Flame curtain pyrolysis kiln and biochar preparation method

By designing wedge-shaped channels and ultrasonic washing treatment in the flame curtain pyrolysis kiln, the problems of poor windproof effect and small specific surface area of ​​biochar are solved, and more efficient biochar preparation and stronger windproof performance are achieved, suitable for agriculture and High value-added field.

CN119040024APending Publication Date: 2024-11-29YUNNAN NORMAL UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411313871.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing flame curtain pyrolysis kiln has poor windproof effect and the prepared biochar is small in specific surface area, resulting in low agricultural application efficiency and insufficient applicability in high value-added fields.

Method used

A flame curtain pyrolysis kiln is designed, including the angle between the bottom wall and the side wall is greater than 90°, the lower end of the side wall is smaller than the upper end, and a wedge-shaped channel that penetrates the inside and outside on the top table. The wedge-shaped channel gradually decreases from the outside to the inside, and the wedge-shaped channel is The width is 5 mm-20 mm, combined with ultrasonic washing treatment to increase the specific surface area of ​​the biochar.

Benefits of technology

It significantly improves the windproof performance of the kiln body in outdoor environments, promotes the full carbonization of biochar, increases the specific surface area, and reduces combustible gas emission pollution. It is suitable for agriculture and high value-added fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040024A_ABST
    Figure CN119040024A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of agricultural and forestry waste biomass resource utilization and biochar preparation, and particularly provides a flame curtain pyrolysis kiln and a biochar preparation method. The pyrolysis kiln comprises a bottom wall and a side wall, the included angle between the side wall and the bottom wall is larger than 90 degrees, the size of the lower end of the side wall is smaller than that of the upper end of the side wall, a top table top is arranged at the upper end of the side wall, the top table top is arranged on the edge of the side wall by a circle, and a wedge-shaped channel penetrating inside and outside is formed in the top table top. The method comprises the following steps that S1, comburent is placed in the pyrolysis kiln to be combusted; s2, when the comburent on the surface layer is extinguished and no smoke is generated, ashing is started, and then cooling is conducted; and S3, carrying out ultrasonic washing on the extract, and obtaining the biochar after the washing is finished. The wedge-shaped channel arranged on the top table top of the pyrolysis kiln accelerates air to enter the kiln, so that the oxygen combustion-supporting effect is enhanced, and the windproof performance of the kiln body in the outdoor environment is effectively improved. Under the combined action of the wedge-shaped channel and the flame curtain, the wind resistance of the pyrolysis kiln is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of resource utilization of agricultural and forestry waste biomass and biochar preparation, and specifically, to a flame curtain pyrolysis kiln and a biochar preparation method. Background Art

[0002] The flame curtain pyrolysis kiln is a device that uses the surface raw materials to contact the air for full combustion to create an oxygen-deficient environment inside the raw materials, thereby achieving carbonization. Due to its advantages of high yield, smokeless and in-situ preparation of biochar, it is more suitable for agricultural-scale biochar preparation.

[0003] When in use, after the raw materials above are ignited, they burn violently under the action of air convection. This combustion not only generates a lot of heat, but also effectively prevents oxygen from entering the interior of the carbonizer. When working outdoors, it is easily disturbed by wind, causing holes or blown away in the flame curtain on the top of the kiln. The combustible gas escaping from the kiln loses the decomposition of the flame curtain and is directly discharged from the top of the kiln, forming thick smoke, which seriously pollutes the air; and due to insufficient pyrolysis, biochar cannot be formed. The paper named "Kon-TiKiflame curtain pyrolysis for the democratization of biochar production" (TheBiochar Journal, 2014: 14-24) provides a method of using stones to block the surrounding of the earth pit kiln and installing metal barrels around the metal kiln to reduce the impact of wind by "blocking", which has a certain protective effect on smaller breezes; however, the blocking effect on slightly larger winds is very weak; the windproof effect of the pyrolysis kiln is poor.

[0004] The prepared biochar material is subjected to a gas adsorption (N2) test to obtain the corresponding specific surface area parameters. Biochar with a larger specific surface area can stimulate N2O reducing microorganisms, increase the abundance of nitrogen fixation, nitrification and denitrification functional genes, and thus reduce N2O emissions. Therefore, the relative specific surface area of ​​biochar should be taken into consideration when applying biochar in agriculture. At the same time, increasing the specific surface area can reduce the amount of biochar applied and reduce costs. Biochar with a high specific surface area is more suitable for non-agricultural high value-added fields, such as as an electrode material for electronic double-layer capacitors. The Ithaka Institute in Switzerland earlier reported a method of quenching hot biochar with water to increase the specific surface area of ​​biochar, and obtained a specific surface area of ​​289m 2 / g of biochar; the specific surface area of ​​Eupatorium adenophorum biochar prepared based on flame curtain pyrolysis kiln is 11-215m 2 / g, with an average of 97m 2 / g (see the article entitled "Fourfold Increase in Pumpkin Yield in Response to Low-Dosage Root ZoneApplication of Urine-Enhanced Biochar to a Fertile Tropical Soil" (Agriculture, 2015, 5(3): 723-741)); the specific surface area of ​​durian wood biochar is 103±1m 2 / g of biochar.

[0005] In summary, the existing pyrolysis kilns have poor wind protection effects and the specific surface area of ​​the prepared biochar is small. Summary of the invention

[0006] The purpose of the present invention is to provide a flame curtain pyrolysis kiln and a biochar preparation method to address the deficiencies in the above-mentioned prior art, so as to solve the problems in the prior art that the pyrolysis kiln has poor windproof effect and the specific surface area of ​​the prepared biochar is small.

[0007] In the flame curtain pyrolysis kiln, due to the barrier effect of the flame curtain, an oxygen depletion zone is formed under the carbonizer. In this area, the raw materials cannot continue to burn due to lack of oxygen, but are continuously heated by the heat generated by the combustion above through heat conduction and radiation heat transfer. In this high-temperature oxygen-deficient environment, the raw materials begin to undergo carbonization reaction and gradually transform into biochar. At the same time, the raw materials will precipitate combustible gases during the heating process. These combustible gases react with oxygen when passing through the flame curtain, and are fully burned and transformed into carbon dioxide and water. This combustion process not only consumes the precipitated combustible gases, but also further provides the required energy for the carbonization process. This process continues until the carbonizer is completely filled with biochar. At this time, since the oxygen inside the carbonizer has been completely consumed and the external air is effectively blocked by the flame curtain, the raw materials gradually cool down under the condition of air isolation and finally form biochar.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows: The present application provides a flame curtain pyrolysis kiln, which includes a bottom wall and a side wall, wherein the angle between the side wall and the bottom wall is greater than 90°, the size of the lower end of the side wall is smaller than the size of the upper end of the side wall, and a top table is arranged at the upper end of the side wall, and the top table is arranged around the edge of the side wall, and a wedge-shaped channel penetrating inside and outside is arranged on the top table.

[0009] Furthermore, the size of the wedge-shaped channel gradually decreases from the outside to the inside.

[0010] Furthermore, the width of the wedge-shaped channel on the inner side is 5 mm-20 mm.

[0011] Furthermore, the wedge-shaped channel is arranged at a middle height of the top table surface.

[0012] Furthermore, the central axis of the wedge-shaped channel is parallel to the direction of the plane where the top table surface is located.

[0013] Furthermore, the angle between the top table surface and the horizontal plane is 3°-5°.

[0014] Furthermore, a groove is provided on the inner wall of the wedge-shaped channel, and the angle between the side wall and the bottom wall is 110-135°.

[0015] Furthermore, the shape of the bottom wall is circular, and the shape of the side wall is conical; the pyrolysis kiln is one of an earth pit kiln, an iron kiln, and a brick kiln.

[0016] The present application also provides a method for preparing biochar, which comprises the following steps: S1, placing the combustion material in the above pyrolysis kiln for combustion; S2, when the surface combustion material is extinguished and no smoke is generated, ash is started and then the temperature is lowered; S3, subjecting the taken out material to ultrasonic washing, and obtaining biochar after washing.

[0017] Furthermore, the ashing time in step S2 is 10 minutes; and the ultrasonic cleaning time in step S3 is 10-60 minutes.

[0018] Compared with the prior art, the present invention has the following beneficial effects: a wedge-shaped channel is provided on the top table of the pyrolysis kiln of the present application. The provision of the wedge-shaped channel accelerates the air to enter the kiln, thereby enhancing the oxygen combustion-supporting effect and effectively improving the windproof performance of the kiln in outdoor environments. When there is wind, the air is accelerated to enter the kiln through the wedge-shaped channel, igniting the combustible gas in advance to form a flame curtain. Even if the flame on the top of the kiln is blown away by the wind, it can be compensated by the flame that burns in advance, maintaining the continuity of combustion and reducing the impact of external wind on the pyrolysis of biochar. When there is no wind, the hot air floats up to drive the air into the kiln, triggering two combustions of the combustible gas, ensuring more complete combustion and cleaner emissions. The combined effect of the wedge-shaped channel and the flame curtain improves the wind resistance of the pyrolysis kiln, improves the pyrolysis efficiency, promotes the full carbonization of biochar, and reduces the emission pollution of combustible gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A schematic diagram of a flame curtain pyrolysis kiln provided by the present invention; Figure 2 A schematic diagram of a wedge-shaped channel on a top table in a flame curtain pyrolysis kiln provided by the present invention; Figure 3 is the N2 adsorption-desorption isotherm of biochar; Figure 4 is the pore size distribution curve of biochar; Figure 5 These are the results of the full kiln method on the specific surface area of ​​biochar in flame curtain biochar and the specific surface area of ​​activated biochar that has been activated with flame curtain biochar as a precursor.

[0020] Icon: 1- kiln body; 2- top table. DETAILED DESCRIPTION

[0021] In order to make the implementation process of the present invention clearer, it will be described in detail below with reference to the accompanying drawings.

[0022] The present invention provides a flame curtain pyrolysis kiln, such as Figure 1 As shown, the pyrolysis kiln includes a kiln body 1 and a top table 2, and the kiln body 1 includes a bottom wall and a side wall. The angle between the side wall and the bottom wall is greater than 90°, preferably, the angle is 110-135°, and more preferably, the angle between the side wall and the bottom wall is 110-120°, the size of the lower end of the side wall is smaller than the size of the upper end of the side wall, the longitudinal cross-section of the side wall and the bottom wall presents an inverted trapezoid, the shape of the bottom wall is circular, and the shape of the side wall is conical; in this way, the flame above the kiln top is similar to a hat, the flame completely covers the kiln top, and the combustible gas escaping from the kiln has to pass through the flame curtain to obtain full combustion and burn to form biochar; at the same time, as the material is continuously filled, the overfire area gradually increases, which is more conducive to creating an oxygen-deficient environment under the flame curtain, thereby forming fully carbonized biochar, and the 110-135° angle between the side wall and the bottom wall is the result of the interaction between the air supply and the flame curtain. A top table 2 is provided at the upper end of the side wall. The top table 2 is arranged around the edge of the side wall. A wedge-shaped channel is provided on the top table 2, which runs through inside and outside. The wedge-shaped channel is arranged at the middle height of the top table 2. The central axis of the wedge-shaped channel is parallel to the direction of the plane where the top table 2 is located. From the outside to the inside, the size of the wedge-shaped channel gradually decreases to form a wedge-shaped channel. The angle between the two side walls of the wedge-shaped channel is 10-35°, preferably, the angle is 11-15°. The inner radius of the top table is 0.5-1.2 meters, preferably, the radius is 1-1.2 meters. The radius of the bottom wall is 0.1-0.4 meters, preferably, the radius is 0.3-0.4 meters; if the size is too small, it is not conducive to the direct input of materials, and the long materials need to be cut off twice. If the size is too large, the kiln overfire area will be too large and it will be difficult to form a flame curtain.

[0023] like Figure 2As shown, the width of the wedge-shaped channel on the inside is 5mm-20mm, that is, the width at the narrowest point is 5mm-20mm, preferably, the width is 10mm. In this way, when disturbed by wind, as the channel size decreases, the speed of air entering increases, and the wedge-shaped channel on the top table 2 accelerates the air entering the kiln, supplies oxygen in advance to assist combustion, and the combustible gas is ignited before contacting the flame curtain on the kiln top, so that the entire combustion surface is reduced to the cross-section where the wedge-shaped channel is located. The moment the flame curtain on the kiln top is blown away by the wind, it will be compensated by the flame that burns in advance below it, and the flame will be blown out from the top of the kiln with the wind. The external air flow will not affect the internal biochar pyrolysis process, and it has a windproof effect. As the wind blowing intensity increases, under the action of the negative pressure above the kiln top, air will be sucked into the kiln from the wedge-shaped channel at a faster speed, thereby achieving a windproof effect adapted to the wind strength. In this way, the setting of the wedge-shaped channel allows the kiln top to be always covered by the flame curtain, which avoids the serious air pollution caused by the emission of combustible gas to a greater extent, ensures the stable progress of pyrolysis work, and provides a barrier for obtaining more fully carbonized biochar. In the absence of wind, driven by the floating effect of hot air, air will spontaneously enter the kiln through the wedge-shaped channel to ignite the combustible gas for the first combustion. When the burning combustible gas is about to overflow the flame curtain on the kiln top, it will burn again with the air rushing from the kiln top. In this way, under the cooperation of the wedge-shaped channel and the top flame curtain, the combustible gas has two opportunities for oxygen supply and combustion, so that the combustible gas burns more fully and the emission is cleaner. Because the first combustion surface drops, it is more conducive to transferring heat to the material, thereby obtaining more fully carbonized biochar. In both windy and windless conditions, the combustible gas burns more fully, and the cleanliness of combustion emissions is improved, which is beneficial to environmental protection. In general, the wedge-shaped channel on the top table 2 enhances the oxygen combustion-supporting effect, promotes the decomposition of smoke in the kiln, effectively improves the windproof performance of the kiln body in the outdoor environment, fundamentally solves the smoke problem caused by wind interference, and makes the windproof ability adapt to the wind interference intensity; in this way, the pyrolysis process is not easily disturbed by wind.

[0024] In order to further stabilize the airflow, grooves are set on the inner wall of the wedge-shaped channel. The direction of the grooves is from outside to inside, which is consistent with the direction of airflow entering. In this way, the grooves can guide the air to flow along the path and reduce the turbulence of air entering the kiln. Under the guidance of the grooves, the airflow is more stable, and a stable air layer can be formed, which reduces the direct impact of wind speed changes on the flame, making the combustion more uniform and continuous. The grooves set on the inner wall of the channel can reduce the swirl and turbulence of the airflow, prevent the air from forming irregular flows in the channel, and prevent the wind from causing the airflow to flow back into the outside of the kiln. Stable airflow helps to maintain the integrity of the flame curtain, thereby preventing the flame from being extinguished or the combustion from being unstable due to wind. The groove area is relatively small, and the airflow will accelerate into the kiln, thereby increasing the oxygen supply speed and enhancing the combustion effect; the accelerated airflow can also replenish the flame more quickly when the wind blows, reducing the interference of external wind. There are multiple grooves, and grooves are set on the inner wall of the wedge-shaped channel. Preferably, the width of the groove is uneven, the width of the groove gradually decreases from the outside to the inside, and the width of the groove near the inside is greater than the width of the outside; when the air is guided by the gradual contraction in the groove, its flow direction is more controlled, which reduces the backflow or turbulence of the airflow caused by the external wind, and helps to maintain stable oxygen supply and combustion in the kiln. Due to the larger width on the inside, more air can smoothly enter the kiln and fully contact with the combustible gas, thereby improving the combustion efficiency. The narrower width on the outside helps to maintain the stability of the flame curtain, reduce the disturbance of the external wind, and make the flame less likely to be blown away or extinguished under strong wind conditions.

[0025] The angle between the top table 2 and the horizontal plane is 3°-5°, and the top table 2 forms a slope outside the kiln and tilts downward; in this way, due to the floating effect of the hot air in the kiln, air will enter the kiln from the outside of the kiln through the wedge-shaped channel to assist combustion; on the contrary, if the table forms a slope inside the kiln (tilted upward), a chimney effect will be formed, so that the combustible gas will be guided out of the kiln from the kiln through the wedge-shaped channel, posing a fire hazard and thick smoke emissions. The 3°-5° inclination angle can completely prevent the chimney effect, and it can be achieved by lightly knocking on the bricks after the conventional horizontal masonry without changing the conventional horizontal masonry. It effectively prevents the combustible gas or flame from flowing back from the wedge-shaped channel due to the chimney effect, eliminating potential safety hazards. When the pyrolysis kiln is not needed to work, the bottom wall and side walls of the pyrolysis kiln of this application are covered with a water-proof film such as plastic, which can be used as a reservoir for forest land and farmland, expanding the function of the kiln body, and realizing the effective storage and utilization of water resources, providing strong support for agricultural production and ecological environment protection.

[0026] The pyrolysis kiln is one of the earth pit kiln, iron kiln and brick kiln; the material can be earth, iron or brick. Taking the brick kiln as an example, the preparation method is as follows: Step 1: Level the land and locate the area; Remove weeds within 5 meters around the pit, level the ground, and convert slopes into terraces. Determine the diameter of the kiln top according to the size of the kiln, and use lime and other materials to outline the circumference. Use tools such as hoes to point from the circumference to the center of the circle to create a clear circumference.

[0027] Step 2: dig a pit, shape it, and prepare concrete; First, dig a shallow pit from the center of the circle outward, and then finely trim it into a truncated cone-shaped soil pit. The slurry is prepared with 20%-30% ordinary Portland cement, 50%-65% ordinary coarse sand, and 10%-15% of the excavated soil to bond bricks. The soil produced by the excavation is added to the slurry; on the one hand, it reduces the use of commercial construction materials, reduces construction costs, and makes full use of on-site resources; on the other hand, it can effectively avoid the risk of kiln body explosion, can simultaneously meet the two flameout operation modes of annealing and quenching, enhance the functionality and service life of the brick-concrete kiln, and improve its flexibility and reliability in practical applications.

[0028] Step 3: Lay bricks and build a kiln; The 240mm×115mm surface of the brick is always in contact with the earth pit and filled with mortar, first the bottom wall and then the side wall. The bricks are stacked crosswise and filled with mortar. The truncated cone pit surface is covered with bricks, especially the 240mm×115mm surface of the brick is in contact with the earth pit, which effectively prevents the pit surface collapse of the earth kiln built on loam land, and overcomes the difficulty of building earth kilns on sandy land, significantly enhancing the adaptability of the flame curtain pyrolysis technology, so that the technology can be applied in a wider geographical environment.

[0029] Step 4: Build the kiln top table 2.

[0030] The top of the kiln is built to form a top table 2. A unique three-layer brick laying method is adopted. The first brick layer forms a slope of 3-5° with the horizontal plane and points to the outside of the kiln. The second brick layer is laid parallel to the plane where the first brick layer is located. A wedge-shaped channel is reserved between the two bricks close to the inner circular edge. The wedge-shaped channel is wide outside and narrow inside. The two adjacent bricks on the inside do not touch each other, forming a wedge-shaped channel; the width of the wedge-shaped channel at the narrowest point of the wedge-shaped channel is controlled between 5mm and 20mm, preferably 10mm. The third brick layer is also parallel to the second brick layer, and the laying method is consistent with the first brick layer, that is, it forms a slope of 3-5° with the horizontal plane and points to the outside of the kiln. Preferably, it forms a slope of 5° with the horizontal plane. Each layer of bricks is stacked crosswise, and all wedge-shaped channels are filled with mortar for bonding. After the third brick layer is laid, the slurry filled in the wedge-shaped channel of the second brick layer is removed from the inside to the outside; the slurry between the second brick layers can be hollowed out with a thin iron wire. The preparation of the pyrolysis kiln of this application is completed. The wedge-shaped channels between the countertop bricks are hollowed out on the basis of conventional bricklaying concrete filling. Compared with the masonry method with special gaps, it is more stable and durable, which not only ensures the structural strength of the countertop, but also extends its service life.

[0031] The present application also provides a method for preparing biochar, which comprises the following steps: S1, placing the combustion material in the above pyrolysis kiln for combustion; The combustion material can be grapevine, citrus branch, walnut branch, chestnut branch, palm branch, pear branch, olive branch, cypress branch, pine branch, pine cone, rice straw, corn straw, corn cob, etc. In this embodiment, a small amount of branches are taken as an example, and they are arranged in a "well" shape that is interwoven horizontally and vertically at the bottom of the flame curtain pyrolysis kiln, and stacked layer by layer to form a "wood chimney". Since the pyrolysis kiln has a certain depth, it is easy to extinguish the flame due to lack of oxygen if the branches are directly ignited. Through the "wood chimney", the hot air floating effect can be used to suck cold air from all sides into the kiln, so that air convection can be made to maintain combustion. Thinner branches are placed vertically in the cavity in the middle of the "wood chimney", which can more easily lead the fire from the top to the bottom, allowing the material to burn fully, forming a stronger air convection, and burning more fully. Prevent ignition materials, such as dry weeds, in the middle of the top of the "wood chimney". Ignite the weeds, and the flames will ignite the "wood chimney" from top to bottom, forming a smokeless combustion, until the "wood chimney" burns to natural collapse, forming a fire surface at the bottom of the kiln. Then, put branches into the kiln, observe the burning state of the flame, and gradually add branches under the condition of maintaining vigorous burning of the flame.

[0032] S2, when the surface combustion material is extinguished and no smoke is generated, ash is started and then the temperature is lowered; When the branches are converted into biochar and fill the charcoal kiln, stop feeding, and the biochar fills the flame curtain pyrolysis kiln, the temperature is higher, the temperature field is more uniform, the annealing and cooling time is longer, the material is more fully carbonized, and the proportion of aromatic carbon contributing to the specific surface area of ​​biochar is increased, thereby increasing the specific surface area of ​​biochar, and can also give full play to the load of the kiln and increase the output. When the flame of the last layer of branches is extinguished and no smoke is generated, continue to keep it for more than 10 minutes to allow the surface of the biochar to be fully and completely ash. You can use wet soil to cover the fire or metal cover to cool down naturally. Wet soil refers to soil with a moisture content of 60%, and the thickness of the wet soil is 20 cm. Among them, it takes at least 10 days to remove the product when covering with wet soil to extinguish the fire, and it takes at least 24 hours to remove the product when using a metal cover. Natural annealing of biochar can greatly increase the specific surface area of ​​biochar, while saving quenching water and biochar drying.

[0033] S3, subjecting the taken out material to ultrasonic washing, and obtaining biochar after washing.

[0034] Ultrasonic washing is carried out under an ultrasonic power of 80w-300w, preferably, the power is 120W, and the ultrasonic wave is applied for 10-60min. Specifically, the biochar block is placed in a glass beaker, water is added to cover the biochar block, and the biochar block is placed in an ultrasonic oscillator for treatment for 30min. The water is naturally drained under the action of gravity, and the biochar is dried in a 40°C constant temperature forced air drying oven to constant weight. Ultrasonic treatment increases the specific surface area of ​​biochar, which is due to the combined effect of the following three aspects: First, ultrasonic treatment cleans the larger ash particles in the rich pore structure of biochar more thoroughly into the aqueous solution, exposing more mesopores (pore size 2-50 nanometers) and macropores (pore size greater than 50 nanometers) in the biochar. Secondly, the hexagonal carbon atoms in graphite are bonded by strong covalent bonds (the distance between carbon atoms is about 0.142 nanometers), and the effect of ultrasonic oscillation on them can be ignored. However, the graphite layers bonded by van der Waals forces are prone to sliding. Under the action of ultrasonic oscillation, the interlayer spacing may increase and compress instantly. Small-sized impurity atoms will move back and forth between the graphite layers and the aqueous solution, and form a dynamic equilibrium under the action of constant-power ultrasonic oscillation. Once the disturbance stops, some small-sized impurity atoms will be between the graphite layers, and the interlayer spacing of graphite is difficult to return to the original approximately 0.335 nanometers. To a certain extent, the interlayer spacing of graphite is filled and expanded by small-sized impurity atoms, which is equivalent to increasing the micropores (pore diameter is less than 2 nanometers, and the general diameter of nitrogen molecules is about 0.364 nanometers, which is most suitable for measuring gaps of about 0.4-50 nanometers. The enlarged spacing may just fall into the range of 0.364-0.4 nanometers, with a high degree of response). On the third aspect, ultrasonic oscillation can increase the interlayer spacing of graphite oxide to a certain extent through the cavitation effect produced in water, so that the graphite oxide with a larger interlayer spacing is peeled off, and its fragments may be intertwined with other fragments, defects, and voids in the complex biochar structure to form micropores. In particular, the latter two reasons greatly increase the specific surface area of ​​biochar after ultrasonic oscillation treatment, because the contribution of voids to the specific surface area mainly depends on micropores (less than 2 nanometers) within a certain range. Ultrasonic washing treatment can not only effectively increase the specific surface area of ​​biochar, but also save energy and protect the environment. The present application can also easily obtain biochar without impurities such as soil and rust. This pure biochar has higher quality and application value, and can meet the needs of different fields for high-quality biochar. On the basis of ensuring that the flame curtain pyrolysis kiln is windproof, combustion-supporting, environmentally friendly, safe, and durable, the specific surface area of ​​biochar is substantially increased, and large-scale, cheap, and low-carbon footprint preparation of activated biochar is realized.

[0035] The following are the results of the comparative tests. First, burn 1 ton of nectarine branches, cover the biochar with bricks, seal it with soil from the dug pit, and anneal and cool it naturally. The diameter of the kiln top is 2 meters, the diameter of the kiln bottom is 0.6 meters, the kiln depth is 1 meter, and the volume is 2 cubic meters. The surface area parameter of the biochar prepared by the full kiln method of the pit kiln (non-windproof kiln) is: 389.346m2 / g, total pore volume: 0.1949cm 3 / g, the average pore size is: 2.002nm, and the specific surface area of ​​the biochar prepared by the full kiln is larger. The N2 adsorption-desorption isotherm of the biochar is shown in Figure 3 As shown in Figure 1, when the relative pressure approaches 0, the adsorption amount of N2 gas suddenly increases, indicating that there is an obvious micropore filling process. The desorption curve completely coincides with the adsorption curve, indicating that there are no ink bottle pores and the adsorbent can be desorbed when it enters the pores. Therefore, using it as a fertilizer carrier can not only maintain fertility but also effectively release nutrients slowly. The pore size distribution curve is shown in Figure 1. Figure 4 As shown in the figure, the pore volume of biochar is mainly contributed by micropores with a pore size of less than 2nm, and the peak of the distribution curve appears before 2nm, indicating that the micropores below 2nm in biochar are the most developed. This shows that the full kiln method can effectively improve the adsorption performance of biochar, increase the number of micropores (<2nm), and increase its pore volume and specific surface area. Figure 5 The specific surface area of ​​biochar prepared by the full kiln method is higher than that of biochar prepared by flame curtain biochar and activated biochar with flame curtain biochar as precursor. The specific surface area of ​​biochar prepared by the full kiln method not only exceeds the specific surface area of ​​biochar prepared by flame screening pyrolysis kiln including quenching method (the data reported so far: the article named "Partial Substitution of peat moss with biochar for sustainable cultivation of Durio zibethinus L. in nurseries" (Arabian Journal of Geosciences, 2018, 11(15): 426(1-9)) reported that the specific surface area of ​​biochar is 103±1m 2 / g; The article titled “Fourfold Increase in Pumpkin Yield in Response to Low-Dosage Root Zone Application of Urine-Enhanced Biochar to a Fertile Tropical Soil” (Agriculture, 2015, 5(3): 723-741) reported that the specific surface area of ​​biochar is 215m 2 / g; The article titled “Utilization of pine tree biochar produced by flame-curtainpyrolysis in two non-agricultural applications” (Bioresource Technology Reports, 2020, 9: 1-8) reported that the specific surface area of ​​biochar is 266m 2 / g; The article titled “Fourfold Increase in Pumpkin Yield in Response to Low-Dosage Root Zone Application of Urine-Enhanced Biochar to a Fertile Tropical Soil” (Agriculture, 2015, 5(3):723-741) reported that the specific surface area of ​​biochar is 289m 2 / g; The article titled “Flame curtain pyrolysis of oil palm fronds for potential acidic soil amelioration and climate change mitigation” (Journal of Environmental Chemical Engineering, 2020, 8(4): 103982(1-39)) reported that the specific surface area of ​​biochar is 303m 2 / g; The article titled “Characterization and Determination of the Toxicological Risk of Biochar Using Invertebrate Toxicity Tests in the State of Agusascalients, Mexico” (Applied Sciences, 2019, 9(8): 1706(1-19)) reported that the specific surface area of ​​biochar is 305m 2 / g) and exceeded the biochar activated carbon prepared from pine wood residue reported in the article titled "Utilization of pine tree biochar produced by flame-curtain pyrolysis in two non-agricultural applications" (Bioresource Technology Reports, 2020, 9: 1-8) (the biochar prepared in the flame curtain pyrolysis kiln was used as a precursor, and further activated at 600°C for 1 hour under nitrogen protection according to the ratio of biochar: H3PO4=1:3 (w / w), cooled, repeatedly washed with water, and dried at 80°C for 24 hours to obtain a specific surface area of ​​325m 2 / g of biomass activated carbon). And it has fallen into the article named "Utilization of pine tree biochar produced by flame-curtain pyrolysis in two non-agricultural applications" (Bioresource Technology Reports, 2020,9: 1-8) reported that the biomass activated carbon prepared by using biochar prepared in flame curtain pyrolysis kiln as precursor was 325m 2 / g-2503m 2 / g specific surface area. Therefore, the full kiln method can significantly increase the specific surface area of ​​biochar and has the potential to prepare activated biochar.

[0036] Converting materials into biochar to fill or nearly fill the kiln can significantly increase the specific surface area of ​​biochar without adding any cost or equipment. A 2-cubic-meter kiln, even if filled to 3 / 4 of the depth, has a filling volume of slightly less than 1 cubic meter (because the kiln is an inverted cone with a large top and a small bottom, which is easy to calculate), which is equivalent to using a 1-cubic-meter kiln to prepare biochar. Therefore, for kilns of the same size, especially kilns with a volume of 2 cubic meters, the filling amount has a significant effect on the specific surface area of ​​biochar. A higher filling amount means higher temperature, more uniform temperature field, more complete carbonization of materials, more complete conversion of materials into aromatic carbon, and an increase in the proportion of aromatic carbon in biochar, thereby obtaining a higher specific surface area, because the hemicellulose, cellulose and lignin that constitute the biomass itself are difficult to contribute to the specific surface area. On the other hand, annealing will increase the degree of crystallization of the material, make the atomic arrangement more orderly, and have fewer defects. The flame curtain earth pit kiln full kiln preparation is extinguished by isolating oxygen annealing. The highest annealing temperature (generally below 500°C) is not enough to collapse the micropores that were previously formed and played a decisive role in the specific surface area (the collapse temperature is generally above 800°C, which is related to the material and activation method), and it is even more impossible to make the carbon material enter the crystallization temperature range (2300-3000°C). Therefore, annealing allows the incompletely carbonized materials to be more thoroughly carbonized, increasing the proportion of aromatic carbon in the biochar to obtain a higher specific surface area. In other words, both the full kiln and annealing increase the proportion of aromatic carbon that contributes to the specific surface area in the biochar by affecting the temperature, thereby increasing the specific surface area of ​​the biochar.

[0037] In the flame curtain brick kiln, 834 kg of nectarine branches were burned for 4 hours, and then the wedge-shaped channel between the stainless steel cover and the top of the brick kiln was sealed with soil from the pit, and the biochar was naturally annealed and cooled. The volume of the flame curtain brick kiln is 1.9m 3 , bottom diameter 40-44cm, top diameter 188-193cm, and the outer angle between the side wall and the horizontal plane is 60-65°. The surface area results of the biochar obtained by annealing and natural annealing are shown in Table 1. Different sampling numbers represent different samples. In order to reduce the error, 13 samples were taken at different positions for memory testing in this embodiment of the application. Table 2 shows the surface area results of the samples obtained by quenching with water. From the average value, the specific surface area of ​​the quenched biochar is 158.67m 2 / g, and the specific surface area of ​​annealed biochar is 188.3m 2 / g, annealing is more conducive to increasing the specific surface area of ​​biochar; compared with quenching that happens in an instant, annealing gives biomass sufficient time to transform into aromatic carbon, increasing the proportion of aromatic carbon that contributes to the specific surface area in biochar, thereby increasing the specific surface area of ​​biochar.

[0038] Table 1: Surface area results of biochar obtained by annealing; Table 2: Surface area results of biochar obtained by quenching; The annealed biochar and quenched biochar at the same position were selected and washed as follows: the annealed biochar fragments were added to a beaker, submerged with deionized water, and the beaker was placed in an ultrasonic oscillator filled with water for treatment, with an ultrasonic power of 30-240w and a treatment time of 15-120min. Preferably, the ultrasonic oscillation was performed at 120w for 30 minutes. Table 3 shows the specific surface area analysis results of the annealed biochar after ultrasonic treatment, and Table 4 shows the specific surface area analysis results of the quenched biochar after ultrasonic treatment. A surface area of ​​up to 641.23m 2 / g specific surface area, indicating that ultrasonic cleaning can significantly increase the specific surface area of ​​annealed biochar. The reasons are as follows: First, ultrasonic oscillation can effectively clean the large-particle ash in biochar, exposing more mesopores and macropores. Secondly, ultrasonic oscillation may cause the van der Waals force bonding between graphite layers to slide, resulting in an instantaneous increase and compression of the interlayer spacing. Small-particle impurity atoms will be embedded in the graphite interlayer, preventing it from returning to its original spacing, thereby expanding the microporous structure. Finally, ultrasonic oscillation increases the interlayer spacing of graphite oxide through the cavitation effect in water, and the exfoliated graphite oxide fragments may be intertwined with other structures in biochar to form micropores. These mechanisms, especially the latter two points, increase the number of micropores, and micropores contribute the most to the specific surface area, thereby significantly increasing the specific surface area of ​​biochar. The power of the ultrasound is 120w, and the oscillation time is 30min; this can open the graphite layer or form a significant cavitation effect; a larger power can better open the graphite layer or form a significant cavitation effect, allowing small particle size impurities to instantly shuttle between the graphite layer and the aqueous solution and form a dynamic balance, which can increase the number of micropores in a very short time, thereby increasing the specific surface area; the power makes the graphite layer open to the maximum extent.

[0039] Table 3: Specific surface area analysis results of annealed biochar after ultrasonic treatment; Table 4: Specific surface area analysis results of quenched biochar after ultrasonic treatment.

[0040] The flame curtain earth pit kiln of this embodiment was built in the rose garden of Yunnan Agricultural Vocational College in Kunming, Yunnan Province, China. The flame curtain brick kiln was built in the nectarine garden and pear garden of Yunnan Agricultural Vocational College in Kunming, Yunnan Province, China, the peach and plum base in Shuangbai County, Chuxiong City, Yunnan Province, and the olive base in Songming County, Kunming City, Yunnan Province. The windproof flame curtain brick kiln was built in the flue-cured tobacco planting base in Changning County, Baoshan City, Yunnan Province, and the grape planting base and citrus planting base in Binchuan County, Yunnan Province. It is only introduced as an example and does not limit the area where the pyrolysis kiln is built.

[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A flame curtain pyrolysis kiln, comprising a bottom wall and a side wall, characterized in that: The angle between the side wall and the bottom wall is greater than 90°, the size of the lower end of the side wall is smaller than the size of the upper end of the side wall, the upper end of the side wall is provided with a top table, the top table is arranged around the edge of the side wall, and a wedge-shaped channel penetrating inside and outside is provided on the top table.

2. The flame curtain pyrolysis kiln according to claim 1, characterized in that: From outside to inside, the size of the wedge-shaped channel gradually decreases.

3. The flame curtain pyrolysis kiln according to claim 2, characterized in that: The width of the wedge-shaped channel on the inner side is 5 mm-20 mm.

4. The flame curtain pyrolysis kiln according to claim 3, characterized in that: The wedge-shaped channel is arranged at the middle height of the top table.

5. The flame curtain pyrolysis kiln according to claim 4, characterized in that: The central axis of the wedge-shaped channel is parallel to the direction of the plane where the top table surface is located.

6. The flame curtain pyrolysis kiln according to claim 5, characterized in that: The angle between the top table and the horizontal plane is 3°-5°.

7. The flame curtain pyrolysis kiln according to claim 6, characterized in that: A groove is arranged on the inner wall of the wedge-shaped channel, and the angle between the side wall and the bottom wall is 110-135°.

8. The flame curtain pyrolysis kiln according to claim 7, characterized in that: The bottom wall is circular in shape, and the side wall is conical in shape; the pyrolysis kiln is one of an earth pit kiln, an iron kiln, and a brick kiln.

9. A method for preparing biochar, characterized in that: The method comprises the following steps: S1, placing the combustion material in the pyrolysis kiln as claimed in claim 1 for combustion; S2, when the surface combustion material is extinguished and no smoke is generated, ash is started and then the temperature is lowered; S3, subjecting the taken out material to ultrasonic washing, and obtaining biochar after washing.

10. The method for preparing biochar according to claim 9, characterized in that: The ashing time in step S2 is 10 minutes; the ultrasonic cleaning time in step S3 is 10-60 minutes.