Near-infrared response self-repairing photocuring polyurethane material as well as preparation method and application thereof
By introducing thiocarbamate bonds and polydopamine nanoparticles into photocured polyurethane materials, the self-healing of the material is achieved by using near-infrared light, the problem of insufficient self-healing ability in the prior art is solved, and the fracture healing of the material is improved and degradation performance have expanded its application in the field of high-end materials.
Patent Information
- Application Number
- CN202310618694.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-29
AI Technical Summary
The existing photocured polyurethane materials have poor self-repair capabilities, and the traditional thermal repair methods consume high energy and do not have local repair capabilities for materials, which limits the application of materials in high-end fields.
The preparation method of near-infrared response self-healing photocurable polyurethane material is adopted, and the introduction of thiocarbamate bonds into the polyurethane oligomer and combined with polydopamine nanoparticles and photoinitiator is achieved by stimulating ultraviolet light or near-infrared light. Self-healing of materials.
It improves the self-healing ability of the material, realizes fracture healing and local fixed-point repair of the material, reduces energy consumption, and imparts the degradable properties of the material, broadens its application in flexible conductive materials and photoactuated materials.
Smart Images

Figure CN119039734A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and specifically to a near-infrared responsive self-repairing photocurable polyurethane material and a preparation method and application thereof. Background Art
[0002] Photocurable polyurethane materials are widely used at this stage because the urethane bonds on the polymer chain segments have strong polarity and hydrogen bonds exist between the chain segments, which can form effective physical cross-linking points to enhance the mechanical properties of the material. They also have excellent chemical resistance and high and low temperature resistance. However, due to the problem that the internal stress of the material cannot be well released during the photocuring process, weak points and defects are prone to appear inside the material. These drawbacks will cause the material to be easily damaged and broken during use, thereby limiting the application of photocurable polyurethane materials in some high-end fields. Giving photocurable polyurethane materials self-healing capabilities can effectively solve this problem. Therefore, designing and preparing new self-healing photocurable polyurethane materials is of great significance to broadening the application range of photocurable polyurethane materials.
[0003] Thiocarbamate bonds are a new type of reversible covalent bond that has been studied in recent years. Since the construction of thiocarbamate bonds has the advantages of abundant raw materials, simple preparation, and high reaction yield, and at the same time, thiocarbamate bonds can be broken in alcohol solvents to give the material degradable properties, it has shown great application potential in the fields of self-healing materials and degradable materials. Therefore, applying thiocarbamate bonds to photocurable polyurethane materials is expected to give the materials excellent repair properties, increase the service life of the materials, and make the materials degradable.
[0004] However, there are few reports on photocurable self-healing materials based on thiocarbamate bonds at present, and most of the self-healing materials with thiocarbamate bonds are repaired by heating. The thermal repair method will cause energy waste; and during the repair process, the entire material needs to be heated, so that the undamaged parts are also heated, causing aging of the material and reducing the service life of the material. Light, as a stimulus source, is cheap and a clean energy source. It does not introduce any chemicals during the repair process and will not cause damage to the material. In addition, light can control the self-healing process remotely and in real time, and can perform local fixed-point repairs on the material. It is one of the hot spots in the research of self-healing materials.
[0005] The Chinese patent application document with publication number CN113788927A discloses a self-healing polyurethane material and its preparation method. A step-by-step preparation method is adopted to first obtain a disulfide bond-containing macromolecular diol, and then use the disulfide bond-containing macromolecular diol as a raw material to prepare a disulfide bond-containing polyurethane solution. At the same time, a conventional macromolecular diol is used as a raw material to prepare a hard segment polyurethane solution. Finally, the two polyurethane solutions are mixed and cast in a certain proportion to obtain a self-healing polyurethane material with excellent mechanical properties. The self-healing polyurethane material provided by this patent can be applied to flexible electronic devices. However, the self-healing ability of this material is poor, so it needs to be further improved. Summary of the invention
[0006] The technical problem to be solved by the present invention is how to solve the problem that the existing polyurethane material has poor self-repairing ability.
[0007] The present invention solves the above technical problems through the following technical means:
[0008] The first aspect of the present invention provides a method for preparing a near-infrared responsive self-repairing photocurable polyurethane material, comprising the following steps:
[0009] (1) Preparation of polyurethane oligomers containing thiocarbamate bonds:
[0010] The macromolecular chain extender, catalyst 1, and diisocyanate are heated for reaction; when the residual amount of -NCO is 50%, a small molecule alcohol chain extender is dissolved in an organic solvent 1, and then added dropwise to the reaction system to continue the reaction; then a small molecule thiol chain extender and catalyst 2 are dissolved in an organic solvent 1, and then added dropwise to the reaction system to continue the reaction; a capping agent is then added to the reaction system to continue the reaction until the amount of -NCO is 0, and the organic solvent 1 is removed to obtain a polyurethane oligomer containing a thiocarbamate bond;
[0011] (2) Preparation of polydopamine nanoparticles (PDA):
[0012] The organic solvent 2, the solvent 3 and water are mixed, and then dopamine hydrochloride (DA) monomer is added thereto, heated for reaction, centrifuged, the lower layer of solid is taken out, and dried to obtain polydopamine nanoparticles (PDA);
[0013] (3) The polyurethane oligomer containing thiocarbamate bonds and polydopamine nanoparticles (PDA) prepared above are mixed with an acrylate monomer and a photoinitiator, and cured under ultraviolet light to obtain a near-infrared light-responsive self-healing photocurable polyurethane material based on thiocarbamate bonds.
[0014] The macromolecular chain extender is selected from one or more of polyether diols or polyether polyols with a molecular weight of 200 to 10,000, and polyester diols or polyester polyols with a molecular weight of 1,000 to 10,000.
[0015] Beneficial effects: The present invention first prepares a polyurethane oligomer containing a thiocarbamate bond; then, mixes it with polydopamine nanoparticles, commercial acrylate monomers and a photoinitiator; finally, under ultraviolet light irradiation, a near-infrared light-responsive self-healing photocurable polyurethane material based on the thiocarbamate bond is obtained, and the healing of the damaged part of the material is achieved through the photothermal conversion ability of the polydopamine nanoparticles under near-infrared light irradiation, thereby improving the self-healing ability of the material.
[0016] Preferably, the macromolecular chain extender is polyethylene glycol with a molecular weight of 1000 to 2000.
[0017] The diisocyanate is selected from one or more of 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), trimethyl 1,6-hexamethylene diisocyanate (TMHDI), hydrogenated 4,4-diphenylmethane diisocyanate (HMDI), trans-cyclohexane isocyanate (CHDI), diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), dicyclohexylmethane diisocyanate (HMDI), and methylcyclohexyl diisocyanate (HTDI).
[0018] Preferably, the diisocyanate is isophorone diisocyanate (IPDI).
[0019] The small molecule alcohol chain extender is selected from C2-C16 dihydric or polyhydric alcohols.
[0020] Preferably, the small molecule alcohol chain extender is a C2-C16 diol.
[0021] Preferably, the small molecule alcohol chain extender is a C2-C16 straight chain diol.
[0022] Preferably, the small molecule alcohol chain extender is a C2-C6 straight chain diol.
[0023] The small molecule mercaptan chain extender is selected from C2-C16 dihydric or polyhydric mercaptan.
[0024] Preferably, the small molecule thiol chain extender is a C2-C16 dihydric thiol.
[0025] Preferably, the small molecule thiol chain extender is a C2-C16 straight chain dihydric thiol.
[0026] Preferably, the small molecule thiol chain extender is a C2-C6 straight chain dihydric thiol.
[0027] The catalyst 1 and the catalyst 2 are both selected from one or more of an organic bismuth catalyst, an organic tin catalyst, and an amine catalyst.
[0028] Preferably, the organic bismuth catalyst is selected from one or more of bismuth isooctanoate, bismuth laurate, bismuth neodecanoate, and bismuth cyclopentanoate.
[0029] Preferably, the organotin catalyst is selected from one or more of monobutyltin oxide, dibutyltin oxide, dibutyltin diacetate and dibutyltin dilaurate.
[0030] Preferably, the amine catalyst is selected from one or more of triethylamine, 1,5-diazabicyclo[4,3,0]-5-nonene, and N,N-diisopropylethylamine.
[0031] Preferably, the catalyst 1 is dibutyltin dilaurate.
[0032] Preferably, the catalyst 2 is 1,5-diazabicyclo[4,3,0]-5-nonene.
[0033] Preferably, the organic solvent 1 is selected from one or more of dimethyl sulfoxide, acetone, dioxane, tetrahydrofuran, methyl formate, methyl ethyl ketone, butyl acetate, propylene glycol methyl ether acetate, ethyl acetate and isopropyl ether.
[0034] Preferably, the organic solvent 1 is tetrahydrofuran.
[0035] Preferably, the end-capping agent is one or more of hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).
[0036] Preferably, in the reaction system of step (1), the ratio of the molar number of -NCO groups of the isocyanate raw material to the total molar number of hydroxyl groups and mercapto groups in the system is 1:1.
[0037] Preferably, the number average molecular weight of the polyurethane oligomer containing thiol carbamate bonds prepared in step (1) is 7000-15000; the content of thiol carbamate bonds in the polyurethane oligomer containing thiol carbamate bonds is 0.5wt%-10wt%.
[0038] Preferably, the organic solvent 2 is an alcohol compound. Preferably, the organic solvent 2 is anhydrous ethanol.
[0039] Preferably, the solvent 3 is an alkaline substance. Preferably, the solvent 3 is aqueous ammonia.
[0040] Preferably, the acrylic acid ester monomer is one or more of monofunctional, difunctional or multifunctional acrylic acid ester monomer, methacrylic acid ester monomer, acrylic acid, acrylamide, methacrylic acid and methacrylamide.
[0041] Preferably, the photoinitiator is selected from a mixture of one or more of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one (2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), methyl phenylacetoate (MBF), diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO), and bis (2,4,6-trimethylbenzoyl) phenyl phosphine oxide (BAPO).
[0042] The second aspect of the present invention proposes a near-infrared light-stimulated self-repairing photocurable polyurethane material prepared by the above-mentioned preparation method.
[0043] The near-infrared responsive self-repairing photocurable polyurethane material consists of two parts; the first component: 10-60wt% of polyurethane oligomer containing thiocarbamate bonds; 40-90wt% of active diluent monomer; the second component (based on the first component as 100%): 0.5-5wt% of photoinitiator and 0.5-5wt% of polydopamine nanoparticles.
[0044] Beneficial effects: The material has a fracture stress of 0.5-3MPa and a fracture elongation of 100-1500%; it has good self-repairing properties under 980nm near-infrared irradiation; and it can be degraded in alcohol solvents.
[0045] The third aspect of the present invention proposes the use of the near-infrared light-stimulated self-repairing photocurable polyurethane material prepared by the above preparation method in flexible conductive materials and photoactuated materials.
[0046] Synthesis principle
[0047] The following takes the preparation of a near-infrared light-responsive self-healing photocurable polyurethane material using preferred raw materials as an example to explain the synthesis principle.
[0048] 1. First, weigh the raw materials polyethylene glycol-1000, isophorone diisocyanate and catalyst dibutyltin dilaurate and add them to the flask. Replace the reaction atmosphere with nitrogen atmosphere by vacuuming and passing nitrogen to prevent the influence of water vapor in the air on the reaction system, and then place the system at 80°C for reaction. After reacting for 4 hours, weigh 1,4-butanediol and dissolve it in anhydrous tetrahydrofuran (THF), slowly add it to the three-necked flask with a syringe, and continue to react at 80°C for 4 hours after the addition is complete until the -OH reaction is complete. Then weigh 1,3-propanedithiol and dissolve it in anhydrous THF, then add 1,5-diazabicyclo[4.3.0]-5-nonene, take it out with a syringe and slowly add it to the three-necked flask, and continue to react at 80°C for 5 hours after the addition is complete. Finally, weigh hydroxyethyl acrylate and dissolve it in anhydrous THF, slowly add it to the three-necked flask, and end the reaction 5 hours after the addition is complete. After removing tetrahydrofuran, the polyurethane oligomer PETU-B3S4 can be obtained. In the reaction system, the ratio of the molar number of -NCO groups of the isocyanate raw material to the total molar number of hydroxyl groups and mercapto groups in the system is 1:1.
[0049] The reaction formula is as follows:
[0050]
[0051] The infrared spectrum, nuclear magnetic hydrogen spectrum and Raman spectrum of compound PETU-B3S4 are shown in the attached Figure 1 , Attachment Figure 2 and attached Figure 3 , the relevant data are as follows:
[0052] FTIR(KBr,cm -1 )3336(-NHCOS-and-NHCOO-),2954and 2865(-CH3 and-CH2-),1716(-C=O),812(-CH=CH2).
[0053] 1 H NMR (400MHz, Chloroform-d) δ6.67-5.90(-OOCCH=CH2),5.40-4.98(-NHCOS-,-NHCOO-),4.32-3.98(-NHCOOCH2-,-O-CH2-CH2-OOCCH=CH2),3.64(-CH2 of PEG-1000,-CH-NHCOO,-CH-NHCOS),3.01-2.77(-CH2-NHCOO,-CH2-NHCOS,-NHCOS-CH2),1.92-1.79(-CH2 ofIPDI,-NHCOOCH2-CH2),1.07-0.86(-CH3 of IPDI).
[0054] The molecular weight test results of the compound PETU-B3S4 are as follows: number average molecular weight / Mn: 14052, dispersion index (PDI): 2.46.
[0055] 2. Take anhydrous CH3CH2OH, ammonia water and H2O respectively and mix them together. Then add dopamine hydrochloride (DA) monomer, the reaction system changes from colorless to dark brown, and react at 30℃ for 28h. After the reaction, centrifuge the solution, take the lower layer of solid and dry it in a vacuum oven at 65℃ for 6h to obtain the product PDA. The infrared spectrum of the product PDA is shown in the attached figure. Fig.10 .
[0056] 3. First, weigh a certain mass of PDA, dissolve it in anhydrous tetrahydrofuran (THF), and ultrasonicate it for a certain period of time to evenly disperse it in THF. After the ultrasonication, mix it with the PETU-B3S4 oligomer, continue ultrasonication to mix the PDA and oligomer evenly, and then remove THF. The oligomer evenly mixed with PDA is mixed with other monomers hydroxyethyl acrylate (HEA), isobornyl acrylate (IBOA) and photoinitiator BAPO to prepare a photosensitive liquid. Spread the prepared photosensitive liquid evenly on a dumbbell-shaped polytetrafluoroethylene mold, and then cover it with a layer of polyvinyl butyral film to prevent the photosensitive liquid from contacting with the air to cause oxygen inhibition and incomplete curing, and then place it under a UV lamp to cure to obtain a light-cured polyurethane material.
[0057] The advantages of the present invention are:
[0058] 1. The present invention first prepares a polyurethane oligomer containing a thiocarbamate bond; then, mixes the oligomer with polydopamine nanoparticles, an acrylate monomer and a photoinitiator; finally, under ultraviolet light irradiation, a near-infrared light-responsive self-healing photocurable polyurethane material based on the thiocarbamate bond is obtained, and the healing of the damaged part of the material is achieved through the photothermal conversion ability of the polydopamine nanoparticles under near-infrared light irradiation, thereby improving the self-healing ability of the material.
[0059] 2. The material has excellent self-repairing ability and photo-actuated effect under 980nm near-infrared stimulation;
[0060] 3. The material also has good degradation performance, which effectively solves the problem of serious environmental pollution caused by material disposal. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 is the infrared spectrum of PETU-B3S4 prepared in Example 1;
[0062] Figure 2 is the H NMR spectrum of PETU-B3S4 prepared in Example 1;
[0063] Figure 3 is the Raman spectrum of PETU-B3S4 prepared in Example 1;
[0064] Figure 4 is the infrared spectrum of PTTU-B3S4 prepared in Example 2;
[0065] Figure 5 is the H NMR spectrum of PTTU-B3S4 prepared in Example 2;
[0066] Figure 6 is the Raman spectrum of PTTU-B3S4 prepared in Example 2;
[0067] Figure 7 is the infrared spectrum of PPTU-B3S4 prepared in Example 3;
[0068] Figure 8 is the H NMR spectrum of PPTU-B3S4 prepared in Example 3;
[0069] Fig. 9 is the Raman spectrum of PPTU-B3S4 prepared in Example 3;
[0070] Fig.10 is the infrared spectrum of PDA prepared in Example 4;
[0071] Fig.11 is a schematic diagram of the photoactivation process of (PETU-B3S4)3-HI-1.0 prepared in Example 5;
[0072] Fig.12 This is a schematic diagram of the application of (PETU-B3S4)3-HI-1.0 prepared in Example 5 in the field of flexible electronic substrates. DETAILED DESCRIPTION
[0073] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0074] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0075] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0076] Source of raw materials
[0077] Isobornyl acrylate (IBOA, AR): Tianjin Xiens Biochemical Technology Co., Ltd.
[0078] Hydroxyethyl acrylate (HEA, AR): Tianjin Xiens Biochemical Technology Co., Ltd.
[0079] 1,3-Propanedithiol (AR): Tianjin Xiens Biochemical Technology Co., Ltd.
[0080] Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (BAPO, AR): Huaian Shuangying Chemical Co., Ltd. Isophorone diisocyanate (IPDI, AR): Anaiji (Shanghai) Pharmaceutical Chemical Co., Ltd.
[0081] Polyethylene glycol-1000 (PEG-1000, AR): Anaiji (Shanghai) Pharmaceutical Chemistry Co., Ltd.
[0082] Polytetrahydrofuran-1000 (PTMG-1000, AR): Anaiji (Shanghai) Pharmaceutical Chemical Co., Ltd.
[0083] Polypropylene glycol-1000 (PPG-1000, AR): Anaiji (Shanghai) Pharmaceutical Chemical Co., Ltd.
[0084] n-Butyltin dilaurate (DBTDL, AR): Anaiji (Shanghai) Pharmaceutical Chemical Co., Ltd.
[0085] Tetrahydrofuran (THF, AR): Anaiji (Shanghai) Pharmaceutical Chemistry Co., Ltd.
[0086] Anhydrous methanol (AR, AR): Anaiji (Shanghai) Pharmaceutical Chemistry Co., Ltd.
[0087] N,N-Dimethylformamide (DMF, AR): Fuchen (Tianjin) Chemical Reagent Co., Ltd.
[0088] 1,4-Butanediol (BDO, AR): Anaiji (Shanghai) Pharmaceutical Chemical Co., Ltd.
[0089] 1,5-Diazabicyclo[4,3,0]-5-nonene (DBN, AR): Anaiji (Shanghai) Pharmaceutical Chemistry Co., Ltd. Ammonia (AR): San Chemical Technology Co., Ltd.
[0090] Dopamine hydrochloride (DA, AR): Tianjin Xiens Biochemical Technology Co., Ltd.
[0091] Anhydrous ethanol (AR): Anaiji (Shanghai) Pharmaceutical Chemistry Co., Ltd.
[0092] Nano silver glue: Nanjing Xilite Adhesive Co., Ltd.
[0093] Example 1
[0094] Synthesis of photocurable polyurethane oligomers containing thiocarbamate bonds:
[0095] Step 1: Add 4.44 g (20 mmol) of isophorone diisocyanate, 10 g (10 mmol) of polyethylene glycol-1000 and 0.02 g of dibutyltin dilaurate (DBTDL) into a 250 mL three-necked flask. Then install a nitrogen valve, a thermometer and a condenser on the three-necked flask, and change the reaction system into a nitrogen atmosphere by vacuuming and passing nitrogen. Heat the oil pan to 80°C and react for 4 hours.
[0096] Step 2: Dissolve 0.27 g (3 mmol) of 1,4-butanediol in 20 mL of anhydrous tetrahydrofuran solution, and slowly add it dropwise into the three-necked flask via a syringe to continue the reaction for 4 hours.
[0097] Step 3: Dissolve 0.43 g (4 mmol) of 1,3-propanedithiol in 20 mL of anhydrous tetrahydrofuran solution, then add 0.01 g of 1,5-diazabicyclo[4.3.0]-5-nonene as a catalyst to the tetrahydrofuran solution, slowly drip it into the three-necked flask through a syringe and continue the reaction for 5 hours.
[0098] Step 4: Add 0.696 g (6 mmol) of hydroxyethyl acrylate (HEA) to the system, continue the reaction for 4 h, and remove the tetrahydrofuran solvent to obtain the product PETU-B3S4.
[0099] The reaction formula is as follows:
[0100]
[0101] The infrared spectrum, nuclear magnetic hydrogen spectrum and Raman spectrum of compound PETU-B3S4 are shown in the attached Figure 1 , Attachment Figure 2 and attached Figure 3 , the relevant data are as follows:
[0102] FTIR(KBr,cm -1 )3336(-NHCOS-and-NHCOO-),2954and 2865(-CH3 and-CH2-),1716(-C=O),812(-CH=CH2).
[0103] 1H NMR (400MHz, Chloroform-d) δ6.67-5.90(-OOCCH=CH2),5.40-4.98(-NHCOS-,-NHCOO-),4.32-3.98(-NHCOOCH2-,-O-CH2-CH2-OOCCH=CH2),3.64(-CH2 of PEG-1000,-CH-NHCOO,-CH-NHCOS),3.01-2.77(-CH2-NHCOO,-CH2-NHCOS,-NHCOS-CH2),1.92-1.79(-CH2 ofIPDI,-NHCOOCH2-CH2),1.07-0.86(-CH3 of IPDI).
[0104] The molecular weight test results of the compound PETU-B3S4 are as follows: number average molecular weight / Mn: 14052, dispersion index (PDI): 2.46.
[0105] Example 2
[0106] The steps of Example 1 were repeated, except that the raw material polyethylene glycol-1000 used in the first step was replaced with polytetrahydrofuran-1000, and the added amount was 10 mmol (10 g). The reaction formula is as follows:
[0107]
[0108] The infrared spectrum, nuclear magnetic hydrogen spectrum and Raman spectrum of the compound PTTU-B3S4 are shown in the attached Figure 4 , Attachment Figure 5 and attached Figure 6 , the relevant data are as follows:
[0109] FTIR(KBr,cm -1 )3331(-NHCOS-and-NHCOO-),2964and 2873(-CH3 and-CH2-),1238(COC),1715(-C=O),810(-CH=CH2).
[0110] 1H NMR (400MHz, Chloroform-d) δ6.50-5.83(-CH=CH2),5.05-4.81(-NHCOO,-NHCOS),4.16-3.80(-NHCOOCH2,-CH2-OOCCH=CH2),3.59-3.32(-O-CH2 of PTMG-1000,-CH-NHCOO,-CH-NHCOS),3.06-2.88(CH2-NHCOO,CH2-NHCOS,-NHCOS-CH2),1.77-1.54(CH2 ofIPDI and PTMG,-NHCOOCH2-CH2),1.11-0.82(-CH3 of IPDI).
[0111] The molecular weight test results of the compound PTTU-B3S4 are as follows: number average molecular weight / Mn: 14399, dispersion index (PDI): 2.36.
[0112] Example 3
[0113] The steps of Example 1 were repeated, except that the raw material polyethylene glycol-1000 used in the first step was replaced with polypropylene glycol-1000, and the added amount was 10 mmol (10 g). The reaction formula is as follows:
[0114]
[0115] The infrared spectrum, nuclear magnetic hydrogen spectrum and Raman spectrum of the compound PPTU-B3S4 are shown in the attached Figure 7 , Attachment Figure 8 and attached Fig. 9 , the relevant data are as follows:
[0116] FTIR(KBr,cm -1 )3335(-NHCOS-and-NHCOO-),2968and 2869(-CH3 and-CH2-),1240(COC),1717(-C=O),813(-CH=CH2).
[0117] 1H NMR (400MHz, Chloroform-d) δ6.48-5.85(-CH=CH2),5.00-4.60(-NHCOO,-NHCOS),4.37-3.92(-NHCOOCH2,-CH2-OOCCH=CH2),3.70-3.29(CH2 and CH of PPG-1000,-CH-NHCOO,-CH-NHCOS),3.01-2.77(CH2-NHCOO,CH2-NHCOS,-NHCOS-CH2),1.89-1.81(CH2 ofIPDI,-NHCOOCH2-CH2),1.27-0.80(-CH3 of IPDI and PPG).
[0118] The molecular weight test results of the compound PPTU-B3S4 are as follows: number average molecular weight / Mn: 14829, dispersion index (PDI): 2.42.
[0119] Example 4
[0120] Preparation of polydopamine nanoparticles (PDA):
[0121] Take anhydrous CH3CH2OH (2 mL), ammonia (1 mL) and H2O (5 mL) respectively and mix them together. Then add 0.5 g of dopamine hydrochloride (DA) monomer, the reaction system changes from colorless to dark brown, and reacts at 30°C for 28 hours. After the reaction is completed, centrifuge the solution, take out the lower layer of solid and dry it in a vacuum oven at 65°C for 6 hours to obtain the product PDA. See the attached infrared spectrum for its attached Fig.10 .
[0122] Example 5
[0123] The purpose of this example is to illustrate that the photocurable polyurethane oligomer PETU-B3S4 containing thiocarbamate bonds prepared in Example 1 and the PDA prepared in Example 5 can be used to prepare a near-infrared responsive self-healing photocurable polyurethane material (PETU-B3S4) 3-HI-1.0.
[0124] First, weigh PDA and dissolve it in 10 mL of anhydrous THF. Ultrasonicate for a certain period of time to evenly disperse it in THF. After the ultrasound is over, mix it with the PETU-B3S4 oligomer, continue to ultrasonicate to mix the PDA and oligomer evenly, and then remove THF. The oligomer mixed evenly with PDA is mixed evenly with other monomers hydroxyethyl acrylate (HEA), isobornyl acrylate (IBOA) and photoinitiator BAPO to prepare a photosensitive solution for use. The mass ratio of PETU-B3S4:HEA:IBOA:PDA:BAPO in the photosensitive solution is 60:20:20:1:1. Spread the prepared photosensitive solution evenly on a dumbbell-shaped polytetrafluoroethylene mold, and then cover it with a layer of polyvinyl butyral film to prevent the photosensitive solution from contacting with air and causing oxygen inhibition, resulting in incomplete curing, and then place it under a UV lamp (wavelength 365nm, light intensity 100mW cm -2 ) and cured for 20 min to obtain near-infrared responsive self-healing photocurable polyurethane material (PETU-B3S4) 3-HI-1.0.
[0125] The self-healing photocurable material (PETU-B3S4) 3-HI-1.0 was cut in the middle using a razor blade, and then squeezed with fingers to make the fracture surfaces contact each other for at least 1 min; then it was placed under 1.5 W cm -2 The repair was carried out by irradiating the sample with a 980nm near-infrared lamp for 30 minutes. The mechanical properties of the initial material and the repaired material were tested using an electronic material testing machine, and the repair efficiency was calculated based on the ratio of the fracture stress and elongation at break of the repaired sample to the initial sample.
[0126] The near-infrared responsive self-healing photocurable polyurethane material (PETU-B3S4) 3-HI-1.0 has an elongation at break of 1021%, a fracture stress of 1.06 MPa, a repair efficiency of elongation at break of 91%, and a repair efficiency of fracture stress of 91%.
[0127] Example 6
[0128] The steps of Example 5 were repeated to prepare a near-infrared responsive self-healing photocurable polyurethane material (PTTU-B3S4) 3-HI-1.0. The difference from Example 5 was that "PETU-B3S4" was replaced by "PTTU-B3S4" of Example 2.
[0129] The near-infrared responsive self-healing photocurable polyurethane material (PTTU-B3S4) 3-HI-1.0 has an elongation at break of 1425%, a fracture stress of 1.83 MPa, a repair efficiency of elongation at break of 90%, and a repair efficiency of fracture stress of 91%.
[0130] Example 7
[0131] Repeat the steps of Example 5 to prepare a near-infrared responsive self-healing photocurable polyurethane material (PPTU-B3S4) 3-HI-1.0. The difference from Example 5 is that "PETU-B3S4" is replaced by "PPTU-B3S4" of Example 3.
[0132] The near-infrared responsive self-healing photocurable polyurethane material (PPTU-B3S4) 3-HI-1.0 has an elongation at break of 1095%, a fracture stress of 1.01 MPa, a repair efficiency of elongation at break of 90%, and a repair efficiency of fracture stress of 90%.
[0133] Example 8
[0134] The purpose of this example is to illustrate that the near-infrared light-responsive self-repairing photocurable polyurethane materials prepared in Examples 5, 6, and 7 have degradable capabilities. Take a photocurable film with a mass of m0 and soak it in a mixed solution of 20 mL of methanol and N,N-dimethylformamide containing 0.5 mL of DBN. Soak it at 100°C for 0 h, 2 h, 4 h, 6 h, and 7 h, respectively. After drying the residue, weigh its residual mass m x , the degradation rate of the photocured film at different times was calculated by formula (1). The degradation rates of the self-healing materials at different times are shown in Table 1. The data in Table 1 show that the degradation rate of the cured film increases with the increase of immersion time, and is completely degraded after immersion for 7 hours. This shows that the cured film has good degradability.
[0135]
[0136] Table 1. Degradation rate of cured films
[0137]
[0138] Example 9
[0139] The purpose of this example is to illustrate that the near-infrared light responsive self-healing photocurable polyurethane material prepared in Example 5 has certain photo-actuated properties. We used the dumbbell-shaped material (PETU-B3S4) 3-HI-1.0, through a heating and cooling fixation process, to produce a shape with a bending angle of 50°, and then placed it under 980nm NIR irradiation for 10 seconds. The material then recovered most of its shape. After irradiation for 60 seconds, the material was basically fully unfolded and restored to shape. Based on this function, this type of material can be used in the field of remote control unloading of objects. After the hook loaded with the object is exposed to near-infrared light for 10 seconds, the material will be activated to unload the object, such as the attached Fig.11 shown.
[0140] Example 10
[0141] The purpose of this example is to illustrate that the near-infrared light responsive self-healing photocurable polyurethane material prepared in Example 5 can be applied to the field of flexible conductive materials. Nano silver glue is coated on the prepared sample (PETU-B3S4) 3-HI-1.0 and placed at room temperature for 3 hours to solidify the silver glue, thereby coating a conductive layer on the surface of the material. The conductive material is then connected to a battery and an LED lamp, and its conductivity is verified by the brightness of the bulb. After the circuit is turned on, the small bulb lights up, indicating that the prepared functional material has excellent conductive properties. In addition, the brightness of the lamp is not affected when the material is curled or folded, indicating that the material has good flexibility. In addition, after we repaired the damaged material, its conductivity and flexibility were not affected. When bent, the LED lamp remained bright, as shown in the attached Fig.12 shown.
[0142] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a near-infrared responsive self-repairing photocurable polyurethane material, characterized in that: The following steps are involved: (1) Preparation of polyurethane oligomers containing thiocarbamate bonds: The macromolecular chain extender, catalyst 1, and diisocyanate are heated for reaction; when the -NCO residual amount is 50%, the small molecule alcohol chain extender is dissolved in the organic solvent 1, and then added dropwise to the reaction system to continue the reaction; then the small molecule thiol chain extender and catalyst 2 are dissolved in the organic solvent 1, and then added dropwise to the reaction system to continue the reaction; then the end-capping agent is added to the reaction system to continue the reaction until the -NCO amount is 0, and the organic solvent 1 is removed to obtain; (2) Preparation of polydopamine nanoparticles: The organic solvent 2, the solvent 3 and the deionized water are mixed, and then dopamine hydrochloride monomer is added thereto, heated for reaction, centrifuged, the lower layer of solid is taken out, and dried to obtain; (3) The polyurethane oligomer containing thiocarbamate bonds and polydopamine nanoparticles prepared above are mixed with an acrylate monomer and a photoinitiator, and irradiated with ultraviolet light to obtain a near-infrared light-responsive self-healing photocurable polyurethane material based on thiocarbamate bonds.
2. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 1, characterized in that: The macromolecular chain extender is selected from one or more of polyether diols or polyether polyols with a molecular weight of 200 to 10,000, and polyester diols or polyester polyols with a molecular weight of 1,000 to 10,000.
3. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 1 or 2, characterized in that: The diisocyanate is selected from one or more of 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), trimethyl 1,6-hexamethylene diisocyanate (TMHDI), hydrogenated 4,4-diphenylmethane diisocyanate (HMDI), trans-cyclohexane isocyanate (CHDI), diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), dicyclohexylmethane diisocyanate (HMDI), and methylcyclohexyl diisocyanate (HTDI).
4. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 3, characterized in that: The small molecule alcohol chain extender is selected from C2-C16 dihydric or polyhydric alcohols; the small molecule thiol chain extender is selected from C2-C16 dihydric or polyhydric thiols; the catalyst 1 and the catalyst 2 are both selected from one or more of organic bismuth catalysts, organic tin catalysts, and amine catalysts; the end-capping agent is one or more of hydroxyethyl acrylate (HEA), hydroxypropyl acrylate (HPA), hydroxyethyl methacrylate (HEMA), and hydroxypropyl methacrylate (HPMA).
5. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 4, characterized in that: The organic solvent 1 is selected from one or more of dimethyl sulfoxide, acetone, dioxane, tetrahydrofuran, methyl formate, methyl ethyl ketone, butyl acetate, propylene glycol methyl ether acetate, ethyl acetate and isopropyl ether; the organic solvent 2 is an alcohol compound; the solvent 3 is an alkaline substance; the acrylate monomer is one or more of monofunctional, difunctional or multifunctional acrylate monomers, methacrylate monomers, acrylic acid, acrylamide, methacrylic acid, and methacrylamide.
6. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 1, characterized in that: In the reaction system of step (1), the ratio of the molar number of -NCO groups of the isocyanate raw material to the total molar number of hydroxyl groups and mercapto groups in the system is 1:
1.
7. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 1, characterized in that: The number average molecular weight of the polyurethane oligomer containing thiourethane bonds prepared in the step (1) is 7000-15000; the content of thiourethane bonds in the polyurethane oligomer containing thiourethane bonds is 0.5wt%-10wt%.
8. The method for preparing the near-infrared responsive self-repairing photocurable polyurethane material according to claim 1, characterized in that: The photoinitiator is selected from 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one (2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), methyl phenylacetoate (MBF), diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO), bis (2,4,6-trimethylbenzoyl) phenyl phosphine oxide (BAPO) and a mixture of one or more thereof.
9. A near-infrared responsive self-repairing photocurable polyurethane material prepared by the preparation method according to any one of claims 1 to 8.
10. Application of the near-infrared responsive self-repairing photocurable polyurethane material according to claim 9 in flexible conductive materials and photoactuated materials.
Citation Information
Patent Citations
Self-healing polyurethane resin containing disulfide bond and preparation method thereof
CN105482065A
Photoresponse shape-memory self-repairing composite material and preparation method, repairing method and application thereof
CN107057326A
Self-repairing polyurethane containing dynamic thionocarbamate bond and preparation method thereof
CN109942773A
Preparation method of high-strength photoresponse self-repairing nano-composite polyurethane film
CN112898611A
Self-repairing acrylate polyurethane material and synthesis method thereof
CN113461891A