Method for preparing three-dimensional ordered porous silicon carbide with double-type pore structure

Through the cross-linking and high-temperature ceramicization of SiO2 nanosphere template and polycarbosilane pioneer, combined with template removal and hydrofluoric acid etching, the problem of insufficient resistance of three-dimensional ordered porous materials in high-temperature oxidation and corrosion environments was solved, and the problem of insufficient resistance of three-dimensional orderly porous materials in high-temperature oxidation and corrosion environment was prepared. The double-pore structure silicon carbide ceramic with excellent oxidation resistance and corrosion resistance has expanded its application range.

CN119039040AInactive Publication Date: 2024-11-29NINGBO ZHONGXING NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202310616662.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing three-dimensional ordered porous materials have poor resistance in high-temperature oxidation and corrosion environments, which limits their application range.

Method used

SiO2 nanospheres are self-assembled into a template, and three-dimensional orderly porous silicon carbide ceramics with a double-porous structure are prepared by cross-linking and high-temperature ceramicization of polycarbonsilane pioneers, combined with template removal and hydrofluoric acid etching, and three-dimensional orderly porous silicon carbide ceramics with double-porous structure are improved. Antioxidant and corrosion resistance.

Benefits of technology

Three-dimensional orderly porous silicon carbide ceramics with excellent oxidation resistance and corrosion resistance were prepared, which expanded its application range in high-temperature oxidation and corrosion environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039040A_ABST
    Figure CN119039040A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing three-dimensional ordered porous silicon carbide with a double-type pore structure, which comprises the following steps: uniformly dispersing SiO2 nanospheres with uniform diameter in a solvent, self-assembling to form a three-dimensional ordered template, removing the solvent, and drying; pouring a polycarbosilane precursor dispersion liquid into a container in which the template is positioned, dipping, and removing the solvent; performing crosslinking in an oxygen-containing atmosphere; performing ceramization in an inert atmosphere; performing heat treatment in an oxidizing atmosphere; and dipping and cleaning in hydrofluoric acid to obtain the target ceramic. According to the invention, the three-dimensional ordered porous SiC ceramic with a double-type pore structure and a high specific surface area can be prepared, so that the three-dimensional ordered porous material can be used in high-temperature, oxidized and corrosive environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing three-dimensional ordered porous silicon carbide, and in particular to a method for preparing three-dimensional ordered porous silicon carbide with a dual-type pore structure. Background Art

[0002] Three-dimensional ordered porous materials have many excellent properties such as three-dimensional through-pore structure, large specific surface area, light weight, etc., and are widely used in adsorption, filtration, catalysis, hydrogen storage, lightweight materials and thermal insulation. They are urgently needed in aviation, aerospace, military and other fields.

[0003] Since the 1990s, three-dimensional ordered porous materials have developed rapidly, and the preparation technologies of three-dimensional ordered porous SiO2 and three-dimensional ordered porous carbon with various pore types and pore sizes have been mastered successively. The above materials have super large specific surface area and super strong adsorption capacity, and show excellent performance in catalysis, hydrogen storage and other fields. However, the above porous materials have poor resistance to high temperature oxidation and corrosion, which limits their application range. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a new method for preparing three-dimensional ordered porous silicon carbide with a dual-type pore structure.

[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: A method for preparing three-dimensional ordered porous silicon carbide with a dual-type pore structure comprises the following steps: (1) Dispersing SiO2 nanospheres of uniform diameter uniformly in a solvent, allowing the SiO2 nanospheres to self-assemble into a three-dimensional ordered template through natural deposition, removing the solvent and drying; the deposition process can be carried out in a container of a specific shape, and the shape of the naturally deposited SiO2 nanospheres is related to the shape of the container. The macroscopic shape of the obtained template and even the final ceramic is affected by the shape of the container in which the SiO2 nanospheres are naturally deposited. The shape of the container can be selected according to actual needs; (2) Pour a polycarbosilane precursor (PCS) dispersion into the container where the template is located, immerse it, and remove the solvent; when the volume of the PCS used is equivalent to the volume of the template, the production efficiency is the highest; when the volume of the PCS is large, the non-porous part beyond the template can be removed by cutting and grinding after the material is formed, thereby obtaining an ideal structure; when the volume of the PCS is small, the template is not fully utilized, but the obtained material still has the expected structure; (3) cross-linking the product obtained in step (2) in an oxygen-containing atmosphere to introduce oxygen during the cross-linking process; (4) The product obtained in step (3) is heat treated in an inert atmosphere to ceramicize it; (5) The product obtained in step (4) is heat-treated in an oxidizing atmosphere to remove free carbon; after the free carbon is removed, micropores are formed at the positions originally occupied by carbon; (6) The product obtained in step (5) is immersed in hydrofluoric acid to etch away some components in the template and the ceramic product, and then cleaned to obtain the target ceramic.

[0006] The solvent can be removed by distillation under reduced pressure, or other methods that can remove the solvent are also feasible.

[0007] By adopting the above technical solution, three-dimensional ordered porous silicon carbide with a dual-type pore structure is obtained.

[0008] Preferably, in step (1), ultrasound is used to assist the dispersion of SiO2 nanospheres.

[0009] The above technical solution is adopted to help disperse SiO2 nanospheres.

[0010] Preferably, in step (1), the particle size of the SiO2 nanospheres is less than 1000 nm, more preferably 10-800 nm.

[0011] By adopting the above technical solution, the obtained silicon carbide ceramic has a reasonable pore structure.

[0012] Preferably, in step (1), the solvent is anhydrous ethanol.

[0013] The SiO2 nanospheres have good dispersibility in anhydrous ethanol. The above technical solution is helpful for the dispersion and natural deposition of SiO2 nanospheres, and anhydrous ethanol is easy to remove; it is also feasible to use other solvents with similar properties.

[0014] Preferably, in step (1), the weight ratio of SiO2 nanospheres to solvent is 5-30:100.

[0015] By adopting the above technical solution, better dispersion and deposition effects are achieved.

[0016] Preferably, in step (2), the solvent in the PCS dispersion is tetrahydrofuran (THF).

[0017] The solvent plays a role in dispersing PCS. By adopting the above technical solution, PCS can be dispersed in the dispersion liquid; it is also feasible to use other solvents with similar properties.

[0018] Preferably, in step (2), the concentration of the PCS dispersion is 10-80% (g / g), more preferably 25-70% (g / g).

[0019] By adopting the above technical solution, a better impregnation effect is achieved.

[0020] Preferably, in step (2), the immersion time is 5 to 30 hours, more preferably 10 to 24 hours.

[0021] By adopting the above technical solution, a better impregnation effect is achieved.

[0022] Preferably, in step (3), the oxygen-containing atmosphere is an air atmosphere.

[0023] The atmosphere is used to provide oxygen. The above technical solution can provide an oxygen-containing atmosphere. It is also feasible to use other oxygen-containing atmospheres that can provide oxygen to the system during the crosslinking process.

[0024] Preferably, in step (3), the temperature during cross-linking is 150-250° C., more preferably 160-220° C., and the cross-linking time is 2-30 h, more preferably 5-25 h.

[0025] By adopting the above technical solution, PCS can be oxidatively cross-linked and oxygen can be introduced.

[0026] Preferably, in step (4), the inert atmosphere is an argon atmosphere. The inert atmosphere is used to provide an environment that does not participate in chemical reactions. The above technical solution can provide a suitable reaction environment; other atmospheres that can achieve this effect are also feasible.

[0027] Preferably, in step (4), the temperature of the ceramic heat treatment is 800-1650° C., more preferably 1000-1600° C., and the temperature is maintained for 0.5-5 h, more preferably 0.5-3 h.

[0028] By adopting the above technical solution, a better ceramicizing effect is achieved.

[0029] Preferably, in step (4), the heating rate is 5 to 50°C / min, more preferably 10 to 30°C / min.

[0030] By adopting the above technical solution, a better ceramicizing effect is achieved.

[0031] Preferably, in step (5), the oxidizing atmosphere is an air atmosphere.

[0032] By adopting the above technical solution, free carbon can be oxidized into gas and thus removed; other oxidizing atmospheres that can achieve oxidation during heat treatment and remove free carbon are also feasible.

[0033] Preferably, in step (5), the temperature of the carbon removal heat treatment is 550-950°C, more preferably 600-900°C, and the temperature is maintained for 1-20 hours, more preferably 5-15 hours.

[0034] The adoption of the above technical solution has a better effect of removing free carbon.

[0035] Preferably, in step (5), the heating rate is 5 to 50°C / min, more preferably 10 to 30°C / min.

[0036] The adoption of the above technical solution has a better effect of removing free carbon.

[0037] Preferably, in step (6), the concentration of hydrofluoric acid is 10-50% (g / g), more preferably 15-30% (g / g).

[0038] By adopting the above technical solution, a better etching effect is achieved.

[0039] Preferably, in step (6), the immersion time is 3 to 50 hours, more preferably 10 to 30 hours.

[0040] By adopting the above technical solution, a better etching effect is achieved.

[0041] Precursor conversion technology is an important method for preparing non-oxide ceramics. This method is based on the synthesis of ceramic precursors, and finally obtains non-oxide ceramics through crosslinking and high-temperature inorganic conversion. Due to the excellent process characteristics of the precursor polymer and the adjustable components, the precursor conversion technology has become the most effective and widely used preparation method for preparing non-oxide ceramics with special structures, properties and compositions. The present invention combines the precursor conversion technology with the template technology. In the process of using the template beads to occupy the position and the pores after removal, the PCS immersed in the template is oxidatively crosslinked, thereby introducing oxygen into the PCS structure, and then converted into C / SiC / SiO2, C / SiC / SiOC or C / SiC / SiO2 / SiOC through high-temperature inorganic conversion. Finally, C is removed by air oxidation and SiO2 or SiOC is removed by etching in HF solution, thereby preparing a three-dimensional ordered porous SiC ceramic with a dual-type pore structure.

[0042] The dual-type pore structure of the present invention is mainly formed by the following ways: 1) the pores are formed after the small ball template occupies the site and is removed, and 2) the pores are formed after the C, SiO2 and SiOC generated by the oxidation cross-linking-ceramicization of PCS are removed.

[0043] SiC ceramic materials have excellent oxidation resistance, corrosion resistance and thermal stability. The present invention prepares a three-dimensional ordered porous SiC ceramic with a dual-type pore structure, which lays an important foundation for the application of three-dimensional ordered porous materials with different pore diameters and pore types in high temperature, oxidation and corrosion environments.

[0044] Beneficial effects of the present invention: The invention can prepare a three-dimensionally ordered porous SiC ceramic with a dual-type pore structure, a high specific surface area, and can make the three-dimensionally ordered porous material usable in high-temperature, oxidative, and corrosive environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 1 is the N2 adsorption-desorption isothermal characteristic curve and pore size distribution curve of the porous SiC ceramic obtained in Example 1 of the present invention, and the inset is the pore size distribution curve.

[0046] Figure 2 This is a SEM photograph of the porous SiC ceramic prepared using 350 nanometer SiO2 balls as a template in Example 2 of the present invention.

[0047] Figure 3 This is a TEM photograph of the porous SiC ceramic prepared using 350 nanometer SiO2 balls as a template in Example 2 of the present invention. DETAILED DESCRIPTION

[0048] The present invention is further described below in conjunction with embodiments and drawings.

[0049] The raw materials used in the embodiments of the present invention are all obtained through conventional commercial channels. Example 1

[0050] The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure in this embodiment comprises the following steps: (1) Under the assistance of ultrasound, 3 g of SiO2 nanospheres with a uniform particle size of 500 nm were uniformly dispersed in 12 g of ethanol (the weight ratio of SiO2 nanospheres was 25%). The dispersion was then placed in a flat-bottomed vertical glass tube, and the SiO2 nanospheres were naturally deposited to self-assemble into a three-dimensional ordered sphere template. The solvent was removed and dried. (2) Place a 30% (g / g) PCS THF dispersion (PCS dosage 4 g) in a glass bottle containing the template, immerse for 24 hours, and then remove the solvent by vacuum distillation; the volume of PCS used is equivalent to the volume of the template; (3) The mixture was then cross-linked in air at 190°C for 15 h; (4) The obtained product was cracked at 1250°C in an Ar atmosphere (heating rate of 20°C / min) and kept at 1250°C for 0.5 h; (5) The obtained product was first treated at 650°C in air for 5 h (heating rate of 20°C / min); (6) The product was immersed in 30% (g / g) hydrofluoric acid for 24 h, and the target ceramic was obtained after washing and drying.

[0051] The adsorption-desorption curve of the SiC ceramic product obtained in this example is as follows: Figure 1 As shown, the BET specific surface area was measured to be 352 m 2 / g. Example 2

[0052] The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure in this embodiment comprises the following steps: (1) Under the assistance of ultrasound, 3 g of SiO2 nanospheres with a uniform particle size of 350 nm were uniformly dispersed in 12 g of ethanol (the weight ratio of SiO2 nanospheres was 25%). The dispersion was then placed in a flat-bottomed vertical glass tube, and the SiO2 nanospheres were naturally deposited to self-assemble into a three-dimensional ordered sphere template. The solvent was removed and dried. (2) Place a 30% (g / g) PCS THF dispersion (PCS dosage 4 g) in a glass bottle containing the template, immerse for 24 hours, and then remove the solvent by vacuum distillation. The volume of PCS used is equivalent to the volume of the template; (3) The mixture was then cross-linked in air at 190°C for 15 h; (4) The resulting product was then cracked at 1250 °C in an Ar atmosphere (heating rate of 20 °C / min) and kept at 1250 °C for 0.5 h; (5) The obtained product was first treated at 650°C in air for 5 h (heating rate of 20°C / min); (6) The product was immersed in 30% (g / g) hydrofluoric acid for 24 h, and the target ceramic was obtained after washing and drying.

[0053] The SEM and TEM photos of the SiC ceramic product obtained in this example are as follows: Figure 2 , Figure 3 As shown, the pore structure formed by the ball template is clearly visible.

[0054] The BET specific surface area of ​​the SiC ceramic product obtained in this embodiment is measured to be 443 m 2 / g. Example 3

[0055] The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure in this embodiment comprises the following steps: (1) Under the assistance of ultrasound, 3 g of SiO2 nanospheres with a uniform particle size of 500 nm were uniformly dispersed in 12 g of ethanol (the weight ratio of SiO2 nanospheres was 25%). The dispersion was then placed in a flat-bottomed vertical glass tube, and the SiO2 nanospheres were naturally deposited to self-assemble into a three-dimensional ordered sphere template. The solvent was removed and dried. (2) Place a 30% (g / g) PCS THF dispersion (PCS dosage 4 g) in a glass bottle containing the template, immerse for 24 hours, and then remove the solvent by vacuum distillation; the volume of PCS used is equivalent to the volume of the template; (3) the mixture was then cross-linked in air at 200°C for 20 h; (4) The obtained product was cracked at 1250°C in an Ar atmosphere (heating rate of 20°C / min) and kept at 1250°C for 0.5 h; (5) The obtained product was first treated at 650°C in air for 5 h (heating rate of 20°C / min); (6) The product was immersed in 30% (g / g) hydrofluoric acid for 24 h, and the target ceramic was obtained after washing and drying.

[0056] The BET specific surface area of ​​the SiC ceramic product obtained in this embodiment is measured to be 385 m 2 / g.

Claims

1. A method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure, characterized in that: The following steps are involved: (1) Dispersing SiO2 nanospheres with uniform diameter uniformly in a solvent, allowing the SiO2 nanospheres to self-assemble into a three-dimensional ordered template through natural deposition, removing the solvent and drying; (2) pouring a polycarbosilane precursor dispersion into the container where the template is located, immersing the template, and removing the solvent; (3) cross-linking the product obtained in step (2) in an oxygen-containing atmosphere to introduce oxygen during the cross-linking process; (4) The product obtained in step (3) is heat treated in an inert atmosphere to ceramicize it; (5) The product obtained in step (4) is heat treated in an oxidizing atmosphere to remove free carbon; (6) The product obtained in step (5) is immersed in hydrofluoric acid to etch away some components in the template and the ceramic product, and then cleaned to obtain the target ceramic.

2. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to claim 1, characterized in that: In step (1), ultrasound is used to assist the dispersion of SiO2 nanospheres; the particle size of the SiO2 nanospheres is less than 1000 nm.

3. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to claim 1 or 2, characterized in that: In step (1), the solvent is anhydrous ethanol.

4. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 3, characterized in that: In step (1), the weight ratio of SiO2 nanospheres to solvent is 5-30:

100.

5. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 4, characterized in that: In step (2), the solvent in the polycarbosilane precursor dispersion is tetrahydrofuran; the concentration of the polycarbosilane precursor dispersion is 10-80%, in g / g.

6. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 5, characterized in that: In step (2), the immersion time is 5 to 30 hours.

7. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 6, characterized in that: In step (3), the oxygen-containing atmosphere is an air atmosphere; the temperature during cross-linking is 150-250° C., and the cross-linking time is 2-30 hours.

8. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 7, characterized in that: In step (4), the inert atmosphere is an argon atmosphere; the temperature of the ceramic heat treatment is 800-1650°C, and the temperature is kept at this temperature for 0.5-5h; the heating rate is 5-50°C / min.

9. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 8, characterized in that: In step (5), the oxidizing atmosphere is an air atmosphere; the temperature of the carbon removal heat treatment is 550-950°C, and the temperature is maintained for 1-20 hours; the heating rate is 5-50°C / min.

10. The method for preparing three-dimensional ordered porous silicon carbide having a dual-type pore structure according to any one of claims 1 to 9, characterized in that: In step (6), the concentration of hydrofluoric acid is 10-50%, expressed in g / g; and the immersion time is 3-50 h.

Citation Information

Patent Citations

  • Preparation method of a Cf / SiC composite ordered porous ceramic joint

    CN102167613A

  • Connection method of Cf / SiC composite

    CN102167614A

  • Synthesis Of Ordered Mesoporous Carbon-Silicon Nanocomposites

    US20100040834A1

Cited By

  • Ytterbium oxide modified silicon carbide-zirconium carbide multiphase ceramic material as well as preparation method and application thereof

    CN120398553A