Surface treatment method of glass accessory
Through the new surface treatment methods of glass accessories, including isopropanol solution soaking, plasma treatment, coating cleaners and primers, and the use of combined glue, the poor bonding reliability of high-glass fiber materials and glass is solved. Problem, improving bond strength and production stability.
Patent Information
- Application Number
- CN202411245825.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the bonding reliability of glass accessories with high-glass fiber materials (glass fiber accounts for >30%) and glass is poor, and it is easy to cause bonding failure or strength does not meet the requirements.
A new method of surface treatment for glass accessories, including cleaning treatment, plasma treatment, coating attachment cleaning agents and primers, and using a combined glue to improve bonding strength, specific steps include isopropanol solution soaking, plasma treatment , coating accessories cleaners and primers, and the use of combined glue.
It effectively improves the bonding reliability of high-glass fiberglass accessories and glass, ensures that the production process is stable and the strength after bonding meets the requirements, improves product results, and has good promotion prospects and application value.
Smart Images

Figure CN119038889A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass accessories, and in particular to a surface treatment method for a glass accessory. Background Art
[0002] In recent years, with the development of the automobile industry, smooth and flowing flush doors with beautiful installation and low wind noise have gradually become a popular trend; among them, some OEMs' flush doors have begun to use high-glass fiber materials as sliders and other glass accessories to be glued and fixed to the glass, so as to guide the glass to slide in the door.
[0003] In the prior art, when glass accessories such as sliders are bonded to the door glass, the accessories need to be surface treated first, and then glue is applied to the surface of the accessories, so that a better bonding effect can be achieved between the accessories and the glass. The surface treatment method of the accessories is: first wipe and clean the surface of the accessories, then activate the surface of the accessories, and finally apply a primer on the surface of the accessories. The Chinese patent document with the publication number CN103639157A and the publication date March 19, 2014, entitled "A Surface Treatment Method for Glass Accessories", discloses a surface treatment method for glass accessories, which first cleans the bonding area of the surface of the glass accessories with alcohol, then performs plasma treatment, and then applies a primer to achieve the best bonding effect.
[0004] However, research has found that the above surface treatment method is only suitable for glass accessories with low glass fiber content (glass fiber ratio ≤ 30%) or PBT (polybutylene terephthalate), while for glass accessories with high glass fiber content (glass fiber ratio > 30%), the bonding to glass is prone to poor CF (Cohesion Failure) status, for example: after environmental hanging weight, CF is less than 80%, the tensile or shear force cannot meet the requirements, or even defective products with no CF status. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a surface treatment method for a glass accessory to solve the problem of poor bonding reliability between existing glass accessories made of high glass fiber materials (glass fiber ratio>30%) and glass.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a surface treatment method for a glass accessory, wherein the glass fiber content of the glass accessory is greater than 30%, and the surface treatment method for the glass accessory comprises the following steps: S1: cleaning the bonding area of the glass accessory; S2: plasma treating the bonding area of the glass accessory; S3: applying an accessory cleaner to the bonding area of the glass accessory, and then drying; S4: evenly applying an accessory primer to the bonding area of the glass accessory, and then drying.
[0007] In the above technical scheme of the present invention, in order to solve the problem of poor bonding reliability between existing glass accessories made of high glass fiber materials (glass fiber ratio > 30%) and glass, a new process flow of a surface treatment method for glass accessories is designed. The process flow is simple and a new material surface treatment process is adopted, thereby effectively improving the bonding reliability between high glass fiber glass accessories and glass, especially glass accessories with a glass fiber ratio of more than 30%, which can ensure the stability of the production process and that the strength after bonding meets the requirements, improve the product effect obtained by bonding high glass fiber glass accessories and glass together, and is easy to implement and has good promotion prospects and application value.
[0008] Furthermore, in the surface treatment method of the present invention, in step S1, the bonding area of the glass accessory is soaked in an isopropanol solution, and the bonding area of the glass accessory is soaked in the isopropanol solution for 10-50 minutes, and then dried. Specifically, the bonding area of the glass accessory is soaked in the isopropanol solution for 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, etc.
[0009] It should be noted that in the above step S1, when the bonding area of the glass accessory is cleaned, the bonding area of the glass accessory can be soaked in an isopropyl alcohol solution and then dried. The concentration of the isopropyl alcohol solution and the soaking time of the glass accessory directly affect whether the bonding area of the glass accessory is effectively cleaned.
[0010] Therefore, in order to obtain a better implementation effect, in actual application, an isopropyl alcohol solution with an isopropyl alcohol content of >99.6% can be selected, and the bonding area of the glass accessory can be immersed in the isopropyl alcohol solution for 10-50 minutes to be completely cleaned.
[0011] Furthermore, in the surface treatment method of the present invention, in step S2, the compressed air used for plasma treatment is filtered and dried; wherein the oil content of the compressed air after the filtration and drying process is less than 0.05 mg / m 3 , dust particle size <0.05μm, no water, flow rate is 60-100L / min, and the plasma treatment speed of the bonding area of the glass accessories is 1-3cm / s. Specifically, the plasma treatment speed of the bonding area of the glass accessories is 1cm / s, 1.5cm / s, 2cm / s, 2.5cm / s, 3cm / s.
[0012] Furthermore, in the surface treatment method of the present invention, in step S2, the surface energy of the bonding area of the glass accessory after plasma treatment is ≥40mN / m. Specifically, the surface energy of the bonding area of the glass accessory after plasma treatment is ≥45mN / m, or ≥50mN / m, or ≥55mN / m, or ≥60mN / m, etc.
[0013] Furthermore, in the surface treatment method of the present invention, in step S3, the accessory cleaning agent contains 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine.
[0014] Further, in the surface treatment method of the present invention, in step S3, the mass percentage content of 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine is both less than 5%. Specifically, the mass percentage content of 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine is both ≤4.5%, or ≤4.0%, or ≤3.5%, or ≤3.0%, or ≤2.5%, or ≤2.0%, or ≤1.5%, or ≤1.0%, etc.
[0015] In the above technical solution of the present invention, in step S3, the reason why the accessory cleaner is applied to the bonding area of the glass accessory and the accessory cleaner is controlled to contain 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine is that: 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine can generate silanol (-Si-OH) under the catalysis of water, and the silanol reacts with the glass to generate new chemical bonds for deep cleaning.
[0016] Among them, considering that if the content of 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine in the above-mentioned accessory cleaning agent is too high, it will not only increase the production cost but also affect the subsequent application effect. In actual application, the mass percentage content of the above-mentioned 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine can be specifically controlled to be less than 5%.
[0017] Furthermore, in the surface treatment method of the present invention, in step S4, the accessory primer contains: ethyl acetate, diisocyanate, n-butyl acetate and polyisocyanate.
[0018] In the above technical solution of the present invention, the reason why the accessory primer contains: ethyl acetate, diisocyanate, n-butyl acetate and polyisocyanate is to ensure that the primer contains isocyanate groups (-N=C=O). When the accessory primer is actually used, the isocyanate groups in the accessory primer can react with epoxy groups, or thiol groups (-SH), or amino groups (-NH), or hydroxyl groups (-OH) to generate new chemical bonds; and the isocyanate groups (-N=C=O) contained in the primer can polymerize under the catalysis of water to generate polyurea (-NH-CO-NH-), thereby promoting the adhesion between the glass accessory and the glass.
[0019] Furthermore, the surface treatment method of the present invention further comprises step S5: coating glue on the bonding area of the glass attachment.
[0020] Further, in the surface treatment method of the present invention, in step S5, the glue includes a first glue and a second glue, the first glue is applied to the left and right end regions of the bonding area of the glass attachment, and the second glue is applied to the middle region of the bonding area of the glass attachment; wherein the area ratio of at least one of the left and right end regions to the middle region is 0.2 to 5. Specifically, the area ratio of at least one of the left and right end regions to the middle region is 0.2, 0.7, 1, 1.3, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.3, 3.5, 3.8, 4, 4.3, 4.5, 4.8, 5, etc.
[0021] Furthermore, in the surface treatment method described in the present invention, the first glue is polyurethane glue or PU glue, and the second glue is a two-component fast-curing glue.
[0022] In the above technical solution of the present invention, in order to further improve the bonding effect between the glass attachment and the glass, in actual setting, a combined glue can also be used for bonding, that is, the glue used includes a first glue and a second glue, and the first glue and the second glue have different components, so that the two glues are respectively coated on different preset areas on the bonding area of the glass attachment, and the area ratio of each coating area is controlled. Among them, in some preferred embodiments, in order to obtain better implementation effects, the first glue can be specifically polyurethane glue or PU glue, and the second glue can be selected as a two-component fast curing glue.
[0023] For example, when the width of the bonding area is uniform, a left end area, a middle area and a right end area can be arranged in sequence along the length direction of the bonding area, the first glue is applied to the left and right end areas, and the second glue is applied to the middle area; wherein the area areas of the left end area and the right end area can be consistent, that is, the length dimensions of the left and right end areas along the length direction of the bonding area can be consistent.
[0024] When the total length of the bonding area is 120 mm, the length of the left end area may be 40 mm, the length of the middle area may be 40 mm, and the length of the right end area may be 40 mm.
[0025] When the total length of the bonding area is 120 mm, the length of the left end area may be 17.15 mm, the length of the middle area may be 85.7 mm, and the length of the right end area may be 17.15 mm.
[0026] When the total length of the bonding area is 120 mm, the length of the left end area may be 54.5 mm, the length of the middle area may be 11 mm, and the length of the right end area may be 54.5 mm.
[0027] It should be noted that, in actual application, the coating amount of the first glue and the second glue as bonding glue also directly affects the subsequent installation effect of the glass accessory. Therefore, in actual application, according to actual needs, the coating thickness of the first glue and the second glue can be controlled to be 0.2-1.2 mm. Specifically, the coating thickness of the first glue and the second glue is 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, etc. Most preferably, the coating thickness can be controlled to be 0.6 mm.
[0028] Accordingly, the glass accessory after the surface treatment according to the present invention can be installed together with the glass by the following accessory installation method, which includes the steps of:
[0029] The glass accessory treated by any one of the surface treatment methods described above in the present invention is placed on a positioning workpiece; the bonding area of the glass is wiped, and a glass cleaner is applied to the bonding area of the glass, and then dried; a glass primer is applied to the bonding area of the glass, and after the glass primer is dried, the glass is placed on the positioning workpiece, so that the bonding area of the glass and the bonding area of the glass accessory are positioned and bonded to each other through the positioning workpiece.
[0030] It should be noted that, in the above-mentioned accessory installation method, in order to obtain a better installation effect, when wiping the bonding area of the above-mentioned glass, a felt may be used to wipe the bonding area of the glass in one direction.
[0031] The beneficial effects of the present invention are: a new surface treatment method for glass accessories is designed, the process flow is simple, and a new material surface treatment process is adopted, thereby effectively improving the bonding reliability of high glass fiber materials and glass, especially materials with a glass fiber ratio of more than 30%, which can ensure the stability of the production process and the strength after bonding meets the requirements.
[0032] Accordingly, in actual application, in order to obtain better bonding effect, the bonding area of the glass can also be surface treated so that the above-mentioned high-glass fiber glass accessories can be better bonded to the glass, thereby improving the product effect obtained by bonding the high-glass fiber glass accessories and the glass together. It is easy to implement and has good promotion prospects and application value.
[0033] The present invention aims to solve the problem of bonding reliability between high-fiberglass materials and glass, especially materials with a glass fiber content of more than 30%, to ensure a stable production process and that the strength after bonding meets the requirements, and adopts a new material surface treatment process and a combined bonding glue. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The present invention is a flow chart of surface treatment of a glass accessory according to one embodiment of the present invention.
[0035] Figure 2 The flowchart schematically shows the process steps for installing the glass accessories and glass obtained based on the surface treatment method of the present invention. DETAILED DESCRIPTION
[0036] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0037] like Figure 1 As shown, in the present invention, in order to solve the problem of poor bonding reliability between glass accessories made of existing high glass fiber materials (glass fiber content>30%) and glass, the present invention provides a surface treatment method for glass accessories, which is used for glass accessories with glass fiber content>30%. The surface treatment method includes Figure 1 Steps S1-S4 shown: S1: Clean the bonding area of the glass accessory; S2: Plasma treat the bonding area of the glass accessory; S3: Apply accessory cleaner to the bonding area of the glass accessory, and then dry; S4: Evenly apply accessory primer to the bonding area of the glass accessory, and then dry.
[0038] In the above step S1, the bonding area of the glass attachment may be immersed in an isopropyl alcohol solution, and the subsequent steps S2-S4 may be performed after drying.
[0039] It should be noted that when the surface treatment method is actually applied to the surface treatment of glass accessories and the subsequent matching installation with glass, please refer to Figure 2 The process flow shown is:
[0040] Apply glue to the bonding area of the glass accessory after surface treatment, and then place the glass accessory on the positioning workpiece; at this time, you can select the glass and wipe the bonding area of the glass, apply glass cleaner on the bonding area of the glass, and then dry the glass; after the glass is dried, apply glass primer on the bonding area of the glass, and after the glass primer is dry, place the glass on the positioning workpiece, so that the bonding area of the glass and the bonding area of the glass accessory are positioned and bonded to each other through the positioning workpiece.
[0041] Accordingly, in order to facilitate understanding of the surface treatment method of the glass accessory designed by the present invention and to prove that the surface treatment method can improve the bonding reliability between the glass accessory made of high glass fiber material (glass fiber ratio > 30%) and glass, the present invention also provides the following embodiments 1-6 and comparative examples 1-6.
[0042] Examples 1-6 and Comparative Examples 1-6:
[0043] The attachment installation method of the finished bonding product of Examples 1-6 specifically includes the following steps:
[0044] (1) Surface treatment of glass accessories: The glass accessories are selected as sliders or guide rails, and the bonding area of the glass accessories is soaked with isopropyl alcohol, which is then taken out and air-dried; after drying, the bonding area of the glass accessories is plasma treated, and then an accessory cleaner is applied to the bonding area of the glass accessories, which is then blown dry or air-dried. After the surface of the bonding area of the glass accessories is dry, an accessory primer is applied, and the accessory primer is dried or air-dried. After the surface of the bonding area of the glass accessories is dry, glue is applied.
[0045] (2) Surface treatment of the glass: wiping the bonding area of the glass, applying a glass cleaner on the bonding area of the glass, and then drying; applying a glass primer on the bonding area of the glass, and then drying.
[0046] (3) Installing the glass accessory with the glass: placing the glass accessory treated by the surface treatment method in step (1) above into the positioning groove of the positioning workpiece, with the bonding surface facing upward; placing the glass treated by the surface treatment method in step (2) above on the positioning workpiece, so as to align and position the bonding area of the glass with the bonding area of the glass accessory through the positioning workpiece, and bond and fix them to each other.
[0047] It should be noted that the accessory installation method of the present invention adopts a newly designed surface treatment method to perform surface treatment on glass accessories, which is suitable for bonding glass accessories such as sliders or guide rails containing glass fiber to glass, especially glass accessories with a glass fiber content of >30%.
[0048] In the above step (1), the isopropyl alcohol content in the isopropyl alcohol solution is greater than 99.6%, and the bonding area of the glass attachment needs to be completely immersed in the liquid. After soaking for 10-50 minutes, it is picked up and dried, or blown dry with a fan, or wiped dry with gauze or dust-free paper before entering the next process.
[0049] Accordingly, in the above step (1), the glass accessory treated with isopropyl alcohol is subjected to plasma treatment of the bonding area of the glass accessory. The plasma treatment uses a wide jet or small jet low-temperature plasma device. The compressed air used in the plasma treatment needs to be filtered and dried. The compressed air used in the plasma treatment is filtered and dried; wherein the oil content of the compressed air after the filtration and drying treatment is less than 0.05 mg / m 3 , dust particle size <0.05μm, no moisture, flow rate is 60-100L / min, plasma treatment speed of the bonding area of the glass accessories is 1-3cm / s, the glass accessories after plasma treatment enter the next process within 1 hour, preferably within 1 minute after treatment.
[0050] In the above step (1), after the plasma treatment, the glass accessories are cleaned with an accessory cleaner, in particular, an accessory cleaner containing ingredients such as 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine, and the mass percentage of 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine is less than 5%. The accessory cleaner is evenly coated once in one direction, and is applied by a robot and then purged with filtered and dried air; or manually coated and then dried, blown or wiped in one direction, and then the next step is entered within 1 hour, and preferably the next step can be entered within <5 minutes after the drying treatment.
[0051] At the same time, after the accessory cleaner is dry, use the accessory primer to evenly apply it on the bonding area of the glass accessories. The selected accessory primer contains ingredients such as ethyl acetate, diisocyanate, n-butyl acetate and polyisocyanate. It needs to be fully shaken before use to ensure that there is no precipitation before applying. The accessory primer after opening must be used and packaged within 72 hours, and the subpackaged must be used within 8 hours. The coating is automatically applied by a robot, or manually applied and then dried before entering the next process; the primer needs to be dried or baked after application, and the reference standard is that no primer marks are left when pressed with white paper.
[0052] Furthermore, after the primer of the accessory is dry, glue is applied to the bonding area of the glass accessory. The glue uses two glues with different ingredients, namely a first glue and a second glue. Among them, the first glue is specifically selected as polyurethane glue or PU glue, such as HV3 glue; the second glue is specifically selected as a two-component fast-curing glue, such as 7990A / B mixed fast-drying glue.
[0053] In actual application, the first glue is applied to the left and right end areas of the bonding area of the glass accessory, and the second glue is applied to the middle area of the bonding area of the glass accessory, and the coating thickness of the first glue and the second glue is controlled to be 0.2-1.2 mm, and most preferably can be controlled to be 0.6 mm; wherein the area ratio of at least one end area of the left and right end areas to the middle area is 0.2-5.
[0054] Correspondingly, in the above step (2), when the glass is surface treated, the bonding area of the glass is wiped with a felt, and the felt is wiped in one direction; wherein, the glass after the felt is wiped is coated on the bonding area of the glass with a glass cleaner. Preferably, the glass cleaner contains 3-(trimethoxysilyl)-1-propanethiol, N-[3-(trimethoxysilyl)propyl]ethylenediamine and isopropanol, and the mass percentage content of 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine is less than 5%, the mass percentage content of isopropanol is ≥90%, and less than 100%, the cleaner is uniformly coated once in one direction, and after coating with a robot, it is purged with filtered and dried air; or after manual coating, it is dried, blown or wiped in one direction, and then enters the next process within 1 hour, preferably, it can enter the next process within <5 minutes after treatment.
[0055] It should be noted that the glass cleaner may also be a conventional commercially available cleaner, such as Dow VP04604.
[0056] After the glass cleaner is dried, a glass primer is applied. The selected glass primer contains trimethoxysilane, 3-methoxybutyl acetate and butanone, and the mass percentage content of trimethoxysilane is 1-5%, the mass percentage content of 3-methoxybutyl acetate is 5-10%, and the mass percentage content of butanone is ≥50% and <100%. The glass primer needs to be fully shaken before use to ensure that there is no precipitation before coating. The opened glass primer needs to be used and packaged within 72 hours, and the subpackaged needs to be used within 8 hours. The coating is automatically applied by a robot, and after drying in an oven, or after manual coating and drying, step (3) is entered.
[0057] It should be noted that the glass primer may also be a conventional primer available on the market, such as Dow Betaprime 5404.
[0058] In the above step (3), the glass accessory is placed into the positioning groove of the positioning workpiece after being coated with glue. The process from coating the glue to installing the bonded glass needs to be completed within 3 minutes, and preferably the installation can be completed within 90 seconds after coating the glue.
[0059] Different from the preparation process of the bonding product between the glass attachment and the glass in the above-mentioned embodiments 1-6, the inventor also lists comparative examples 1-6 as a control group. The surface treatment process of the glass attachment in comparative examples 1-6 is: first, the bonding surface of the glass attachment such as the guide rail or the slider is cleaned with an isopropyl alcohol solution, and then plasma treated, and then the primer is coated with M300 conventional primer, and then glue is applied after drying. This method is well known in the art and will not be described in detail. The surface treatment process of the glass in comparative examples 1-6 is: wipe the bonding area of the glass, and apply a glass cleaner (such as Dow VP04604) on the bonding area of the glass, and then dry it; apply a glass primer (such as Dow Betaprime5404) on the bonding area of the glass, and then dry it. This method is well known in the art and will not be described in detail.
[0060] Accordingly, further experimental tests were conducted on the bonding products between the glass attachment and the glass of Examples 1-6 and the bonding products between the glass attachment and the glass of Comparative Examples 1-6 to verify the performance differences:
[0061] Tensile test: The finished adhesive products of Examples 1-6 obtained by adopting the present technical solution and the comparative adhesive products of Comparative Examples 1-6 are subjected to a tensile test. The glass is fixed on a tensile testing machine, the adhesive products are fixed by a clamp, the tensile testing machine is started, and the readings are taken after the glass is broken or the slider falls off. The test results indicate the ultimate adhesive force of the adhesive material. If the glass is broken, it means that the ultimate adhesive force is greater than the glass strength.
[0062] During the tensile test, after the adhesive is cured, the temperature is controlled to be at room temperature, the tensile data is controlled, and the states of the slider and the glass of each embodiment and comparative example are observed. The test results are shown in Table 1 below.
[0063] Table 1 lists the tensile test parameters and tensile test results of the finished bonding products of Examples 1-6 and the comparative bonding products of Comparative Examples 1-6.
[0064] Table 1.
[0065]
[0066] It is not difficult to see from the above Table 1 that the comparative bonding products of Comparative Examples 1-6 prepared by the traditional surface treatment method will debond when subjected to an external tensile force of 406-522N, and the bonding state will be destroyed, thereby separating the slider from the glass;
[0067] The finished adhesive products of Examples 1-6 prepared by the surface treatment method designed by the present invention will not debond when subjected to an external tensile force of 1216-1363N, and the bonding effect is very good. The final damage effect is only the breakage of the slider or the shattering of the glass, and there is no problem of debonding and separation of the slider and the glass. This shows that the surface treatment method for glass accessories designed by the present invention can enhance the bonding reliability of high-glass fiber glass accessories and glass.
[0068] From the above, it can be seen that the surface treatment method of glass accessories designed by the present invention can solve the problem of poor bonding reliability between existing glass accessories made of high glass fiber materials (fiber ratio exceeds 30%) and glass. It can make the above-mentioned high glass fiber glass accessories better bonded to the glass, and improve the product effect of the product obtained by bonding the high glass fiber glass accessories to the glass. Its process route is mature and easy to implement, and it has good promotion prospects and application value.
[0069] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A surface treatment method for a glass accessory, characterized in that: The glass fiber content of the glass accessory is greater than 30%, and the surface treatment method of the glass accessory The following steps are involved: S1: cleaning the bonding area of the glass attachment; S2: plasma treatment of the bonding area of the glass attachment; S3: applying an accessory cleaner to the bonding area of the glass accessory, and then drying; S4: evenly applying an accessory primer to the bonding area of the glass accessory, and then drying.
2. The surface treatment method according to claim 1, characterized in that: In step S1, the bonding area of the glass accessory is soaked in an isopropanol solution for 10-50 minutes and then dried.
3. The surface treatment method according to claim 1, characterized in that: In step S2, the compressed air used for plasma treatment is filtered and dried; wherein the oil content of the compressed air after filtering and drying is less than 0.05 mg / m 3 , dust particle size <0.05μm, no moisture, flow rate is 60-100L / min, and the plasma treatment speed of the bonding area of the glass accessories is 1-3cm / s.
4. The surface treatment method according to claim 1, characterized in that: In step S2, the surface energy of the bonding area of the glass attachment after the plasma treatment is ≥40 mN / m.
5. The surface treatment method according to claim 1, characterized in that: In step S3, the accessory cleaning agent contains 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine.
6. The surface treatment method according to claim 5, characterized in that: In step S3, the mass percentage contents of 3-(trimethoxysilyl)-1-propanethiol and N-[3-(trimethoxysilyl)propyl]ethylenediamine in the accessory cleaning agent are both less than 5%.
7. The surface treatment method according to claim 1, characterized in that: In step S4, the accessory primer contains: ethyl acetate, diisocyanate, n-butyl acetate and polyisocyanate.
8. The surface treatment method according to claim 1, characterized in that: The method further comprises step S5: applying glue to the bonding area of the glass attachment.
9. The surface treatment method according to claim 8, characterized in that: In step S5, the glue includes a first glue and a second glue, the first glue is applied to the left and right end areas of the bonding area of the glass attachment, and the second glue is applied to the middle area of the bonding area of the glass attachment; wherein the area ratio of at least one of the left and right end areas to the middle area is 0.2 to 5.