Concrete early-strength high-efficiency water reducing agent and preparation method thereof

By preparing a high-efficiency water-reducing agent for concrete that combines polyether macromonomers with fly ash-carbide slag composite powder, the problem of dosage sensitivity of polycarboxylate water-reducing agents was solved, improving the fluidity and early strength of concrete, as well as its durability and workability.

CN119038895AInactive Publication Date: 2024-11-29XIAMEN HONGFA XIANKE NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162642.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polycarboxylate superplasticizers are sensitive to dosage and water usage, which can easily cause concrete segregation, bleeding, poor system stability, and affect workability and durability.

Method used

A high-efficiency water-reducing agent for concrete is prepared by using polyether macromonomers, acrylic acid, acrylamide, sodium methacrylate sulfonate, chain transfer agent, redox agent, 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, and fly ash-carbide slag composite powder, and through high-temperature activation and alkali activation treatment, forming a stable copolymer structure with higher strength.

Benefits of technology

It significantly improves the fluidity and early strength of concrete, reduces slump loss, improves appearance quality, enhances durability, and reduces the risk of bleeding and cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006876070000111
    Figure BDA0005006876070000111
  • Figure BDA0005006876070000121
    Figure BDA0005006876070000121
Patent Text Reader

Abstract

The invention relates to a concrete early-strength high-efficiency water reducing agent and a preparation method thereof. The concrete early-strength high-efficiency water reducing agent is prepared from a polyether macromonomer, acrylic acid, acrylamide, sodium methallyl sulfonate, a chain transfer agent, a redox agent, 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, fly ash-carbide slag composite powder and deionized water. Wherein the polyether macromonomer is composed of a compound of allyl polyglycol ether and alkylphenol polyglycol ether. According to the scheme provided by the invention, the slump loss problem of the current polycarboxylate superplasticizer can be improved and relieved under the condition that the doping amount is relatively low, and the failure of adsorption and dispersion effects is improved; meanwhile, the strength of the concrete can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of concrete admixtures, and in particular to a concrete early-strengthening high-efficiency water reducing agent and a preparation method thereof. Background Art

[0002] Chemical admixtures play an important role in modern Portland cement concrete materials and technologies, and are the fifth essential component of concrete. Among them, water reducers are the most widely used and largest amount of chemical admixtures. The most important technical approach to achieve the highest performance of concrete is to use high-quality and high-efficiency water reducers.

[0003] Traditional wood sulfonate water reducers have a low water reduction rate. Although naphthalene water reducers can make fresh mortar and concrete have better workability, they cannot have a higher water reduction rate and have a large slump loss. In order to reduce the slump loss of concrete, it is currently mainly achieved by compounding retarders and changing the method of adding water reducers. As a new generation of concrete admixtures, polycarboxylic acid-based high-efficiency water reducers have outstanding advantages such as low dosage, high water reduction rate, and good slump retention. They give concrete excellent workability and durability and have been widely accepted in the concrete industry recently. However, polycarboxylic acid-based water reducers are highly sensitive to dosage and water consumption, which can easily cause problems such as concrete segregation, water bleeding, and poor system stability, which also affects the workability and durability of concrete. Summary of the invention

[0004] In order to solve or partially solve the problems existing in the related art, the present application provides a concrete early-strengthening high-efficiency water-reducing agent and a preparation method thereof, which can improve and alleviate the slump loss problem of the current polycarboxylic acid water-reducing agent at a low dosage and improve the failure of the adsorption and dispersion effect; at the same time, it can also improve the strength of concrete.

[0005] The first aspect of the present application provides a concrete early strength high efficiency water reducing agent, which is made of polyether macromonomer, acrylic acid, acrylamide, sodium methacrylate sulfonate, chain transfer agent, redox agent, 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, fly ash-carbide slag composite powder and deionized water;

[0006] The polyether macromonomer is composed of a complex of allyl polyethylene glycol ether and alkylphenol polyethylene glycol ether.

[0007] In some embodiments of the present application, the mass ratio of the allyl polyethylene glycol ether to the alkylphenol polyethylene glycol ether is (1-5):1.

[0008] In some embodiments of the present application, the chain transfer agent is one or more of thioglycolic acid, mercaptoethanol and sulfonated mercapto acid.

[0009] In some embodiments of the present application, the mass ratio of the polyether macromonomer to the fly ash-carbide slag composite powder is 1:(0.1-0.2).

[0010] In some embodiments of the present application, the mass ratio of the 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose to the fly ash-carbide slag composite powder is (1-5):1.

[0011] The second aspect of the present application provides a method for preparing a concrete early strength high efficiency water reducing agent, comprising:

[0012] (1) mixing a certain amount of fly ash and carbide slag to form a fly ash-carbide slag composite powder, and activating the fly ash and carbide slag composite powder to obtain an activated fly ash and carbide slag composite powder;

[0013] (2) dissolving the polyether macromonomer in deionized water, adding acrylic acid, acrylamide, and sodium methacrylic acid sulfonate under heating and stirring conditions, and simultaneously dropping a chain transfer agent and a redox agent to carry out a polymerization reaction;

[0014] (3) adding activated composite powder and 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, continuing heating and stirring, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0015] In some embodiments of the present application, the activation treatment of the fly ash-carbide slag composite powder in step (1) includes:

[0016] The fly ash-carbide slag composite powder is activated at a high temperature of 280-400°C;

[0017] The fly ash-carbide slag composite powder after high temperature activation is alkali activated in a 2 mol / L sodium hydroxide solution, washed, separated and dried to obtain the activated fly ash and carbide slag composite powder.

[0018] In some embodiments of the present application, the heating and stirring temperature of step (2) and step (3) is 40-45°C.

[0019] The third aspect of the present application provides a use of the water reducer as described in the first aspect of the present application or the water reducer prepared by the water reducer preparation method as described in the second aspect of the present application in preparing concrete.

[0020] In some embodiments of the present application, the dosage of the water reducing agent is 0.15-0.22%.

[0021] The technical solution provided by the present application may include the following beneficial effects: on the one hand, the working performance of the concrete mixture can be maintained, and the fluidity and slump of the concrete mixture can be significantly improved; on the other hand, the problems of large shrinkage and high viscosity of the concrete can be solved, which is beneficial to the discharge of bubbles inside the concrete mixture and on the surface of the formwork, thereby improving the apparent quality of the concrete; at the same time, the water reducer having a fly ash-carbide slag composite powder can also delay the setting time of the concrete, thereby reducing the slump loss and the generation of cracks, and can act as a filler to form a more stable and higher-strength copolymer structure, and can also act as a filler in concrete production, thereby improving the problem of bubbles generated in the concrete, preventing internal tiny bubbles from affecting the strength of the concrete after the concrete solidifies, and improving the early strength of the concrete, while having good durability.

[0022] Furthermore, the present application uses 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose and fly ash-carbide slag composite powders to be cross-linked in the polycarboxylate water-reducing agent base liquid, which can accelerate the cement hydration reaction while making the concrete have good fluidity and better adapt to different types of cement, thereby improving its application scenarios.

[0023] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION

[0024] To make the present invention easy to understand, the present invention will be described in detail below. However, before describing the present invention in detail, it should be understood that the present invention is not limited to the specific embodiments described. It should also be understood that the terms used herein are only for describing specific embodiments and are not intended to be limiting.

[0025] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0026] Where a numerical range is provided, it is to be understood that each intermediate value between the upper and lower limits of the range and any other provisions or intermediate values ​​in the specified range is encompassed within the present invention. The upper and lower limits of these smaller ranges may be independently included in the smaller ranges and are also encompassed within the present invention, subject to any explicitly excluded limits in the specified range. Where a specified range includes one or two limits, the scope excluding any or both of those included limits is also encompassed within the present invention. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically limited.

[0027] Unless otherwise defined, all terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although any methods and materials or equivalent methods and materials described herein can also be used in the practice or testing of the present invention, preferred methods and materials are now described.

[0028] Traditional wood sulfonate water reducers have a low water reduction rate. Although naphthalene water reducers can make fresh mortar and concrete have better workability, they cannot have a higher water reduction rate and have a large slump loss. In order to reduce the slump loss of concrete, it is currently mainly achieved by compounding retarders and changing the method of adding water reducers. As a new generation of concrete admixtures, polycarboxylic acid-based high-efficiency water reducers have outstanding advantages such as low dosage, high water reduction rate, and good slump retention. They give concrete excellent workability and durability and have been widely accepted in the concrete industry recently. However, polycarboxylic acid-based water reducers are highly sensitive to dosage and water consumption, which can easily cause problems such as concrete segregation, water bleeding, and poor system stability, which also affects the workability and durability of concrete.

[0029] In view of the above problems, the embodiments of the present application provide a concrete early strength high efficiency water reducing agent, which can improve and alleviate the slump loss problem of the current polycarboxylate water reducing agent at a low dosage, improve the failure of the adsorption and dispersion effect; and at the same time, can also improve the strength of concrete.

[0030] The concrete early strength high-efficiency water reducing agent of the embodiment of the present application is made of polyether macromonomer, acrylic acid, acrylamide, sodium methacrylate sulfonate, chain transfer agent, redox agent, 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, fly ash-carbide slag composite powder and deionized water; wherein the polyether macromonomer is composed of a complex of allyl polyethylene glycol ether and alkylphenol polyethylene glycol ether.

[0031] The water-reducing agent of the embodiment of the present application can, on the one hand, maintain the working performance of the concrete mixture and significantly improve the fluidity and slump of the concrete mixture; on the other hand, it can solve the problems of large shrinkage and high viscosity of concrete, and is conducive to the discharge of bubbles inside the concrete mixture and on the surface of the formwork, thereby improving the apparent quality of the concrete; at the same time, the water-reducing agent having a fly ash-carbide slag composite powder can also play a role in delaying the setting time of concrete, thereby reducing the slump loss and the generation of cracks, and can play the role of a filler to form a more stable and higher-strength copolymer structure, and can also play the role of a filler in concrete production, thereby improving the bubble problem generated in the concrete, preventing the internal tiny bubbles from affecting the strength of the concrete after the concrete solidifies, and improving the early strength of the concrete, while having good durability.

[0032] In some specific embodiments, the mass ratio of the polyether macromonomer allyl polyethylene glycol ether to the alkylphenol polyglycol ether is (1-5): 1, for example 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, or any value within the above range; preferably 2: 1. By combining the polyether macromonomer within the above suitable range with acrylic acid, ammonium acrylate, and sodium methacrylic acid sulfonate, it is helpful to form a copolymer product with a higher degree of crosslinking and a more complex copolymer after the copolymerization reaction, thereby obtaining a polycarboxylate water reducer that can significantly improve the fluidity of the concrete mixture.

[0033] In some specific embodiments, the mass ratio of the polyether macromonomer to the small monomer is 1:(3-5); preferably 1:4; wherein the small monomer includes acrylic acid, acrylamide and sodium methacrylic acid. Further, the mass ratio of acrylic acid, acrylamide and sodium methacrylic acid is 2:1:1. The composite small monomer system formed by acrylic acid, acrylamide and sodium methacrylic acid can not only increase the main chain length of the polycarboxylic acid by polymerization reaction with the polyether macromonomer, but also enable the water reducer to have side chain groups containing N and S elements, so as to be more conducive to its role as a water reducer in cement mortar and concrete slurry, improve the fluidity and slump of concrete, and also enable it to have a more complex cross-linking structure, so that the water reducer has good early strength function, which is conducive to its adaptation to different cement varieties; and it can exert better water reducer performance and early strength agent performance with less admixture. Further, the polycarboxylic acid-based water reducer base liquid formed by the polymerization of macromonomers and small monomers under appropriate conditions has a better water reduction improvement effect on concrete.

[0034] In some specific embodiments, the chain transfer agent can be selected from one or more of thioglycolic acid, mercaptoethanol and sulfonated mercapto acid; preferably, a complex of thioglycolic acid and sulfonated mercapto acid; more preferably, thioglycolic acid and sulfonated mercapto acid in a mass ratio of 3:1. The synthesis of the polycarboxylate water reducer by the above chain transfer agent is conducive to improving the conversion rate of the polymerization reaction.

[0035] In some specific embodiments, the amount of chain transfer agent is 1-3wt% of the polyether macromonomer, specifically 1wt%, 2wt%, 3wt%, etc., or any value within the above range. The above amount of chain transfer agent not only helps to improve the conversion rate of the polymerization reaction, but also can increase the molecular weight of the polycarboxylate water reducer, not only can improve the dispersion effect in the initial stage of concrete production, ensure that the concrete has good pumping performance, but also has a strong retention capacity, can better maintain the flow properties of the concrete slurry, and can maintain the strength of the concrete and improve its compressive strength.

[0036] In some specific embodiments, the redox agent is a mixture of 5 mol / L hydrogen peroxide and 3 mol / L ascorbic acid solution, and the volume ratio of hydrogen peroxide solution to ascorbic acid solution is 1: 5. Further, the redox agent is 1-5 wt% of the polyether macromonomer, specifically 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, etc., or any value within the above range.

[0037] In some specific embodiments, the mass ratio of the polyether macromonomer to the fly ash-carbide slag composite powder is 1:(0.1-0.2), specifically 1:0.1, 1:0.15, 1:0.2, etc., or any value within the above range. By adjusting the addition amount of the polyether macromonomer and the fly ash-carbide slag composite powder, the polyether macromonomer can be further cross-linked with the fly ash-carbide slag composite powder after copolymerization to form a polycarboxylate water-reducing agent base liquid, thereby enhancing the strength of the cement particle solidification network and improving the early strength of the concrete. At the same time, it can also coordinate the establishment and cross-linking of the three-dimensional silicate network inside the cement, reduce the slump loss, and improve the compressive strength of the concrete.

[0038] In some specific embodiments, the mass ratio of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose and fly ash-carbide slag composite powder is (1-5): 1, specifically 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, etc., or any value within the above range. By coordinating the amount of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose and fly ash-carbide slag composite powder, on the one hand, the fly ash-carbide slag composite powder can be better cross-linked and composited with the polycarboxylate water-reducing agent base liquid as an early strength agent, significantly improving the early strength of the concrete, and at the same time, it can have a better filling effect, forming a more dense and stable, higher strength concrete internal network cross-linked structure, and at the same time, it can better solve the influence of bubbles inside the concrete on the strength and apparent quality of the concrete, improve the surface smoothness of the concrete, and reduce surface pores.

[0039] In some embodiments, the fly ash-carbide slag composite powder has a mass ratio of fly ash to carbide slag of (1-3): (1-3); preferably 1: 1. The fly ash and carbide slag composite powder has higher calcium, aluminum and silicon contents in its components, so that after being mixed with cement and water, it can quickly react chemically with the components in cement particles, promote the hydration reaction of cement, generate complexes, reduce the surface tension of concrete slurry, and improve the early strength and density of concrete.

[0040] The preparation method of the concrete early strength high efficiency water reducing agent of the embodiment of the present application comprises the following steps:

[0041] (1) mixing a certain amount of fly ash and carbide slag to form a fly ash-carbide slag composite powder, and activating the fly ash and carbide slag composite powder to obtain an activated fly ash and carbide slag composite powder;

[0042] (2) dissolving the polyether macromonomer in deionized water, adding acrylic acid, acrylamide, and sodium methacrylic acid sulfonate under heating and stirring conditions, and simultaneously dropping a chain transfer agent and a redox agent to carry out a polymerization reaction;

[0043] (3) adding activated composite powder and 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, continuing heating and stirring, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0044] The water reducing agent of the present application, the activation treatment of the fly ash-carbide slag composite powder in step (1) comprises:

[0045] The fly ash-carbide slag composite powder is activated at a high temperature of 280-400°C;

[0046] The fly ash-carbide slag composite powder after high temperature activation is alkali activated in a 2 mol / L sodium hydroxide solution, washed, separated and dried to obtain the activated fly ash and carbide slag composite powder.

[0047] The fly ash-carbide slag composite powder after high-temperature activation and alkali activation can be mixed with the polycarboxylate water-reducing agent base liquid, and then, under the action of the redox initiator, it can better undergo a grafting reaction with 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose and the polycarboxylate water-reducing agent base liquid to obtain a concrete early-strength high-efficiency water-reducing agent with better mechanical properties, which is beneficial to improving the early strength and durability of concrete.

[0048] The high temperature activation time can be 30 min-1 h; the alkali activation time can be 2 h-3 h.

[0049] The polymerization reaction of the polyether macromonomer in step (2) is carried out at 40-45° C.; the temperature of the grafting reaction in step (3) is 40-45° C.; the redox agent added in step (2) can also serve as an initiator for the grafting reaction in step (3), and acrylic acid, acrylamide and sodium methyl methacrylate sulfonate that do not participate in the polymerization reaction can also further participate in the reaction of step (3), so that the concrete early strength high-efficiency water reducing agent obtained after cross-linking and grafting has a higher structural complexity and a better cross-linking effect, which is beneficial to improving the early strength of concrete and can also reduce the water bleeding rate and cracking of concrete.

[0050] The concrete early strength high-efficiency water reducing agent prepared according to the above method can be used in the preparation of concrete, and its dosage is 0.15-0.22%, for example, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, etc., or any value within the above range.

[0051] The present application adopts the above-mentioned water reducing agent, which can accelerate the cement hydration reaction while making the concrete have good fluidity, better adapt to different types of cement, improve the early strength and construction performance of concrete, and can improve the stability and durability of concrete, reduce the incidence of problems such as water seepage and cracking of concrete, and achieve good collapse protection performance.

[0052] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.

[0053] Example 1

[0054] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0055] (1) 0.25 kg of fly ash and 0.25 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0056] (2) 5 kg of allyl polyethylene glycol ether and 5 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, and 20 kg of acrylic acid, 10 kg of acrylamide, and 10 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.1 kg of thioglycolic acid and 0.3 kg of a redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0057] (3) Adding activated composite powder and 0.5 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0058] Example 2

[0059] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0060] (1) 0.25 kg of fly ash and 0.25 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0061] (2) 8.3 kg of allyl polyethylene glycol ether and 1.7 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, 20 kg of acrylic acid, 10 kg of acrylamide, and 10 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.1 kg of thioglycolic acid and 0.3 kg of a redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0062] (3) Adding activated composite powder and 0.5 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0063] Example 3

[0064] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0065] (1) 0.25 kg of fly ash and 0.25 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0066] (2) 6.7 kg of allyl polyethylene glycol ether and 3.3 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, 20 kg of acrylic acid, 10 kg of acrylamide, and 10 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.1 kg of thioglycolic acid and 0.3 kg of a redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0067] (3) Adding activated composite powder and 0.5 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0068] Example 4

[0069] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0070] (1) 0.25 kg of fly ash and 0.25 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0071] (2) 6.7 kg of allyl polyethylene glycol ether and 3.3 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, 4 kg of acrylic acid, 3 kg of acrylamide, and 3 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.1 kg of thioglycolic acid and 0.3 kg of redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0072] (3) Adding activated composite powder and 0.5 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0073] Example 5

[0074] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0075] (1) 0.25 kg of fly ash and 0.25 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0076] (2) 6.7 kg of allyl polyethylene glycol ether and 3.3 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, and 20 kg of acrylic acid, 10 kg of acrylamide, and 10 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.1 kg of thioglycolic acid, 0.1 kg of sulfonated mercapto acid, and 0.3 kg of a redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0077] (3) Adding activated composite powder and 0.5 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0078] Example 6

[0079] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0080] (1) 0.25 kg of fly ash and 0.25 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0081] (2) 6.7 kg of allyl polyethylene glycol ether and 3.3 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, and 20 kg of acrylic acid, 10 kg of acrylamide, and 10 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.3 kg of thioglycolic acid, 0.1 kg of sulfonated thioglycolic acid, and 0.3 kg of a redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0082] (3) Adding activated composite powder and 0.5 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0083] Example 7

[0084] A concrete early strength high efficiency water reducing agent comprises the following preparation steps:

[0085] (1) 0.35 kg of fly ash and 0.65 kg of carbide slag are mixed to form a fly ash-carbide slag composite powder, and the fly ash-carbide slag composite powder is activated to obtain an activated fly ash and carbide slag composite powder;

[0086] (2) 6.7 kg of allyl polyethylene glycol ether and 3.3 kg of alkylphenol polyethylene glycol ether polyether macromonomer were dissolved in 10 L of deionized water, 20 kg of acrylic acid, 10 kg of acrylamide, and 10 kg of sodium methyl propylene sulfonate were added under stirring at 45° C., and 0.1 kg of thioglycolic acid and 0.3 kg of a redox agent were added dropwise to carry out polymerization reaction for 3 hours;

[0087] (3) Adding activated composite powder and 1.2 kg of 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, heating and stirring are continued, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

[0088] Comparative Example 1

[0089] The difference from Example 1 is that the polyether macromonomer in step (2) is 10 kg of allyl polyethylene glycol ether.

[0090] Comparative Example 2

[0091] The difference from Example 1 is that the small monomer in step (2) is 20 kg of acrylic acid.

[0092] Comparative Example 3

[0093] The difference from Example 1 is that 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose is not added in step (3).

[0094] Comparative Example 4

[0095] The difference from Example 1 is that in step (2), after the polymerization reaction, the pH is adjusted to neutral with alkali solution to obtain a concrete early strength high efficiency water reducing agent.

[0096] Comparative Example 5

[0097] The difference from Example 1 is that in step (1), only 0.5 kg of fly ash is used, and no calcium carbide slag powder is added.

[0098] The water reducing agents prepared in the above-mentioned embodiments and comparative examples were applied to the evaluation of cement paste fluidity, cement mortar performance and concrete performance.

[0099] The ingredients of the cement paste are: water-cement ratio 0.32, 5 kg of silicate cement, and the prepared water reducer is added to the cement paste in an amount of 0.18% of the cement material.

[0100] The ingredients of cement mortar are: water-cement ratio 0.48, 5kg of silicate cement, 10kg of standard sand, and the prepared water reducing agent is added to the cement mortar according to the dosage of 0.18% of the cement material.

[0101] The pipe pile adopts C60 concrete formula (1L): water-cement ratio 0.42, 5kg of Portland cement, 9.8kg of sand, 10.3kg of gravel, and the prepared water reducer is added to the concrete formula according to the dosage of 0.18% of the cement material.

[0102] The evaluation results are recorded in Table 1.

[0103] Table 1

[0104]

[0105]

[0106] According to the comparison of the embodiment and the comparative example, the water reducer produced by the formula and preparation method of the embodiment of the present application has good comb-like molecular structure characteristics, good dispersibility for cement, and excellent water reduction, slump retention, plasticization, reinforcement and low shrinkage performance when used in concrete. The water reducer described in the embodiment of the present application has a small blending ratio in the cement material, and can exert good water reduction and reinforcement performance at a small blending ratio; the reason may be that when it is mixed with the cement material, the cement particles and multiple molecules in the water reducer act on each other, and can exert its water reduction performance without affecting the cement hydration process, shorten the coagulation and hardening time of cement slurry and concrete, and improve the early strength of cement slurry and concrete, while not affecting the late strength of concrete.

[0107] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A concrete early strength high efficiency water reducing agent, characterized in that: It is made of polyether macromonomer, acrylic acid, acrylamide, sodium methyl propylene sulfonate, chain transfer agent, redox agent, 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, fly ash-carbide slag composite powder and deionized water; The polyether macromonomer is composed of a complex of allyl polyethylene glycol ether and alkylphenol polyethylene glycol ether.

2. The water reducing agent according to claim 1, characterized in that: The mass ratio of the allyl polyglycol ether to the alkylphenol polyglycol ether is (1-5):

1.

3. The water reducing agent according to claim 1, characterized in that: The chain transfer agent is one or more of thioglycolic acid, mercaptoethanol and sulfonated mercapto acid.

4. The water reducing agent according to claim 1, characterized in that: The mass ratio of the polyether macromonomer to the fly ash-carbide slag composite powder is 1:(0.1-0.2).

5. The water reducing agent according to claim 1, characterized in that: The mass ratio of the 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose to the fly ash-carbide slag composite powder is (1-5):

1.

6. A method for preparing a concrete early strength high efficiency water reducing agent, characterized in that: include: (1) mixing a certain amount of fly ash and carbide slag to form a fly ash-carbide slag composite powder, and activating the fly ash and carbide slag composite powder to obtain an activated fly ash and carbide slag composite powder; (2) dissolving the polyether macromonomer in deionized water, adding acrylic acid, acrylamide, and sodium methacrylic acid sulfonate under heating and stirring conditions, and simultaneously dropping a chain transfer agent and a redox agent to carry out a polymerization reaction; (3) adding activated composite powder and 2-hydroxyethyl-2-hydroxypropyl methyl ether cellulose, continuing heating and stirring, and then adjusting the pH to neutral with alkali solution to obtain a concrete early strength high-efficiency water reducing agent.

7. The method for preparing a water reducing agent according to claim 6, characterized in that: The activation treatment of the fly ash-carbide slag composite powder in step (1) includes: The fly ash-carbide slag composite powder is activated at a high temperature of 280-400°C; The fly ash-carbide slag composite powder after high temperature activation is alkali activated in a 2 mol / L sodium hydroxide solution, washed, separated and dried to obtain the activated fly ash and carbide slag composite powder.

8. The method for preparing a water reducing agent according to claim 6, characterized in that: The heating and stirring temperature in step (2) and step (3) is 40-45°C.

9. Use of the water reducing agent according to any one of claims 1 to 5 or the water reducing agent prepared by the method for preparing the water reducing agent according to any one of claims 6 to 8 in preparing concrete.

10. The use according to claim 9, characterized in that: The dosage of the water reducing agent is 0.15-0.22%.