Recycled concrete with self-repairing capability and preparation method thereof
By using Bacillus Pasteuris and Bacillus amyloid in concrete, the combination of calcium salt and sorbitol expansion agent, the problem of difficult self-repair of traditional concrete cracks is solved, and efficient self-repair effect and excellent resistance are achieved The permeability of chloride ion extends the service life of concrete.
Patent Information
- Application Number
- CN202411264662.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional concrete is prone to cracks due to external factors during long-term use, and existing self-repairing technologies rely on external repair agents, which are complex in operation and limited in effect.
The microbial repair agent composed of Bacillus Pasteuris suspension and Bacillus amylase solution is used to combine an expansion agent composed of calcium salt and sorbitol to promote self-repair of concrete cracks, and fill the cracks through the precipitation and expansion of calcium carbonate produced by bacteria. Restore the integrity and strength of concrete.
The independent repair ability of concrete is achieved, the resistance to chloride ion permeability and dry shrinkage value performance is improved, the compressive strength can be maintained for a long time, the aging resistance is good, the construction cycle is shortened and the engineering efficiency is improved.
Smart Images

Figure BDA0005036788250000041 
Figure BDA0005036788250000051 
Figure BDA0005036788250000061
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to a recycled concrete with self-repairing ability and a preparation method thereof. Background Art
[0002] At present, concrete is a widely used building material and is favored for its high strength and durability. However, traditional concrete is prone to cracks due to external factors (such as temperature changes, load effects, etc.) during long-term use, which in turn affects the overall performance and service life of the structure. To solve this problem, researchers are constantly exploring new concrete materials, one of which is self-repairing concrete. Existing self-repairing concrete technology mostly relies on the injection of external repair agents, which is complicated to operate and has limited effects. Therefore, the development of a concrete material that can autonomously repair cracks and its preparation method has important practical value and market demand. Summary of the invention
[0003] In order to solve the above technical problems, the present application provides a recycled concrete with self-repairing ability and a preparation method thereof.
[0004] In the first aspect, the present application provides a recycled concrete with self-repairing ability, characterized in that it specifically includes the following components in parts by weight: 1200-1300 parts of recycled aggregate, 900-1100 parts of cement, 700-800 parts of quartz sand, 100-140 parts of silica fume, 80-100 parts of fly ash, 5-10 parts of water reducer, 1.2-2.4 parts of microbial remediation agent, 20-28 parts of expansion agent, and 400-450 parts of water; The microbial repair agent is composed of a mixture of a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens bacterial solution in a weight ratio of 0.5-1.5:0.5-1.5; the concentration of the Bacillus pasteurianus suspension is 6-8×10 7 cell / mL, and the concentration of the Bacillus amyloliquefaciens culture solution is 1-3×10 7 cell / mL; The bulking agent consists of calcium salt and sorbitol in a weight ratio of 9:1-3.
[0005] By using the above technical solution provided by the present application, a microbial repair agent is formed by mixing a suspension of Bacillus pasteurianus and a suspension of Bacillus amyloliquefaciens at a weight ratio of 0.5-1.5:0.5-1.5, and an expansion agent is formed by using calcium salt and sorbitol, which can promote carbonate precipitation and promote the self-repair effect of concrete cracks. The recycled concrete prepared by the present application has excellent resistance to chloride ion penetration and shrinkage value. The compressive strength loss rate after aging for 720 hours at 80°C is less than 2.5%, indicating that it can maintain a high compressive strength for a long time and has a good aging resistance effect.
[0006] The present application aims to solve the problem that traditional concrete is prone to cracks and difficult to self-repair during long-term use, and to provide a recycled concrete with self-repairing ability and a preparation method thereof.
[0007] Through the above basic scheme, the self-repairing concrete prepared can trigger the self-repair mechanism when cracks appear, fill the cracks and restore the integrity and strength of the concrete through the action of microbial repair agents and special additives; the microbial repair agents are selected from bacteria that can produce mineralization, which can produce calcium carbonate precipitation in concrete cracks, thereby effectively filling the cracks. The calcium-based expansion agent with expansion properties and sorbitol can produce micro-expansion inside the concrete, further promoting the healing of cracks.
[0008] In the presence of microbial remediation agents, sorbitol can promote the reaction of free calcium in concrete to generate water-insoluble calcium salts, thereby increasing the bonding strength between concrete raw materials and reducing the strength loss of concrete. In addition, the synergistic effect of the raw materials in this application also has the effect of promoting the early strength development of concrete, which can shorten the construction period and improve engineering efficiency.
[0009] At the same time, the raw materials of the present application use a specific type of bacterial liquid to form a microbial remediation agent. After compounding with an expansion agent, the two can be mixed to form a dense curing film, which can block the capillary channels of the concrete slurry and isolate its surface from the air. Through the effects of embedding and interface barriers, the concrete material sample has a higher anti-permeability performance, and the recycled concrete has excellent resistance to chloride ion penetration.
[0010] Preferably, the recycled concrete with self-repairing ability specifically includes the following components in parts by weight: 1220-1280 parts of recycled aggregate, 950-1050 parts of cement, 730-770 parts of quartz sand, 110-130 parts of silica fume, 85-95 parts of fly ash, 6-9 parts of water reducer, 1.6-2.0 parts of microbial remediation agent, 22-26 parts of expansion agent, and 410-440 parts of water.
[0011] Preferably, the recycled concrete with self-repairing ability specifically includes the following components in parts by weight: 1250 parts of recycled aggregate, 1000 parts of cement, 750 parts of quartz sand, 120 parts of silica fume, 90 parts of fly ash, 8 parts of water reducer, 1.8 parts of microbial remediation agent, 24 parts of expansion agent, and 420 parts of water.
[0012] Preferably, the microbial remediation agent is composed of a mixture of a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens liquid in a weight ratio of 0.5-1:1-1.5.
[0013] Preferably, the microbial remediation agent is composed of a mixture of a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens liquid in a weight ratio of 0.5-0.8:1.2-1.5.
[0014] In some specific embodiments, in the microbial remediation agent, the ratio of Bacillus pasteurianus suspension and Bacillus amyloliquefaciens solution can be 0.5:1-1.2, 0.5:1.2-1.3, 0.5:1.3-1.5, 0.5-0.8:1.5, 0.6-0.8:1, 0.6-0.8:1.2, 0.6-0.8:1.3, 0.6-0.8:1.5, 0.8:1-1.2, 0.8:1.2-1.3, 0.8:1.3-1.5, 0.8:1-1.5, 1:1-1.3, 1:1.2-1.5, 1-1.5:1.3, and 1-1.5:1.5.
[0015] In a specific embodiment, in the microbial remediation agent, the ratio of Bacillus pasteurianus suspension and Bacillus amyloliquefaciens solution can also be 0.5:1, 0.5:1.2, 0.5:1.3, 0.5:1.5, 0.6:1, 0.6:1.2, 0.6:1.3, 0.6:1.5, 0.8:1, 0.8:1.2, 0.8:1.3, 0.8:1.5, 1:1, 1:1.2, 1:1.3, and 1:1.5.
[0016] Through experimental analysis, it can be known that the present application uses the Bacillus pasteurianus suspension and the Bacillus amyloliquefaciens bacterial solution in the above weight ratio as a microbial repair agent, which can further improve the performance of recycled concrete.
[0017] Preferably, the calcium salt is selected from one or more of calcium sulfoaluminate, calcium sulfate, calcium gluconate, calcium hydrogen phosphate, calcium lactate and calcium chloride.
[0018] Preferably, the bulking agent consists of calcium lactate and sorbitol in a weight ratio of 9:1-3.
[0019] In some specific embodiments, in the bulking agent, the weight ratio of calcium lactate to sorbitol can be 9:1-2 or 9:2-3.
[0020] In a specific embodiment, in the bulking agent, the weight ratio of calcium lactate to sorbitol can also be 9:1, 9:2, or 9:3.
[0021] Through experimental analysis, it is known that the type of calcium salt and the usage ratio of calcium salt to sorbitol have an impact on the performance of concrete. The present application uses calcium lactate and sorbitol in the above weight ratio as expansion agents to further improve the performance of recycled concrete.
[0022] Preferably, the quartz sand is composed of 0.5-2 mm quartz sand and 0.08-0.25 mm quartz sand mixed in a weight ratio of 1-5:5-9.
[0023] Preferably, the density of the fly ash is 2200-2400 kg / m 3 , water requirement ratio 90-95%, fineness 16-19%, loss on ignition 1.8-2.1%.
[0024] In a second aspect, the present application provides a method for preparing the above-mentioned recycled concrete with self-repairing ability, which specifically comprises the following steps: Weigh each raw material according to its weight and set aside; The recycled aggregate, cement, quartz sand, silica fume and fly ash are mixed evenly and added to water to prepare a premix; the water reducing agent and expansion agent are added to the premix and stirred to mix evenly; then the microbial remediation agent is added and mixed evenly; The mixed materials are cast and molded, and then cured to obtain the recycled concrete with self-repairing ability.
[0025] In summary, the technical solution of this application has the following effects: The technical solution provided by the present application is to mix a suspension of Bacillus pasteurianus and a suspension of Bacillus amyloliquefaciens in a weight ratio of 0.5-1.5:0.5-1.5 to form a microbial repair agent, and to use calcium salt and sorbitol as an expansion agent, which can promote carbonate precipitation and promote the self-repair effect of concrete cracks. At the same time, the recycled concrete prepared by the present application has better resistance to chloride ion penetration and shrinkage value, can maintain a high compressive strength for a long time, and has good aging resistance. DETAILED DESCRIPTION
[0026] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application. Example
[0027] Examples 1-5 Examples 1-5 respectively provide a recycled concrete and a preparation method thereof.
[0028] The difference between the above embodiments is that the amount of each component in the recycled concrete is different, as shown in Table 1.
[0029] The preparation method of recycled concrete in the above embodiment is: Preparation of microbial remediation agent: 15.0 g of casein peptone, 5.0 g of soy peptone, 5.0 g of sodium chloride, 20.0 g of agar, and 20.0 g of urea were added to 1 L of ultrapure water, the pH value was adjusted to 7.3, sterilized at 121° C. for 30 min, and cooled to room temperature to prepare a Bacillus pasteurian culture medium, and then inoculated with Bacillus pasteurian (deposit number ATCC 11859), and cultured at 30-35° C. and 120-140 r / min for 24 h to obtain a Bacillus pasteurian bacterial solution; the Bacillus pasteurian bacterial solution obtained in S3 was diluted to 7×10 7 cell / mL; 5.0 g of sodium chloride, 10.0 g of beef extract, 10.0 g of peptone, and 20.0 g of agar were added to 1 L of ultrapure water, the pH value was adjusted to 7.2, sterilized at 121° C. for 30 min, and cooled to room temperature to prepare a Bacillus amyloliquefaciens culture medium, and then inoculated with Bacillus amyloliquefaciens (deposit number CGMCC 1.0504), and cultured at 28-32° C. and 120-140 r / min for 24 h to obtain a Bacillus amyloliquefaciens culture solution; the Bacillus amyloliquefaciens culture solution obtained in S3 was diluted to 2×10 7 cell / mL.
[0030] Take 6g of Bacillus pasteurianus suspension and 13g of Bacillus amyloliquefaciens bacterial solution and mix them to form a microbial repair agent for use.
[0031] Preparation of recycled concrete: weigh each raw material according to its weight and set aside; mix recycled aggregate (5-15 mm), PO 42.5 ordinary Portland cement, quartz sand (mixed with 0.5-2 mm quartz sand and 0.08-0.25 mm quartz sand in a weight ratio of 3:7), silica fume (silica fume is silicon powder with a specific surface area of 28 ± 5 m 2 / g), fly ash (density 2300kg / m 3 , water requirement ratio 93%, fineness 17.8%, loss on ignition 1.9%) are evenly added to water and mixed to obtain a premix; Add polycarboxylate water-reducing agent QS-8020 and expansion agent (composed of calcium lactate and sorbitol in a weight ratio of 9:2) to the premix, stir and mix evenly; then add microbial remediation agent and mix evenly; The mixed materials are cast and molded, and then cured to obtain the recycled concrete with self-repairing ability.
[0032] Table 1 Amount of each component in the recycled concrete in Examples 1-5 Embodiment 6-10 Examples 6-10 respectively provide a recycled concrete and a preparation method thereof.
[0033] The difference between the above embodiment and embodiment 2 is that the composition of the microbial remediation agent is different, as shown below.
[0034] In Example 6: 13 g of Bacillus pasteurianus suspension and 6 g of Bacillus amyloliquefaciens bacterial solution were mixed to form a microbial remediation agent.
[0035] In Example 7: 10 g of Bacillus pasteurianus suspension was mixed with 5 g of Bacillus amyloliquefaciens bacterial solution to form a microbial repair agent.
[0036] In Example 8: 10 g of Bacillus pasteurianus suspension and 10 g of Bacillus amyloliquefaciens bacterial solution were mixed to form a microbial remediation agent.
[0037] In Example 9: 8 g of Bacillus pasteurianus suspension and 12 g of Bacillus amyloliquefaciens bacterial solution were mixed to form a microbial remediation agent.
[0038] In Example 10: 5 g of Bacillus pasteurianus suspension and 15 g of Bacillus amyloliquefaciens bacterial solution were mixed to form a microbial remediation agent.
[0039] The other raw materials and their amounts and the preparation method of recycled concrete in the above embodiment are the same as those in Example 2.
[0040] Examples 11-14 Examples 11-14 respectively provide a recycled concrete and a preparation method thereof.
[0041] The difference between the above embodiment and embodiment 2 is that the composition of the expansion agent is different, as shown below.
[0042] In Example 11: the bulking agent is composed of calcium gluconate and sorbitol in a weight ratio of 9:2.
[0043] In Example 12: the swelling agent is composed of calcium sulphoaluminate and sorbitol in a weight ratio of 9:2.
[0044] In Example 13: the bulking agent is composed of calcium lactate and sorbitol in a weight ratio of 9:1.
[0045] In Example 14: the expander is composed of calcium lactate and sorbitol in a weight ratio of 9:3.
[0046] The other raw materials and their amounts and the preparation method of recycled concrete in the above embodiment are the same as those in Example 2.
[0047] Comparative Example Comparative Examples 1-5 Comparative Examples 1-5 respectively provide a kind of concrete and a preparation method thereof.
[0048] The differences between the above comparative example and Example 2 are specifically as follows.
[0049] In Comparative Example 1: no microbial remediation agent and expansion agent were added to the concrete.
[0050] In Comparative Example 2: no microbial remediation agent was added to the concrete.
[0051] In Comparative Example 3: no expansion agent was added to the concrete.
[0052] In Comparative Example 4, the preparation method of the microbial remediation agent is as follows: 10.0 g of tryptone, 5.0 g of yeast extract, 10.0 g of sodium chloride, 20.0 g of agar, and 10.0 g of urea are added to 1 L of ultrapure water, the pH value is adjusted to 7.4, sterilized at 121 ° C for 30 min and cooled to room temperature to prepare a pasteurian Bacillus culture medium, and then inoculated with Bacillus subtilis (the deposit number is CGMCCNO.20464), and cultured at 30-35 ° C and 120-140 r / min for 24 h to obtain a Bacillus subtilis culture solution; the Bacillus subtilis culture solution obtained in S3 is diluted to 7×10 7 cell / mL; 5.0 g of sodium chloride, 10.0 g of beef extract, 10.0 g of peptone, and 20.0 g of agar were added to 1 L of ultrapure water, the pH value was adjusted to 7.2, sterilized at 121° C. for 30 min, and cooled to room temperature to prepare a Bacillus amyloliquefaciens culture medium, and then inoculated with Bacillus amyloliquefaciens (deposit number CGMCC 1.0504), and cultured at 28-32° C. and 120-140 r / min for 24 h to obtain a Bacillus amyloliquefaciens culture solution; the Bacillus amyloliquefaciens culture solution obtained in S3 was diluted to 2×10 7 cell / mL; Take 6g of Bacillus subtilis suspension and 13g of Bacillus amyloliquefaciens bacterial solution and mix them to form a microbial remediation agent.
[0053] In Comparative Example 5: the expander is composed of calcium sulphoaluminate and mannitol in a weight ratio of 9:2.
[0054] The other raw materials and their amounts and the preparation method of concrete in the above comparative example are the same as those in Example 2.
[0055] Performance testing (1) Compressive strength: The compressive strength of concrete is measured according to GB / T50081-2019 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete".
[0056] (2) Chloride ion penetration resistance: According to the provisions of GBJ82-85 "Test methods for long-term performance and durability of ordinary concrete", a chloride ion penetration resistance test was carried out to test the coulomb charge of concrete for 56 days.
[0057] (3) Shrinkage performance: According to the provisions of GBJ82-85 "Test methods for long-term properties and durability of ordinary concrete", a shrinkage test is carried out to test the 28-day shrinkage value of concrete.
[0058] (4) Aging resistance (80°C, 720 h): The concrete specimens were placed at 80°C for 720 h. The compressive strength of the concrete was measured according to GB / T50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", and the loss rate of compressive strength was calculated.
[0059] Test results: as shown in Table 2.
[0060] Table 2 Performance test results of concrete in the examples and comparative examples Combined with the test results in Table 2, using the technical solution provided by this application, a microbial repair agent is formed by mixing a suspension of Bacillus pasteurianus and a suspension of Bacillus amyloliquefaciens at a weight ratio of 0.5-1.5:0.5-1.5, and an expansion agent is formed by calcium salt and sorbitol, which can promote carbonate precipitation and promote the self-repair effect of concrete cracks. The recycled concrete prepared by this application has excellent resistance to chloride ion penetration and shrinkage value, and the compressive strength loss rate after aging for 720 hours at 80°C is less than 2.5%, indicating that it can maintain a high compressive strength for a long time and has a good aging resistance effect.
[0061] By comparing the test results of Example 2 with those of Examples 6-10, it can be seen that the present application uses a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens bacterial solution in a weight ratio of 0.5-1:1-1.5 as a microbial remediation agent, which can further improve the performance of recycled concrete.
[0062] By comparing the test results of Example 2 with those of Examples 11-14, it can be seen that the type of calcium salt and the usage ratio of calcium salt to sorbitol have an impact on the performance of concrete. The present application uses calcium lactate and sorbitol in a weight ratio of 9:1-3 as expansion agents, which can further improve the performance of recycled concrete.
[0063] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A recycled concrete with self-repairing ability, characterized in that: Specifically, it includes the following components in parts by weight: 1200-1300 parts of recycled aggregate, 900-1100 parts of cement, 700-800 parts of quartz sand, 100-140 parts of silica fume, 80-100 parts of fly ash, 5-10 parts of water reducer, 1.2-2.4 parts of microbial remediation agent, 20-28 parts of expansion agent, and 400-450 parts of water; The microbial repair agent is composed of a mixture of a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens bacterial solution in a weight ratio of 0.5-1.5:0.5-1.5; the concentration of the Bacillus pasteurianus suspension is 6-8×10 7 cell / mL, and the concentration of the Bacillus amyloliquefaciens culture solution is 1-3×10 7 cell / mL; The bulking agent consists of calcium salt and sorbitol in a weight ratio of 9:1-3.
2. The recycled concrete with self-repairing ability according to claim 1, characterized in that: Specifically, it includes the following components in parts by weight: 1220-1280 parts of recycled aggregate, 950-1050 parts of cement, 730-770 parts of quartz sand, 110-130 parts of silica fume, 85-95 parts of fly ash, 6-9 parts of water reducer, 1.6-2.0 parts of microbial remediation agent, 22-26 parts of expansion agent, and 410-440 parts of water.
3. The recycled concrete with self-repairing ability according to claim 1, characterized in that: Specifically, it includes the following components in parts by weight: 1250 parts of recycled aggregate, 1000 parts of cement, 750 parts of quartz sand, 120 parts of silica fume, 90 parts of fly ash, 8 parts of water reducer, 1.8 parts of microbial remediation agent, 24 parts of expansion agent, and 420 parts of water.
4. The recycled concrete with self-repairing ability according to claim 1, characterized in that: The microbial repair agent is composed of a mixture of a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens bacterial solution in a weight ratio of 0.5-1:1-1.
5.
5. The recycled concrete with self-repairing ability according to claim 4, characterized in that: The microbial repair agent is composed of a mixture of a Bacillus pasteurianus suspension and a Bacillus amyloliquefaciens bacterial solution in a weight ratio of 0.5-0.8:1.2-1.
5.
6. The recycled concrete with self-repairing ability according to claim 1, characterized in that: The calcium salt is selected from one or more of calcium sulfoaluminate, calcium sulfate, calcium gluconate, calcium hydrogen phosphate, calcium lactate and calcium chloride.
7. The recycled concrete with self-repairing ability according to claim 1, characterized in that: The bulking agent consists of calcium lactate and sorbitol in a weight ratio of 9:1-3.
8. The recycled concrete with self-repairing ability according to claim 1, characterized in that: The quartz sand is composed of 0.5-2 mm quartz sand and 0.08-0.25 mm quartz sand mixed in a weight ratio of 1-5:5-9.
9. The recycled concrete with self-repairing ability according to claim 1, characterized in that: The density of the fly ash is 2200-2400kg / m 3 , water requirement ratio 90-95%, fineness 16-19%, loss on ignition 1.8-2.1%.
10. The method for preparing recycled concrete with self-repairing ability according to any one of claims 1 to 9, characterized in that: The specific steps include: Weigh each raw material according to its weight and set aside; The recycled aggregate, cement, quartz sand, silica fume and fly ash are mixed evenly and added into water to prepare a premix; Add water reducing agent and expansion agent to the premix, stir and mix evenly; then add microbial remediation agent and mix evenly; The mixed materials are cast and molded, and then cured to obtain the recycled concrete with self-repairing ability.
Citation Information
Patent Citations
Crack self-remediation regenerated concrete based on urease production microorganism mineralization deposition and preparation method
CN106699026A
Bacillus amyloliquefaciens ZJB19161 and application thereof
CN111575210A
Microbial self-repairing concrete and preparation method thereof
CN112500074A
Crack self-repairing cement-based material and preparation method thereof
CN116730685A
Microorganism-containing self-repairing recycled concrete
CN117800662A