Preparation method of copper-modified aluminum composite material and application of copper-modified aluminum composite material to reduction-method complex breaking of alkaline cyanided gold-containing wastewater or wet-process gold extraction pregnant solution and recovery of gold from alkaline cyanided gold-containing wastewater or wet-process gold extraction pregnant solution
Through the mechanical ball milling preparation of copper-modified aluminum composite materials, the gold recycling problem caused by the stability of gold cyanide under alkaline conditions is solved, efficient gold bursting and recycling is achieved, and the inefficiency and pollution problems of traditional methods are overcome. Provides an economical and sustainable water treatment technology.
Patent Information
- Application Number
- CN202411527338.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-30
AI Technical Summary
The prior art is difficult to efficiently crack the gold cyanide complex under alkaline conditions, resulting in difficulty in recycling gold. Traditional methods have problems such as low utilization rate and secondary pollution.
The copper-modified aluminum composite is prepared by mechanical ball milling, and the aluminum-copper microcell is formed by cutting the aluminum surface oxide film with copper salt to achieve direct reduction of gold cyanide complex and recovery of gold.
Effectively cracking gold cyanide complex under strong alkaline conditions, improving the recycling efficiency of gold, widely used materials, low prices, simple preparation technology, suitable for industrial production, and has stability and continuous utilization capabilities.
Smart Images

Figure CN119038697A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution treatment and resource utilization, and specifically relates to a preparation method of a copper-modified aluminum composite material and its application in breaking chelates in alkaline cyanide gold-containing wastewater or wet gold extraction precious liquid reduction method and recovering gold therefrom. Background Art
[0002] Due to the irreplaceable advantages of cyanide in the gold industry, cyanide plating solution is usually used to improve the quality of the coating during gold plating. Every year, my country produces a large amount of cyanide gold-containing wastewater in the electroplating, electronics, jewelry processing and other industries. In addition, as the world's largest gold producer, wet gold extraction is widely used, and the gold extraction precious liquid is usually reduced by zinc method. At present, about 80% of the world's gold is still leached through cyanide. In cyanide gold-containing wastewater and wet gold extraction precious liquid, gold and cyanide ions will form a stable complex Au(CN)2 - , which increases the difficulty of gold recovery. However, the reserves of gold are limited, and recovering gold from cyanide wastewater or improving the efficiency of gold extraction precious liquid treatment still has extremely important practical significance.
[0003] There are two difficulties in recovering gold from water containing gold-cyanide complex: ① The complex formed by cyanide and gold is very stable (lg β Au(CN)2- = 36.6), which increases the difficulty of gold recovery; ② This type of water is usually highly alkaline (pH = 9.5 ~11), and lowering the pH will dissociate highly toxic cyanide ions or hydrocyanic acid gas ( p K a = 9.21). Given the difficulty in recovering gold from wastewater containing gold-cyanide complexes, there are few related studies. Traditional adsorption, solvent extraction, and electrodialysis methods can only be used for simple enrichment without breaking the complex, and further extraction and reduction are required. In addition, the commonly used zero-valent metal (zinc powder) reduction replacement method for extracting gold from cyanide precious liquid is simple and easy to implement, but it has disadvantages such as low utilization rate and easy to generate secondary pollution.
[0004] In order to meet the requirements of efficient and convenient gold recovery, it is urgent to develop a new technology to break the composite stability of gold cyanide under alkaline conditions and recover gold from low-concentration gold cyanide water. 0 ) has better performance and is developing a new type of water treatment technology. 0 Has an extremely negative redox potential (E0(Al 3+ / Al 0) = - 2.33 V), has stronger reducing properties, and has amphoteric properties. It is still highly active under strong alkaline conditions and is expected to achieve efficient direct reduction of gold-cyanide complexes. However, the presence of an oxide film on the aluminum surface will inhibit its active release. Zero-valent copper is generated in situ on the zero-valent aluminum surface modified by copper salts, forming an aluminum-copper primary battery to promote the transmission of electrons. Based on this, the present invention uses a one-step addition of copper-modified aluminum composite materials, and for the first time uses zero-valent aluminum materials to achieve the reduction and decomposition of gold in gold-cyanide complex water and simultaneously recover Au. 0 . Summary of the invention
[0005] The purpose of the present invention is to overcome the application bottleneck of zero-valent aluminum to prepare a copper-modified aluminum composite material, and to achieve direct reduction and decomposition of a gold-cyanide complex by simply adding the copper-modified aluminum composite material in one step.
[0006] By mechanical ball milling with the assistance of copper salt, a new copper-modified micron aluminum material (copper-modified aluminum composite material) is obtained. The oxide film on the surface of the micron aluminum is destroyed by the cutting action of the copper salt crystals, and the solid phase reduction occurs during the ball milling process to make the Cu 0 The copper-copper composite material can be locally generated and covered on the aluminum surface to prevent secondary passivation of the material. In addition, due to the formation of aluminum-copper micro-batteries, the electronic transmission function of the material is improved. Based on this, the copper-modified aluminum composite material can be reduced and broken and gold can be recovered in strong alkaline cyanide gold-containing wastewater or wet gold extraction precious liquid. The high-priced Au is converted into Au 0 The material of the invention has wide sources, low price, simple preparation process, and can maintain high activity and high electron utilization under strong alkaline conditions.
[0007] The present invention provides a preparation method of a copper-modified aluminum composite material and its application in reducing alkaline cyanide gold-containing wastewater or wet gold extraction precious liquid to break the chelate and recover gold therefrom. The specific steps are as follows: P1. Preparation method of copper-modified aluminum composite material: zero-valent aluminum powder and copper salt are mixed, grinding balls are used as grinding media, and ball milling is performed in a ball mill in an inert gas protective atmosphere. Then, the copper-modified aluminum composite material can be obtained; P2. Add the copper-modified aluminum composite material to the cyanide gold-containing wastewater or wet gold extraction precious liquid, and stir / shake continuously to ensure that the material is in full contact with the gold cyanide complex ions in the water, so that it remains in a suspended state and undergoes a reduction and decomplexation reaction.
[0008] As above, in step P1, the molar ratio of zero-valent aluminum powder to copper salt is 5-200:1. The grinding balls are one or more of zirconium oxide grinding balls, chromium alloy cast iron grinding balls, martensitic ductile iron grinding balls, steel balls and agate balls. The copper salts include but are not limited to CuSO4 and its hydrates, CuCl2 and its hydrates, Cu(NO3)2 and its hydrates, etc. The inert gas is nitrogen, helium or argon, etc.
[0009] As described above, in step P2, the copper-modified aluminum composite material is added in an amount of 0.5 to 4 g / L (not limited thereto, the amount depends on the content of the gold-cyanide complex in the water, calculated as gold element).
[0010] As mentioned above, step P2 requires deoxygenation of the water (continuously introducing inert gas, or isolating the water from air in a closed environment after introducing inert gas for a certain period of time) to maintain the dissolved oxygen concentration < 0.5 mg / L.
[0011] As above, after step P2 is fully reacted, the stirring / vibration is stopped and the Au 0 The solid powder was recovered by negative pressure filtration and freeze drying.
[0012] The present invention can prepare copper-modified aluminum composite materials by a simple mechanical ball milling process, and the oxide film on the surface of micron aluminum is destroyed by the cutting effect of copper salt crystals, and at the same time, the solid phase chemical reaction can generate Cu in situ. 0 It partially covers the aluminum surface to inhibit the secondary formation of the passivation film. In addition, due to the formation of the aluminum-copper primary battery, the electronic utilization rate of the material can be improved.
[0013] The advantages of the present invention are as follows: (1) The copper salt used in the present invention is an industrial-grade raw material and can be used on a large scale. Aluminum resources are abundant and micron aluminum is cheap.
[0014] (2) The preparation method of the copper-modified aluminum composite material is carried out at room temperature and pressure. The reaction conditions are mild and simple and it is completed in one step. The mechanical ball milling powder material preparation process involved is suitable for industrial production.
[0015] (3) The removal method of the present invention is simple. The material can be directly added under the original alkaline conditions of cyanide gold-containing wastewater or wet gold extraction precious liquid. No other pretreatment is required, and no repeated pH adjustment is required. It is convenient and quick.
[0016] (4) The present invention solves the problem of surface passivation film hindering electron release in the current practical application of zero-valent aluminum, and enables it to have a certain degree of stability and sustainable utilization ability.
[0017] (5) The present invention can effectively break the complex and recover gold in a strong alkaline pH range, under various ion interferences and in a variety of real water environments, thus realizing the resource utilization of sewage treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 To remove Au(CN)2 from the copper-modified aluminum composites prepared by ball milling micron aluminum with CuSO4·5H2O, CuCl2·2H2O, and Cu(NO3)2·3H2O - 's effect diagram.
[0019] Figure 2 Removal of Au(CN)2 from copper-modified aluminum composites prepared with different ball milling times - 's effect diagram.
[0020] Figure 3 Removal of Au(CN)2 from copper-modified aluminum composites prepared at different ball milling speeds - 's effect diagram.
[0021] Figure 4 Au(CN)2 was removed from copper-modified aluminum composites, micronized aluminum alone, CuSO4·5H2O alone, ball-milled micronized aluminum alone, ball-milled CuSO4·5H2O alone, and physical mixture of micronized aluminum and CuSO4·5H2O. - 's effect diagram.
[0022] Figure 5 Decomplexation and removal of Au(CN)2 from copper-modified aluminum composites at different pH conditions - 's effect diagram.
[0023] Figure 6 Decomplexation and removal of Au(CN)2 from copper-modified aluminum composites at different dissolved oxygen concentrations - 's effect diagram.
[0024] Figure 7 The effect of different addition amounts of copper-modified aluminum composites on Au(CN)2 - Diagram of the decomplexation and removal effect.
[0025] Figure 8 Cyclic degradation of Au(CN)2 in copper-modified aluminum composites - .
[0026] Fig. 9 Decomplexation and removal of Au(CN)2 from copper-modified aluminum composites under the interference of different coexisting substances - 's effect diagram.
[0027] Fig.10 Copper modified aluminum composites and Au(CN)2 - XPS spectrum of the solid filtered out after the reaction was complete. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with specific implementation cases. The described specific implementation cases are only used to explain the present invention and are not limited to the present invention.
[0029] Example 1 Removal of Au(CN)2 from water by copper-modified aluminum composites ball-milled with different copper salts - Comparison of the effects The micron-sized zero-valent aluminum powder was mixed with CuSO4·5H2O, CuCl2·2H2O, and Cu(NO3)2·3H2O in a certain molar ratio. The mixture was ball-milled in a nitrogen atmosphere to obtain different copper-modified aluminum composite materials. The Au(CN)2 - Simulate water, at room temperature, to adjust Au(CN)2 - Simulate the initial pH of water to 10.5, use nitrogen to remove dissolved oxygen in the water and isolate the air, then add different materials directly into the water and shake them to mix evenly and keep them in suspension to maintain the reduction reaction, and regularly sample and filter the remaining Au(CN)2 in the water for analysis - .like Figure 1 As shown in the figure, different copper salt ball milling materials have good removal effects, proving that aluminum can mechanochemically reduce Cu(II) to Cu during ball milling. 0 , anions have little effect.
[0030] Example 2 Effect of ball milling time on the removal of Au(CN)2 from water by copper-modified aluminum composites - The impact of the effect Mix micron-sized zero-valent aluminum powder and CuSO4·5H2O in a certain molar ratio. Ball milling was performed in a nitrogen atmosphere. Different copper-modified aluminum composite materials were obtained by ball milling for 0.5 h, 1 h, 2 h, and 3 h respectively. The concentration of Au(CN)2 - Simulate water, at room temperature, to adjust Au(CN)2 - Simulate the initial pH of water to 10.5, use nitrogen to remove dissolved oxygen in the water and isolate the air, then add different materials directly into the water and shake them to mix evenly and keep them in suspension to maintain the reduction reaction, and regularly sample and filter the remaining Au(CN)2 in the water for analysis - .like Figure 2 As shown, a shorter ball milling time is sufficient to fully develop the activity of the material.
[0031] Example 3 Effect of ball milling speed on the removal of Au(CN)2 from water by copper-modified aluminum composites - The impact of the effect Mix micron-sized zero-valent aluminum powder and CuSO4·5H2O in a certain molar ratio. Ball milling was performed in a nitrogen atmosphere, and the rotation speed of the ball mill was adjusted to 100, 150, 200, 250, and 300 rpm to obtain different copper-modified aluminum composite materials. The concentration of Au(CN)2 was 20 mg / L (in terms of gold element). - Simulate water, at room temperature, to adjust Au(CN)2 -Simulate the initial pH of water to 10.5, use nitrogen to remove dissolved oxygen in the water and isolate the air, then add different materials directly into the water and shake them to mix evenly and keep them in suspension to maintain the reduction reaction, and regularly sample and filter the remaining Au(CN)2 in the water for analysis - .like Figure 3 As shown in the figure, a higher ball milling speed is more conducive to the performance of material properties.
[0032] The preparation method of the copper-modified aluminum composite material described below is as follows: micron-sized zero-valent aluminum powder and CuSO4·5H2O are mixed in a molar ratio of 30:1, and ball milled in a nitrogen atmosphere. The ball mill is kept at a speed of 300 rpm for 1 h to obtain the copper-modified aluminum composite material.
[0033] Example 4 Removal of Au(CN)2 from water using different materials - Comparison of the effects Prepare Au(CN)2 at a concentration of 20 mg / L (in terms of gold element) - Simulate water, at room temperature, to adjust Au(CN)2 - The initial pH of the simulated water was set to 10.5, and the dissolved oxygen in the water was removed by nitrogen and the air was isolated. Then, the copper-modified aluminum composite material was directly added to the water and oscillated to mix it evenly and keep it in a suspended state to maintain the reduction reaction. The remaining Au(CN)2 in the water was sampled and filtered at regular intervals for analysis. - At the same time, commercial micron-sized zero-valent aluminum, micron-sized zero-valent aluminum milled alone, commercial CuSO4·5H2O, CuSO4·5H2O milled alone, and a physical mixture of micron-sized aluminum and CuSO4·5H2O were used as controls. Figure 4 As shown in the figure, commercial micron-sized zero-valent aluminum, ball-milled micron-sized zero-valent aluminum alone, commercial CuSO4·5H2O, ball-milled CuSO4·5H2O alone, and physical mixture of micron-sized aluminum and CuSO4·5H2O can only remove a small amount of Au(CN)2 - However, the method of the present invention can efficiently remove Au(CN)2 - More than 99% was achieved, proving that this method can remove Au(CN)2 - feasibility.
[0034] Example 5 Decomplexation and removal of Au(CN)2 from copper-modified aluminum composite materials at different pH conditions - Prepare Au(CN)2 at a concentration of 20 mg / L (in terms of gold element) - Simulate water, at room temperature, to adjust Au(CN)2 -The initial pH of the simulated water was 9.5, 10.0, 10.5, 11.0, 11.5, and 12.0, respectively. Nitrogen was used to remove dissolved oxygen in the water and the air was isolated. Then, the copper-modified aluminum composite material was directly added to the water and oscillated to mix it evenly and keep it in a suspended state to maintain the reduction reaction. The remaining Au(CN)2 in the water was sampled and filtered at regular intervals for analysis. - .like Figure 5 As shown in Figure 2, the copper-modified aluminum composite material can effectively decomplex and remove Au(CN)2 in most strong alkaline environments. - .
[0035] Example 6 Decomplexation and removal of Au(CN)2 from copper-modified aluminum composite materials at different dissolved oxygen concentrations - Prepare Au(CN)2 at a concentration of 20 mg / L (in terms of gold element) - Simulate water, at room temperature, to adjust Au(CN)2 - Simulated water, adjusted the initial pH to 10.5, and subjected to three treatments: nitrogen treatment; no treatment; oxygen treatment. The initial dissolved oxygen content in the water was clearly distinguished. Then copper-modified aluminum composite materials were directly added to the water and shaken to mix evenly and keep the suspension state to maintain the reduction reaction. Samples were taken regularly to filter and analyze the remaining Au(CN)2 in the water. - .like Figure 6 As shown, this method must be carried out under deoxygenated conditions to effectively reduce and decomplex Au(CN)2 - .
[0036] Example 7 Effect of different addition amounts of copper-modified aluminum composite materials on Au(CN)2 - Decomplexation removal At room temperature, the concentration of Au(CN)2 was 20 mg / L (in terms of gold element). - Simulate water, adjust the initial pH to 10.5, remove dissolved oxygen in the water with nitrogen and isolate the air, then add 0.25 g / L, 0.5 g / L, 1.0 g / L, 1.5 g / L, 2.0 g / L of copper-modified aluminum composite materials, shake to mix evenly and keep them in suspension to maintain the reduction reaction, take samples and filter them regularly to analyze the remaining Au(CN)2 in the water - .like Figure 7 As shown, Au(CN)2 can be achieved with less material dosage - Efficient and rapid degradation.
[0037] Example 8 Cyclic degradation of Au(CN)2 by copper-modified aluminum composites - Prepare Au(CN)2 at a concentration of 20 mg / L (in terms of gold element)- Simulating water, at room temperature, by adding ammonia-ammonium chloride buffer solution to Au(CN)2 - The pH value of simulated water was stabilized at 10.5. Nitrogen was used to remove dissolved oxygen in the water and the air was isolated. Then, copper-modified aluminum composite materials were directly added to the water and shaken to mix evenly and keep it in suspension to maintain the reduction reaction. Samples were taken regularly to filter and analyze the remaining Au(CN)2 in the water. - After each reaction, the solid material was separated from the solution by suction filtration, freeze-dried and repeated the above steps, with each reaction time being 30 minutes. Figure 8 As shown, after five cycles, the copper-modified aluminum composite material still has good activity, proving that the material has a certain ability to be reused.
[0038] Example 9 Decomplexation and removal of Au(CN)2 from copper-modified aluminum composite materials under the interference of different coexisting substances - Prepare Au(CN)2 at a concentration of 20 mg / L (in terms of gold element) - Simulate water, add different coexisting substances with the same molar concentration, adjust the initial pH of the simulated water to 10.5 at room temperature, remove dissolved oxygen in the water with nitrogen and isolate the air, then directly add copper-modified aluminum composite material and shake it to mix evenly and keep it in suspension to maintain the reduction reaction, and regularly sample and filter the remaining Au(CN)2 in the water for analysis - .like Fig. 9 As shown, the copper-modified aluminum composite material can effectively shield the interference of multiple coexisting ions, proving that the copper-modified aluminum composite material has a certain anti-interference ability.
[0039] Example 10 Copper-modified aluminum composite material and Au(CN)2 - After sufficient reaction, the Au-attached material is recovered The serum bottle after the reaction was taken out from the oscillator, filtered to separate the solid and liquid, and the filter paper containing the solid powder was placed in a culture dish. After freeze drying, the obtained material was analyzed by X-ray electron spectroscopy. Fig.10 As shown, there is Au on the surface of the material 0 The generation of Au materials is recycling.
Claims
1. A method for preparing a copper-modified aluminum composite material, characterized in that: The method comprises the following steps: Zero-valent aluminum powder and copper salt are mixed in a molar ratio of 5-200:1, grinding balls are used as grinding media, and ball milling is performed in an inert gas (nitrogen, argon, helium, etc.) protective atmosphere. After one-step ball milling, a copper-modified aluminum composite material can be obtained.
2. The preparation method according to claim 1, characterized in that: The grinding balls are one or more of zirconia grinding balls, chromium alloy cast iron grinding balls, martensitic ductile iron grinding balls, steel balls and agate balls; the copper salts include but are not limited to CuSO4 and its hydrates, CuCl2 and its hydrates, Cu(NO3)2 and its hydrates, etc.; the inert gas is nitrogen, helium or argon, etc.
3. An application of the copper-modified aluminum composite material prepared by the preparation method according to claim 1 in reducing and breaking the chelate of alkaline cyanide gold-containing wastewater or wet gold extraction precious liquid and recovering gold at the same time, characterized in that: The prepared copper-modified aluminum composite material is added to alkaline cyanide gold-containing wastewater or wet gold extraction precious liquid, and the copper-modified aluminum composite material and pollutants are fully mixed through shaking / stirring, and the gold is reduced and decomplexed and recovered.
4. The use according to claim 3, characterized in that: The water needs to be deoxygenated (continuously introducing inert gas, or isolating the water from air in a closed environment after introducing inert gas for a certain period of time) to maintain the dissolved oxygen concentration < 0.5 mg / L.
5. The use according to claim 3, characterized in that: The dosage of the copper-modified aluminum composite material is 0.1 to 5 g / L (not limited thereto, a higher dosage is more conducive to performance).
Citation Information
Patent Citations
Preparation method of aluminum-carbon nanotube composite material and application of aluminum-carbon nanotube composite material in removal of refractory pollutants in water
CN113603204A
Preparation method and application of magnetically separable zero-valent aluminum-ferroferric oxide compound
CN114436389A
Preparation method and application of aluminum-copper-carbon composite material for efficiently reducing nitrate into nitrogen
CN116062870A
Preparation method and application of aluminum-zinc-carbon composite material for rapidly and selectively reducing nitrate
CN116161766A
Method for directly reducing, decomplexing and recovering copper from complex copper wastewater
CN116789308A
Cited By
Negative pressure suction filtration type cyanidation gold extraction system and control method thereof
CN119571078A
A negative pressure filtration type cyanide gold extraction system and its control method
CN119571078B
Extremely simple activating and balling method for millimeter-scale commercial aluminum particles
CN121514506A