Modified phosphogypsum lightweight thermal insulation building block and preparation method thereof
Through the preparation of modified phosphogypsum light-weight insulation blocks, the combination of phosphogypsum and other raw materials is used to solve the problems of phosphogypsum storage and performance defects, efficient utilization and performance improvement are achieved, and high performance, energy-saving and environmentally friendly Building materials.
Patent Information
- Application Number
- CN202411213961.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to effectively utilize phosphogypsum, resulting in defects in its storage pressure and performance. Traditional insulation materials have poor fire resistance and durability, making it difficult to meet the requirements of building materials.
Use modified phosphogypsum lightweight insulation blocks, and prepare phosphogypsum with raw materials such as sodium silicate, quicklime, cement, polyaluminum chloride, calcium formate, glue powder, cellulose ether, sodium hydroxide and aluminum powder paste. Combined with the modifier treatment, a product that meets the GB/T11968-2020 standard was prepared to improve the utilization rate and performance of phosphogypsum.
It realizes efficient utilization of phosphogypsum, improves the strength and insulation performance of phosphogypsum, reduces energy consumption of buildings, reduces environmental pollution, and provides a new type of thermal insulation material that is high-performance, energy-saving and environmentally friendly.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a modified phosphogypsum lightweight thermal insulation building block and a preparation method thereof. Background Art
[0002] Autoclaved aerated concrete blocks are porous concrete building wall masonry materials made from fly ash or sand, lime, cement, gypsum, etc. as the main raw materials, with appropriate amounts of gas generating agents, regulators, stabilizers, and a process of batching, mixing, pouring, standing, cutting, and high-pressure steaming.
[0003] Phosphogypsum is a byproduct of the production of phosphoric acid and phosphate fertilizers. Its main component is calcium sulfate dihydrate. Every ton of phosphoric acid produced can produce 4-5 tons of byproduct phosphogypsum. How to apply phosphogypsum on a large scale in the field of building materials has always been the main direction of the comprehensive utilization of phosphogypsum. In recent years, the phosphogypsum developed is mainly used for cement retarders, building gypsum powder, gypsum hollow blocks, gypsum boards and other products, and its comprehensive utilization rate is limited. If phosphogypsum is developed into modified phosphogypsum lightweight insulation block products, the non-condensing energy can significantly improve the utilization rate of phosphogypsum and alleviate the pressure of phosphogypsum storage. By modifying phosphogypsum, some of its original performance defects, such as insufficient strength and poor water resistance, can be improved, so that it can meet the requirements of building materials; the lightweight characteristics can reduce the weight of the building, facilitate construction and transportation; and good thermal insulation performance can reduce the heat exchange inside and outside the building, reduce energy consumption, and conform to the concept of sustainable development.
[0004] In addition, traditional thermal insulation materials may have problems such as poor fire resistance and poor durability during use. During the research and development of modified phosphogypsum, these factors were fully considered, aiming to provide a building material with superior comprehensive performance. It can not only effectively solve the disposal problem of phosphogypsum and reduce environmental pollution, but also provide the construction industry with a high-performance, energy-saving and environmentally friendly new thermal insulation material, promoting the construction industry to develop in a green and low-carbon direction. At the same time, the development of related technologies has also promoted the cross-integration of fields such as materials science and chemical engineering, providing more possibilities for the innovation and optimization of building materials.
[0005] How to effectively utilize phosphogypsum and give full play to its excellence, realize its resource utilization and harmlessness, and achieve sustainable development has become an urgent problem to be solved in the current building materials market. Summary of the invention
[0006] In view of the above shortcomings, the present invention provides a modified phosphogypsum lightweight thermal insulation block and a preparation method thereof. The product indicators meet the relevant requirements of GB / T11968-2020, the product has high strength, low thermal conductivity, can effectively prevent the transfer of heat, and has more outstanding thermal insulation performance and lightweight texture. The specific technical scheme is as follows:
[0007] A modified phosphogypsum lightweight thermal insulation building block comprises the following raw materials in parts by weight:
[0008] 86-120 parts of modified phosphogypsum initial material, 1.5-2 parts of sodium silicate, 4-5 parts of quicklime, 35-45 parts of water, 25-35 parts of cement, 0.15-0.3 parts of polyaluminium chloride, 0.2-0.3 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, 0.2-0.3 parts of sodium hydroxide, 0.2-0.3 parts of water reducing agent and 0.06-0.08 parts of aluminium powder paste.
[0009] Preferably, the modified phosphogypsum lightweight thermal insulation building block comprises the following raw materials in parts by weight:
[0010] 95-110 parts of modified phosphogypsum initial material, 1.5-1.8 parts of sodium silicate, 4-5 parts of quicklime, 38-42 parts of water, 28-32 parts of cement, 0.2-0.3 parts of polyaluminium chloride, 0.2-0.3 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, 0.2-0.3 parts of sodium hydroxide, 0.2-0.3 parts of water reducing agent and 0.06-0.07 parts of aluminium powder paste.
[0011] Preferably, the modified phosphogypsum primary material comprises the following raw materials in parts by weight: 65-80 parts of original phosphogypsum, 15-30 parts of fly ash, 6-10 parts of carbide slag, and 1-5 parts of modifier;
[0012] The preparation method of the modified phosphogypsum raw material is as follows: carbide slag, fly ash, original phosphogypsum and a modifier are stirred and stored for 40-55 hours to obtain the modified phosphogypsum raw material.
[0013] Preferably, the pH value of the original phosphogypsum is 2-3, wherein calcium sulfate is greater than 85%, sulfur trioxide is greater than 40%, phosphorus pentoxide is less than 4%, and the water content is 15-22%; the fly ash is wet discharge stockpile ash from a power plant, wherein silicon dioxide is greater than 40%, aluminum oxide is greater than 15%, loss on ignition is less than 10%, sulfur trioxide is less than 4%, and the water content is 12-16%; the carbide slag is the waste residue after acetylene gas is obtained by hydrolyzing calcium carbide in a chemical plant, wherein calcium oxide is greater than 60%, silicon oxide is greater than 3.5%, aluminum oxide is greater than 2.5%, and the water content is 20-25%.
[0014] Preferably, the modifier is a mixture of citric acid, sodium silicate and calcium stearate in a mass ratio of 1-1.5:1:1.
[0015] Preferably, the water reducer is a polycarboxylic acid high-efficiency water reducer, which reduces water consumption and improves the density and strength of the blocks while ensuring working performance.
[0016] Preferably, the cement is ordinary Portland cement with a strength of not less than 42.5.
[0017] Preferably, the water is industrial water or groundwater, and the pulping water temperature is 20-25°C.
[0018] The present invention also provides a method for preparing a modified phosphogypsum lightweight thermal insulation building block, comprising the following steps:
[0019] S1. Grind the modified phosphogypsum raw material into 40-200 meshes to obtain modified gypsum slurry;
[0020] S2, mixing the modified gypsum slurry, quicklime, sodium silicate and water according to the weight ratio for 30-40 minutes to prepare a premixed slurry;
[0021] S3. Mix the premixed slurry, cement, polyaluminium chloride, calcium formate, rubber powder, cellulose ether, sodium hydroxide and water reducing agent according to the weight ratio for 3-5 minutes, then add aluminium powder into the mixed slurry and stir for 1-2 minutes to prepare the green body casting slurry.
[0022] S4, injecting the prepared green body casting slurry into a mold coated with a release agent, pushing it to a curing room for constant temperature and standing to gasify for 3-4 hours, then demolding and cutting the green body into shape, sending the cut blocks to a curing room for constant temperature curing at 35-40°C for 20-30 hours, packaging the products, and then sending them to a ventilated place for natural curing for 6-7 days to obtain modified phosphogypsum lightweight thermal insulation blocks.
[0023] Preferably, the rubber powder is dispersible latex powder.
[0024] Preferably, the aqueous release agent has a coating thickness of 0.2-0.5 mm.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The modified phosphogypsum lightweight thermal insulation building blocks made by the present invention meet the relevant requirements of GB / T11968-2020. The product has high strength and low thermal conductivity, can effectively prevent the transfer of heat, and has more outstanding thermal insulation performance, so that the building can keep warm in winter and cool in summer, thereby significantly reducing the energy consumption of the building and improving indoor comfort. The thermal insulation building blocks of the present invention use modified phosphogypsum as the main raw material, which improves the utilization rate of phosphogypsum, realizes the resource utilization of industrial waste, effectively reduces environmental pollution, is low-carbon and energy-saving, and has high production efficiency.
[0027] 2. The present invention modifies the original phosphogypsum, adds fly ash, carbide slag and modifiers to the original phosphogypsum, stirs and stores them, significantly improves the performance of the phosphogypsum, eliminates water washing and calcination, avoids too fast gypsum coagulation speed, enables it to meet the requirements of lightweight thermal insulation blocks, has a good phosphorus removal effect, and has a large output and low cost. The modifier composed of citric acid, sodium silicate and calcium stearate is added to help the slurry to entrain air and foam, reduce the bulk density of the blocks, and achieve a lightweight texture. The addition of the modifier can also improve the performance of the phosphogypsum, improve the strength, water resistance and durability, and further improve the modification effect.
[0028] 3. The sodium silicate, quicklime and other ingredients added to the block formula of the present invention help to improve the strength and water absorption of the block and extend the service life of the block; the use of additives such as polyaluminium chloride and calcium formate improves the setting time and crack resistance of the block and improves the quality of the product; the addition of glue powder and cellulose ether enhances the bonding and construction performance of the block, making it easier to construct and operate; the addition of sodium hydroxide can adjust the pH value of the system, optimize the reaction environment, and further improve product performance. The introduction of aluminum powder paste enables the block to produce uniform pores during the preparation process, reduces the bulk density of the block, achieves a lightweight texture, and improves thermal insulation performance. DETAILED DESCRIPTION
[0029] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0030] Example 1
[0031] The modified phosphogypsum lightweight thermal insulation building block of this embodiment includes the following raw materials in parts by weight:
[0032] 86 parts of modified phosphogypsum initial material, 1.5 parts of sodium silicate, 4 parts of quicklime, 35 parts of water, 25 parts of cement, 0.15 parts of polyaluminium chloride, 0.2 parts of calcium formate, 0.01 parts of dispersible latex powder, 0.03 parts of cellulose ether, 0.2 parts of sodium hydroxide, 0.2 parts of polycarboxylic acid high-efficiency water reducing agent, and 0.06 parts of aluminium powder paste.
[0033] The modified phosphogypsum initial material of this embodiment includes the following raw materials in parts by weight: 65 parts of original phosphogypsum, 15 parts of fly ash, 6 parts of carbide slag, and 1 part of modifier.
[0034] The preparation method of the modified phosphogypsum primary material of this embodiment comprises the following steps:
[0035] (1) placing the original phosphogypsum in a washing tank, washing it twice with running water to remove impurities, and then drying it at 80° C. until the water content is less than 5%; placing the dried phosphogypsum in a calcining furnace, and calcining it at 160° C. for 1.5 hours;
[0036] (2) adding a modifier to the calcined phosphogypsum, and stirring the mixture in a high-speed stirrer at a rotation speed of 800 rpm for 20 min to obtain a phosphogypsum mixture;
[0037] (3) The phosphogypsum mixture is stored for 40 hours to obtain the modified phosphogypsum raw material.
[0038] The modifier of this embodiment is a mixture of citric acid, sodium silicate and calcium stearate in a mass ratio of 1:1:1.
[0039] The method for preparing the modified phosphogypsum lightweight thermal insulation building block of this embodiment comprises the following steps:
[0040] S1. Grind the modified phosphogypsum raw material into 40 meshes to obtain modified gypsum slurry;
[0041] S2, mixing the modified gypsum slurry, quicklime, sodium silicate and water according to the weight ratio for 30 minutes to prepare a premixed slurry;
[0042] S3. Mix the premixed slurry, cement, polyaluminium chloride, calcium formate, dispersible latex powder, cellulose ether, sodium hydroxide and polycarboxylic acid high-efficiency water reducing agent according to the weight ratio for 3 minutes, then add aluminium powder into the mixed slurry and stir for 1 minute to prepare the green body casting slurry.
[0043] S4. Inject the prepared green body casting slurry into a mold coated with a 0.2 mm thick water-based release agent, and then push it to a curing room for constant temperature and static gas curing for 3 hours. Then demold and cut the green body into pieces, and send the cut blocks to a curing room for constant temperature curing at 35°C for 20 hours. The products are packaged and then sent to a ventilated place for natural curing for 6 days to obtain modified phosphogypsum lightweight thermal insulation blocks.
[0044] Example 2
[0045] The modified phosphogypsum lightweight thermal insulation building block of this embodiment includes the following raw materials in parts by weight:
[0046] 120 parts of modified phosphogypsum initial material, 2 parts of sodium silicate, 5 parts of quicklime, 45 parts of water, 35 parts of cement, 0.3 parts of polyaluminium chloride, 0.3 parts of calcium formate, 0.02 parts of dispersible latex powder, 0.05 parts of cellulose ether, 0.3 parts of sodium hydroxide, 0.3 parts of polycarboxylic acid high-efficiency water reducing agent, and 0.08 parts of aluminium powder paste.
[0047] The modified phosphogypsum initial material of this embodiment includes the following raw materials in parts by weight: 80 parts of original phosphogypsum, 30 parts of fly ash, 10 parts of carbide slag, and 5 parts of modifier.
[0048] The preparation method of the modified phosphogypsum raw material in this embodiment is to mix and stir electroslag stone, fly ash, original phosphogypsum and modifier and store them for 55 hours to obtain the modified phosphogypsum raw material.
[0049] The modifier of this embodiment is a mixture of citric acid, sodium silicate and calcium stearate in a mass ratio of 1.5:1:1.
[0050] The method for preparing the modified phosphogypsum lightweight thermal insulation building block of this embodiment comprises the following steps:
[0051] S1. Grind the modified phosphogypsum raw material into 200 meshes to obtain modified gypsum slurry;
[0052] S2, mixing the modified gypsum slurry, quicklime, sodium silicate and water according to the weight ratio for 40 minutes to prepare a premixed slurry;
[0053] S3. Mix the premixed slurry, cement, polyaluminium chloride, calcium formate, dispersible latex powder, cellulose ether, sodium hydroxide and polycarboxylic acid high-efficiency water reducer according to the weight ratio and stir for 5 minutes, then add aluminium powder into the mixed slurry and stir for 2 minutes to prepare the green body casting slurry.
[0054] S4. Inject the prepared green body casting slurry into a mold coated with a 0.5 mm thick water-based release agent, and then push it to a curing room for constant temperature and static gas curing for 4 hours. Then demold and cut the green body into pieces, and send the cut blocks to a curing room for constant temperature curing at 40°C for 30 hours. The products are packaged and then sent to a ventilated place for natural curing for 7 days to obtain modified phosphogypsum lightweight thermal insulation blocks.
[0055] Example 3
[0056] The modified phosphogypsum lightweight thermal insulation building block of this embodiment includes the following raw materials in parts by weight:
[0057] 100 parts of modified phosphogypsum raw material, 1.8 parts of sodium silicate, 4.5 parts of quicklime, 40 parts of water, 30 parts of cement, 0.2 parts of polyaluminium chloride, 0.25 parts of calcium formate, 0.01 parts of dispersible latex powder, 0.02 parts of cellulose ether, 0.25 parts of sodium hydroxide, 0.25 parts of polycarboxylic acid high-efficiency water reducing agent, and 0.07 parts of aluminium powder paste.
[0058] The modified phosphogypsum initial material of this embodiment includes the following raw materials in parts by weight: 72 parts of original phosphogypsum, 22 parts of fly ash, 8 parts of calcium carbide slag, and 3 parts of modifier.
[0059] The preparation method of the modified phosphogypsum raw material in this embodiment is to mix and stir electroslag stone, fly ash, original phosphogypsum and modifier and store them for 50 hours to obtain the modified phosphogypsum raw material.
[0060] The modifier of this embodiment is a mixture of citric acid, sodium silicate and calcium stearate in a mass ratio of 1.2:1:1.
[0061] The method for preparing the modified phosphogypsum lightweight thermal insulation building block of this embodiment comprises the following steps:
[0062] S1. Grind the modified phosphogypsum raw material into 100 meshes to obtain modified gypsum slurry;
[0063] S2, mixing the modified gypsum slurry, quicklime, sodium silicate and water according to the weight ratio for 35 minutes to prepare a premixed slurry;
[0064] S3. Mix the premixed slurry, cement, polyaluminium chloride, calcium formate, dispersible latex powder, cellulose ether, sodium hydroxide and polycarboxylic acid high-efficiency water reducer according to the weight ratio and stir for 4 minutes, then add aluminium powder to the mixed slurry and stir for 2 minutes to prepare the green body casting slurry.
[0065] S4. Inject the prepared green body casting slurry into a mold coated with a 0.3 mm thick water-based release agent, and then push it to a curing room for constant temperature and static gas curing for 3-4 hours, then demould and cut the green body into pieces, send the cut blocks to a curing room for constant temperature curing at 40°C for 25 hours, package the products, and then send them to a ventilated place for natural curing for 7 days to obtain modified phosphogypsum lightweight thermal insulation blocks.
[0066] Comparative Example 1: The difference from Example 3 is that the modified phosphogypsum raw material is replaced by original phosphogypsum that has not been modified.
[0067] Comparative Example 2: The difference from Example 3 is that the modifier is removed in the preparation method of the modified phosphogypsum raw material.
[0068] Comparative Example 3: The difference from Example 3 is that the modifier is citric acid.
[0069] Comparative Example 4: The difference from Example 3 is that polyaluminium chloride and calcium formate are not added.
[0070] Comparative Example 5: The difference from Example 3 is that no rubber powder and cellulose ether are added.
[0071] Comparative Example 6: The difference from Example 3 is that no aluminum powder paste is added.
[0072] Comparative Example 7: The difference from Example 3 is that no modifier is added, and the preparation method of the phosphogypsum lightweight thermal insulation block is different, as follows:
[0073] (1) placing the original phosphogypsum in a water washing tank, washing it with running water for 3 times to remove impurities therein, and then drying it at 90° C. until the water content is less than 5%, thereby obtaining washed phosphogypsum;
[0074] (2) Mixing washed phosphogypsum, quicklime, sodium silicate and water according to the weight ratio for 35 minutes to prepare a premixed slurry;
[0075] (3) mixing the premixed slurry, cement, polyaluminium chloride, calcium formate, dispersible latex powder, cellulose ether, sodium hydroxide and polycarboxylic acid high-efficiency water reducer according to the weight ratio for 4 minutes, and then adding aluminium powder to the mixed slurry and stirring for 2 minutes to prepare a green body casting slurry;
[0076] (4) The prepared green body casting slurry is injected into a mold coated with a 0.3 mm thick water-based release agent, and a layered vibration method is adopted, with each layer vibrating for 1-2 minutes and a vibration frequency of 55 Hz. After the vibration is completed, it is pushed to a curing room for constant temperature and static gas curing for 3-4 hours, and then the green body is demolded and cut into shape. The cut blocks are sent to a curing room for constant temperature curing at 40°C for 25 hours. The products are packaged and then sent to a ventilated place for natural curing for 7 days to obtain phosphogypsum lightweight thermal insulation blocks.
[0077] Comparative Example 8: The difference from Example 3 is that the preparation method of the modified phosphogypsum raw material is different, as follows:
[0078] (1) placing the original phosphogypsum in a calcining furnace and calcining it at 170° C. for 2 h;
[0079] (2) adding a modifier to the calcined phosphogypsum, and stirring the mixture in a high-speed stirrer at a rotation speed of 900 rpm for 25 min to obtain a phosphogypsum mixture;
[0080] (3) The phosphogypsum mixture is stored for 50 hours to obtain the modified phosphogypsum raw material.
[0081] The phosphogypsum blocks obtained in the above embodiments and comparative examples were subjected to various performance tests, including mechanical performance tests according to the standard "GB / T17669.3-1999", waterproof performance tests according to "JC474-2008", thermal conductivity tests according to "JGJ / T447-2018", and dry density and dry shrinkage tests according to the standard "B / T11969-2008". The test results are shown in Table 1.
[0082] Table 1 Various properties of modified phosphogypsum lightweight insulation blocks
[0083]
[0084]
[0085] The results show that the blocks of Examples 1-3 have excellent dry density, compressive strength, thermal conductivity, dry shrinkage and water resistance, and the indicators meet the relevant requirements of GB / T11968-2020; Comparative Example 1 has poor performance of the original phosphogypsum, and the resulting blocks have low strength, high water absorption and poor water resistance, which cannot meet the actual use requirements; the strength and thermal conductivity of the blocks of Comparative Example 2 and Comparative Example 3 are significantly reduced, indicating that the modifier plays a key role in improving the thermal insulation performance of phosphogypsum; In Comparative Example 4, no polyaluminum chloride and calcium formate are added, which leads to a long setting time of the blocks, insufficient crack resistance, and easy cracks during use; In Comparative Example 5, no glue powder and cellulose ether are added, the bonding performance and construction performance of the blocks deteriorate, and the construction difficulty increases; In Comparative Example 6, no aluminum powder paste is added, resulting in a larger bulk density of the blocks, making it difficult to achieve a lightweight texture, and the thermal insulation performance is also significantly reduced. The dry density and compressive strength of the blocks are not as good as those of the products of the present invention, and the working performance is also poor; Comparative Examples 7 and 8 respectively use the water washing method and the calcination method to prepare blocks, and the performance of the products is not bad. However, although the water washing method has a good phosphorus removal effect, it has great environmental pollution, high cost, and small output, and cannot form large-scale production. It has little economic benefit and social value, and the vibrating of the thick casting will destroy the bubbles generated by the air entrainment and collapse the mold, making it impossible to achieve foaming and lightweight. In Comparative Example 8, the phosphogypsum will become semi-hydrated gypsum after high-temperature calcination. The production of gypsum products sets very quickly, and the bulk density is greatly increased, so it cannot be used for foaming lightweight blocks.
[0086] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A modified phosphogypsum lightweight thermal insulation building block, characterized in that: The invention comprises the following raw materials in parts by weight: 86-120 parts of modified phosphogypsum initial material, 1.5-2 parts of sodium silicate, 4-5 parts of quicklime, 35-45 parts of water, 25-35 parts of cement, 0.15-0.3 parts of polyaluminium chloride, 0.2-0.3 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, 0.2-0.3 parts of sodium hydroxide, 0.2-0.3 parts of water reducing agent and 0.06-0.08 parts of aluminium powder paste.
2. A modified phosphogypsum lightweight thermal insulation block according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 95-110 parts of modified phosphogypsum initial material, 1.5-1.8 parts of sodium silicate, 4-5 parts of quicklime, 38-42 parts of water, 28-32 parts of cement, 0.2-0.3 parts of polyaluminium chloride, 0.2-0.3 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, 0.2-0.3 parts of sodium hydroxide, 0.2-0.3 parts of water reducing agent and 0.06-0.07 parts of aluminium powder paste.
3. A modified phosphogypsum lightweight thermal insulation block according to claim 1, characterized in that: The modified phosphogypsum primary material comprises the following raw materials in parts by weight: 65-80 parts of original phosphogypsum, 15-30 parts of fly ash, 6-10 parts of carbide slag, and 1-5 parts of a modifier.
4. A modified phosphogypsum lightweight thermal insulation building block according to claim 3, characterized in that: The preparation method of the modified phosphogypsum raw material is as follows: carbide slag, fly ash, original phosphogypsum and a modifier are stirred and stored for 40-55 hours to obtain the modified phosphogypsum raw material.
5. The modified phosphogypsum lightweight thermal insulation building block according to claim 3, characterized in that: The pH value of the original phosphogypsum is 2-3, wherein calcium sulfate is greater than 85%, sulfur trioxide is greater than 40%, phosphorus pentoxide is less than 4%, and the water content is 15-22%; the fly ash is wet discharge stockpile ash from a power plant, wherein silicon dioxide is greater than 40%, aluminum oxide is greater than 15%, loss on ignition is less than 10%, sulfur trioxide is less than 4%, and the water content is 12-16%; the carbide slag is the waste residue after acetylene gas is obtained by hydrolyzing calcium carbide in a chemical plant, wherein calcium oxide is greater than 60%, silicon oxide is greater than 3.5%, aluminum oxide is greater than 2.5%, and the water content is 20-25%.
6. The modified phosphogypsum lightweight thermal insulation building block according to claim 3, characterized in that: The modifier is prepared by mixing citric acid, sodium silicate and calcium stearate in a mass ratio of 1-1.5:1:
1.
7. The modified phosphogypsum lightweight thermal insulation building block according to claim 1, characterized in that: The water reducer is a polycarboxylic acid high efficiency water reducer.
8. The method for preparing a modified phosphogypsum lightweight thermal insulation building block according to any one of claims 1 to 6, characterized in that: The steps include: S1. Grind the modified phosphogypsum raw material into 40-200 meshes to obtain modified gypsum slurry; S2, mixing the modified gypsum slurry, quicklime, sodium silicate and water according to the weight ratio for 30-40 minutes to prepare a premixed slurry; S3, mixing the premixed slurry, cement, polyaluminium chloride, calcium formate, rubber powder, cellulose ether, sodium hydroxide and water reducing agent according to the weight ratio for 3-5 minutes, then adding aluminium powder to the mixed slurry and stirring for 1-2 minutes to prepare the green body casting slurry; S4, injecting the prepared green body casting slurry into a mold coated with a release agent, pushing it to a curing room for constant temperature and standing to gasify for 3-4 hours, then demolding and cutting the green body into shape, sending the cut blocks to a curing room for constant temperature curing at 35-40°C for 20-30 hours, packaging the products, and then sending them to a ventilated place for natural curing for 6-7 days to obtain modified phosphogypsum lightweight thermal insulation blocks.
9. Use of the modified phosphogypsum lightweight thermal insulation block according to any one of claims 1 to 8 in the field of building materials.
Citation Information
Cited By
Partial dry-process fresh semi-hydrated phosphogypsum cementing material
CN119822775A
Method of production of a mineral foam obtained from a foaming slurry of high yield stress
EP4768458A1
Method of production of a mineral foam obtained from a foaming slurry of high yield stress
WO2026139566A1