et al, Journal of Colloid and Interface Science, 632, 345-356, 2023), proving that the product prepared in S1 of Example 1 is pure phase Fe3O4.

[0055] The Fe3O4 / HAP curve has crystal diffraction peaks at 2θ of 25.9°, 31.7°, 32.8° and 33.9°, which correspond to the characteristic peaks of the standard chart of hydroxyapatite (JCPDS 09-0432) on the (002), (211), (112) and (300) crystal planes, respectively. The characteristic peaks of both Fe3O4 and HAP appear in the XRD spectrum of Fe3O4 / HAP, indicating that the structure of Fe3O4 is not destroyed during the preparation of Fe3O4 / HAP in Example 1, and the purpose of using HAP to modify and protect Fe3O4 is successfully achieved. It also proves that HAP is successfully loaded on Fe3O4.

[0056] In addition to the diffraction peak of Fe3O4, the Fe3O4 / HAP / Ag curve also has obvious diffraction peaks at 2θ of 38.1°, 44.2°, 64.3° and 77.5°. These diffraction peaks are attributed to face-centered cubic silver nanoparticles, reflecting from the (111), (200), (220) and (311) crystal planes, indicating that Fe3O4 / HAP / Ag has successfully loaded silver nanoparticles.

[0057] ② FT-IR spectrum characterization of Fe3O4 / HAP / Ag

[0058] The FT-IR spectrum results of Fe3O4 / HAP / Ag are as follows Figure 3 shown. Figure 3 (c) is located at 537.5cm -1 The absorption peak at is the characteristic absorption peak of Fe-O bond on the surface of Fe3O4; Figure 3 (b) is located at 3452cm -1 The absorption peak at 595.8 cm is related to the stretching vibration of OH in HAP. -1 、1345.8cm -1 The absorption peak at 1020.8cm is caused by the bending vibration of OPO in HAP. -1 The absorption peak at is caused by the OP stretching vibration in HAP (“Fe3O4@HAP-enhanced photocatalytic degradation of AcidRed73 in aqueous suspension: Optimization, kinetic, and mechanism studies”, Golshan M et al, Materials Research Bulletin, 91, 59-67, 2017).

[0059] FT-IR data clearly show that Fe3O4 nanoparticles were successfully embedded on the HAP surface by precipitation method. Figure 3(a) has no obvious other absorption peaks compared to (b).

[0060] ③ Characterization of the UV spectrum of nanosilver seed solution

[0061] The nanosilver seed prepared in Example 1 is AgNPs-1, the nanosilver seed solution prepared in Example 1 is AgNPs-2, and the nanosilver seed solution prepared in Comparative Example 1 is AgNPs-3. The UV-visible spectra are as follows: Figure 4 shown.

[0062] The color of AgNPs-1 is bright yellow, and its main UV absorption is Figure 4 The center is 420 nm, indicating that AgNPs-1 are spherical nanoparticles and exhibit typical plasmon resonance.

[0063] By comparing AgNPs-2 and AgNPs-3, as the amount of silver nanoparticles solution increased from 2 mL to 4 mL, the peak underwent a significant red shift, indicating that the shape of the silver nanospheres changed. The spectrum above 500 nm indicated the presence of triangles, and the higher the wavelength of the peak, the more representative the triangular prisms in the colloid.

[0064] ④SEM and TEM characterization of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag

[0065] The SEM morphologies of Fe3O4, Fe3O4 / HAP and Fe3O4 / HAP / Ag are shown in Figure 2. Figure 5 As shown in a, b and c, the TEM of Fe3O4 / HAP / Ag is Figure 5 As shown in middle d.

[0066] like Figure 5 As shown in (a), Fe3O4 particles are composed of irregular spherical particles; after hydroxyapatite coating, the microstructure changes, such as Figure 5 As shown in (b), the surface of the prepared Fe3O4 / HAP is not smooth and is covered with a rod-shaped deposition layer; after loading silver nanoparticles, the particle size of the sample increases and the surface becomes rough. Most of the silver nanoparticles are distributed on the surface of the HAP nanoparticles to form Fe3O4 / HAP / Ag.

[0067] Figure 5 (d) is the transmission electron microscope image of Fe3O4 / HAP / Ag. From the image, the most obvious parts are the silver nanoparticles, which are dark black and round due to their high atomic number, and the HAP particles are rod-shaped.

[0068] Example 3

[0069] This embodiment provides an application of the Fe3O4 / HAP / Ag nanocomposite material prepared in Example 1 for detecting rhodamine 6G (R6G).

[0070] R6G was used as a representative probe to evaluate the SERS performance of the substrate. R6G powder was diluted to 1×10 -4 mol / L of the test solution.

[0071] 1 mg of the Fe3O4 / HAP / Ag powder prepared in Example 1 was prepared into a solution and smeared on a glass plate and dried as a substrate. The above test solution was drop-coated on the substrate for SERS measurement.

[0072] The SERS measurement used a 785 nm laser as the excitation source, with a collection time of 10 s, a laser power of 10 mW, and a spectrum collection range of 600 to 1800 cm -1 .

[0073] The surface enhanced Raman spectroscopy activity of Fe3O4 / HAP / Ag was experimentally studied using R6G dye as the detection molecule.

[0074] Figure 6 The concentration is shown as 10 -4 mol / L of bare R6G and R6G / Fe3O4 / HAP / Ag.

[0075] R6G dye at 1184cm -1 Mode assigned to CC stretching vibration, 1366 cm -1 The modes correspond to heterocyclic stretching and CH plane bending. It can be seen that Fe3O4 / HAP / Ag has a significant enhancement effect on the Raman intensity of R6G compared with that of bare R6G. Therefore, the prepared Fe3O4 / HAP / Ag composite material can be used as a SERS substrate for rapid detection

[0076] In order to evaluate the enhancement performance of the substrate, R6G was selected as the probe molecule and the concentration was 1×10 -4 mol / L solution R6G, and the SERS spectrum was obtained using Fe3O4 / HAP / Ag as the SERS substrate. The SERS signal intensity of R6G obtained with Fe3O4 / HAP / Ag as the substrate was significantly enhanced.

[0077] In addition, R6G has a high affinity to 240 nm at 611, 771, 1183, 1309, 1362, 1507, and 1647 cm -1 The obvious Raman bands at Figure 6 As shown, the Fe3O4 / HAP / Ag substrate has the potential to be used for SERS signal enhancement of target molecules.

[0078] Example 4

[0079] This embodiment provides an application of the Fe3O4 / HAP / Ag nanocomposite material prepared in Example 1 for detecting ciprofloxacin (CIP).

[0080] Take 33 mg of CIP powder and add deionized water to 100 mL to obtain a concentration of 1×10 -3 mol / L CIP solution, and then diluted to 1×10 -3 , 1×10 -4 , 1×10 -5 , 1×10 -6 , 1×10 -7 and 1×10 -8 mol / L CIP solution.

[0081] Then, 1 mg of the Fe3O4 / HAP / Ag powder prepared in Example 1 was prepared into a solution and smeared on a glass plate to dry as a substrate, and the CIP solution was drop-coated on the substrate for SERS measurement.

[0082] The SERS measurement used a 633 nm laser as the excitation source, with an acquisition time of 10 s, a laser power of 50 mW, and a spectrum acquisition range of 600 to 1800 cm -1 .

[0083] The actual method for detecting antibiotic residues on the surface of fish is: first, soak the whole fish in antibiotic aqueous solutions of different concentrations (concentration range 1×10 -3 ~1×10 -8 mol / L) for a few minutes to prepare fish samples with different added antibiotics; then, after wiping off the residual liquid on the fish surface, the Fe3O4 / HAP / Ag nanocomposite was immediately applied on the fish skin, and then the material was transferred to a clean glass slide by an attached magnet for SERS measurement.

[0084] In order to detect antibiotic residues in fish pond water, water from the Han River was used as a simulated fish pond water, and water samples with different concentrations of antibiotics (1×10 -3 , 1×10 -5 and 1×10 -7 mol / L). The spiked water sample was first treated with potassium aluminum sulfate dodecahydrate, and then filtered with a microporous filter (0.22 μm) to remove insoluble impurities. Then, 1 mg of the Fe3O4 / HAP / Ag powder prepared in Example 1 was prepared into a solution and smeared on a glass plate to dry as a substrate. Then, the water sample was drop-coated on the substrate for SERS measurement.

[0085] Stability and reproducibility experiments: To illustrate the stability of Fe3O4 / HAP / Ag as a substrate, samples were tested every 7 days using the same batch of substrates. To illustrate the reproducibility of the Fe3O4 / HAP / Ag substrate, CIP of the same concentration was tested 11 times using different batches of Fe3O4 / HAP / Ag samples.

[0086] Example 5

[0087] In this embodiment, Fe3O4 / HAP / Ag is used as the substrate to detect the content of CIP through SERS.

[0088] Using CIP as the target molecule for analysis, the dispersed Fe3O4 / HAP / Ag particles were coated on a silicon wafer and air-dried at room temperature as a substrate. CIP of different concentrations was dropped on the substrate and the wavelengths of 600 to 1800 cm were measured on a confocal Raman spectrometer (633 nm, Renishaw, Great Britain). -1 SERS spectra of random positions on the Fe3O4 / HAP / Ag substrate within a certain range. At the same time, CIP standard solutions with different concentrations were drop-coated on the substrate for Raman detection.

[0089] 1358cm -1 Mixed vibration (pyrazine ring); 1382cm -1 ν sym (OCO); 1488cm -1 ν(OCO); 1622cm -1 ν symmetry (C=C, aromatic ring).

[0090] In 1.0×10 -8 ~1.0×10 -3 In the mol / L range, 1382 cm -1 The characteristic peak intensity at increases with the increase of CIP concentration. Figure 7 shown.

[0091] Based on the constructed SERS substrate, the Raman characteristic peak intensities of CIP solutions with different concentrations are as follows: Figure 8 As shown in the figure, different concentrations of CIP were used at 1382 cm -1 The working curve was constructed at the intensity of 1.0×10 -8 ~1.0×10 -3 mol / L showed a good linear relationship, R 2 is 0.9960, such as Figure 7 shown.

[0092] like Figure 7 As shown, if the concentration of CIP is less than 10 -9mol / L, there is no detectable signal. At the same time, the detection limit LOD is calculated using the formula (LOD = 3δ / k), where δ is the standard deviation of the blank and k is the slope of the standard curve at 1382 cm -1 peak, the detection limit was 7.5×10 -9 mol / L, the two are basically the same.

[0093] In order to verify the stability of Fe3O4 / HAP / Ag, SERS measurements over time were performed, and the results are shown in Fig. 9 The results show that the intensity of the SERS signal has no significant change within one month, and Fe3O4 / HAP / Ag is stable during the storage process.

[0094] In addition, repeatability plays an important role in surface enhanced Raman scattering. To evaluate the repeatability of Fe3O4 / HAP / Ag, samples were analyzed at 11 random locations under the same conditions, and the relative standard deviation was 8.66%, indicating that the SERS method has good reproducibility, such as Fig.10 shown.

[0095] Ciprofloxacin at 1382 cm -1 The enhancement factor EF at 5 , attributed to the SERS enhancement of CIP by Fe3O4 / HAP / Ag, due to the LSPR of Ag, Fe3O4 / HAP / Ag plays an important role in the enhancement, and silver nanoparticles produce a strong local surface plasmon resonance effect under laser irradiation, which will produce a very strong local electromagnetic field on the surface of silver nanoparticles, thereby greatly enhancing the Raman scattering signal of nearby molecules ("Tunable and enhanced SERS activity of magneto-plasmonic Ag-Fe3O4 nanocomposites with one pot synthesize method", Fan et al, Journal of Optics, 19(1), 015401, December 2016). Fe3O4 / HAP / Ag can play an important role in the electromagnetic field enhancement effect of ciprofloxacin, thereby enhancing its Raman scattering signal.

[0096] The charge transfer effect between ciprofloxacin molecules and HAP will also enhance the Raman signal. This charge transfer will change the vibration mode of the molecule, thereby enhancing the Raman scattering signal. Hydroxyapatite has good biocompatibility and high surface energy, and can adsorb ciprofloxacin molecules. The adsorbed ciprofloxacin molecules undergo chemical interactions on the HAP surface, and these interactions can change the electronic structure of the molecule, thereby affecting its Raman scattering characteristics.

[0097] Because Fe3O4 / HAP / Ag as a Raman substrate can enhance the Raman signal, which can be explained by the principles of electromagnetic field enhancement and charge transfer. Therefore, using Fe3O4 / HAP / Ag material as a substrate for SERS detection can achieve the purpose of rapid detection of antibiotic CIP residues in aquatic organisms.

[0098] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a Fe3O4 / HAP / Ag nanocomposite material, characterized in that: The following steps are involved: S1. Preparation of Fe3O4 nanoparticles: Adding double distilled water into a three-necked flask, placing it in a water bath and mechanically stirring it, introducing nitrogen for deoxygenation, adding FeSO4 and FeCl3·6H2O, stirring until the solid is completely dissolved, heating the water bath to 60°C, then adding sodium hydroxide solution dropwise thereto to adjust the pH value and react fully, stopping stirring, raising the water bath temperature to 80°C, and fully aging, then stopping adding nitrogen, washing the solution after cooling it to room temperature, and obtaining Fe3O4 fluid when the pH value of the solution after washing is 7.0, drying it, and grinding and preserving it after cooling it to room temperature to obtain Fe3O4 nanoparticles; S2. Preparation of magnetic hydroxyapatite (Fe3O4 / HAP) nanoparticles: S201, preparing a hydroxyapatite precursor solution: adding sodium citrate to a calcium nitrate solution, stirring thoroughly, adding a disodium hydrogen phosphate solution dropwise, and then adding a sodium hydroxide solution to adjust the pH value to obtain a mixed solution, and after the reaction is completed, placing the solution under sealing conditions and continuing to stir the reaction to obtain a hydroxyapatite precursor solution; S202, preparing dispersed Fe3O4 nanoparticles: taking the Fe3O4 nanoparticles prepared in S1 and dispersing them by ultrasonic to obtain dispersed Fe3O4 nanoparticles; S203, preparing Fe3O4 / HAP nanoparticles: putting the dispersed Fe3O4 nanoparticles prepared in S202 into the hydroxyapatite precursor solution prepared in S201 and fully stirring, and continuously reacting at high temperature, after the reaction is completed, washing by centrifugation and drying, and grinding to obtain Fe3O4 / HAP nanoparticles; S3, preparing nano silver seed solution: taking silver nitrate solution and sodium citrate solution 1 and mixing them, adding hydrogen peroxide thereto, stirring and mixing them well to obtain a mixed solution, injecting sodium borohydride into the mixed solution with a syringe, and letting it stand at room temperature after sufficient reaction to obtain nano silver seed crystals, taking the nano silver seed crystals and dissolving them in deionized water, adding a mixed solution of sodium citrate solution 2 and ascorbic acid, and then adding silver nitrate solution to continue the reaction to obtain nano silver seed solution; S4, preparation of Fe3O4 / HAP / Ag nanocomposite material: the Fe3O4 / HAP nanoparticles prepared in S2 are dissolved in water to obtain a Fe3O4 / HAP solution, and after ultrasonic dispersion, a sodium hydroxide solution is added to adjust the pH value of the Fe3O4 / HAP solution, and then the solution is heated in a water bath while being stirred, and the nanosilver seed solution prepared in S3 is added to the Fe3O4 / HAP solution, and after sufficient reaction and aging, a precipitate is obtained, which is washed and dried, and then ground to obtain a Fe3O4 / HAP / Ag nanocomposite material.

2. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The mass volume ratio of the double distilled water, FeSO4 and FeCl3·6H2O in S1 is 75.0 mL:1.39 g:2.7 g, and the concentration of the sodium hydroxide solution is 3 mol / L.

3. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The deoxygenation time in S1 is 30 minutes, the pH value is adjusted to 9.0-10.0, the sufficient reaction time is 30 minutes, the aging time is 60 minutes, the washing detergent is anhydrous ethanol and deionized water, the oven temperature is 60°C, and the drying condition is drying in an oven at 60°C for 12 hours.

4. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The mass volume ratio of the calcium nitrate solution, sodium citrate and disodium hydrogen phosphate solution in S201 is 100 mL:2.351 g:100 mL, the concentration of the calcium nitrate solution is 0.30 mol / L, the concentration of the disodium hydrogen phosphate solution is 0.18 mol / L, the time for sufficient stirring in S201 is 10 min, the pH value is 10.0, and the stirring reaction time is 1 to 2 h.

5. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The mass of Fe3O4 in S202 is 2.312 g, the temperature of the ultrasonic cleaner is 45° C., and the dispersion time of the ultrasonic cleaner is 20 min.

6. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The mass volume ratio of the Fe3O4 nanoparticles and the hydroxyapatite precursor solution in S203 is 1:40, the temperature of the high temperature continuous reaction is 180°C, the time of the high temperature continuous reaction is 24h, and the drying condition is drying in an oven at 80°C for 12h.

7. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The volume ratio of the silver nitrate solution, sodium citrate solution 1, hydrogen peroxide and sodium borohydride in S3 is 0.60 mL: 23.5 mL: 0.1 mL: 0.60 mL, the concentration of the silver nitrate solution is 0.01 mol / L, the concentration of the sodium citrate solution 1 is 2.5×10 -4 mol / L, the concentration of the hydrogen peroxide is 1.875 mol / L, the concentration of the sodium borohydride is 0.01 mol / L, the time for sufficient reaction is 15 min, and the standing time is 2 h.

8. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The volume ratio of the nanosilver seeds, deionized water, sodium citrate solution 2, ascorbic acid and silver nitrate solution in S3 is 2mL:16mL:1.0mL:2.0mL:1.0mL, the concentration of the sodium citrate solution 2 is 0.075mol / L, the concentration of the ascorbic acid is 0.1mol / L, and the reaction time is 30min.

9. The method for preparing the Fe3O4 / HAP / Ag nanocomposite material according to claim 1, characterized in that: The mass of the Fe3O4 / HAP nanoparticles in S4 is 0.10g, the volume of the Fe3O4 / HAP solution is 50mL, the ultrasonic dispersion time is 60min, the concentration of the sodium hydroxide solution is 1.0mol / L, the pH value is 10.0, the temperature of the water bath is 70°C, the sufficient reaction time is 1h, the aging time is 24h, the detergent for washing is deionized water, and the drying condition is drying in an oven at a temperature of 80°C for 12h. The method of adding the nanosilver seed solution prepared in S3 to the Fe3O4 / HAP solution in S4 is: adding the nanosilver seed solution prepared in S3 thereto in 8 times, each time with an interval of 20min, and adding 20mL of the nanosilver seed solution each time.

10. An application of the method for preparing Fe3O4 / HAP / Ag composite nanomaterials according to any one of claims 1 to 9, characterized in that: The prepared Fe3O4 / HAP / Ag composite nanomaterial is used as a substrate for SERS detection to detect antibiotic residues in aquatic organisms.

Citation Information

Cited By

  • Antibacterial hydrogel dressing and preparation method thereof

    CN120586147A