Decarburization characteristic method based on heating, rolling and slow cooling processes

By optimizing the heating, rolling, and slow cooling processes, and controlling the temperature and time of the soaking zone, the temperature of the upper cooling bed, and the opening degree of the cooling bed insulation cover, the decarburization problem of spring steel during heating, rolling, and slow cooling was solved, fatigue life was improved, and production accidents were avoided.

CN119040586AInactive Publication Date: 2024-11-29HUNAN VALIN XIANGTAN IRON & STEEL CO LTD

Patent Information

Application Number
CN202411161905.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing technologies, spring steel is prone to developing a decarburized layer during heating, rolling, and slow cooling, which leads to a reduction in fatigue life. In particular, the fatigue performance is significantly reduced when a complete decarburized layer is formed on the surface. Furthermore, research has focused on heating while neglecting the effects during rolling and slow cooling.

Method used

The decarburization depth of 60Si2Mn spring steel can be reduced by optimizing the heating, rolling, and slow cooling processes, specifically by controlling the temperature and time of the soaking zone in the heating furnace, the temperature of the upper cooling bed during the rolling process, and the degree of opening of the cooling bed insulation cover.

Benefits of technology

It effectively reduces the decarburization layer depth of 60Si2Mn spring steel, improves fatigue life, avoids production accidents, improves production efficiency, and meets customers' requirements for product hardness and machinability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040586A_ABST
    Figure CN119040586A_ABST
Patent Text Reader

Abstract

The invention discloses a decarburization characteristic method based on heating, rolling and slow cooling processes, and relates to the technical field of decarburization. The decarburization characteristic method based on the heating, rolling and slow cooling process comprises the following specific steps that S1, the heating process is conducted, specifically, in the actual production process of 60Si2Mn spring steel, surface decarburization of the 60Si2Mn spring steel mainly occurs in the heating process of a heating furnace; s2, a rolling process: according to a production process of a steel rolling mill, phi 25mm (round steel with the diameter of 25mm) produced on site is selected as a test object, a rolling program table is shown in a table 2, the temperature on a cooling bed is controlled, sampling is performed at the cooling bed, and a metallographic sample is prepared after air cooling; and S3, a slow cooling process is conducted, specifically, the consistency of the temperature of a cooling bed is kept, the influence of the cooling speed on the cooling bed after rolling on surface decarburization of the 60Si2Mn spring steel is researched by controlling the opening degree of a heat preservation cover of the cooling bed, the heating temperature of a soaking section is 1000 DEG C, but the actual situation of the site is considered, the temperature of the soaking section is 1050 DEG C, accidents can be controlled on the production site, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of decarburization, and in particular to a decarburization method based on heating, rolling and slow cooling processes. Background Art

[0002] Spring steel includes 60Si2Mn, 50CrV4, 51CrV4, and 52CrMoV4, which are mainly used for automobiles. In recent years, with the upgrading of domestic production equipment and the development of the automobile industry, the demand for spring steel has shown a rapid growth trend. However, due to the high Si content of 60Si2Mn, it is easy to have a full decarburization layer during heating, rolling, and slow cooling. Numerous production practices have proved that the fatigue life of spring steel decreases with the increase of decarburization layer, especially if a full decarburization layer appears on the surface, the fatigue performance of spring steel will decrease significantly.

[0003] Decarburization of spring steel refers to the reduction of carbon atoms on the surface of unoxidized steel, which can be divided into partial decarburization and full decarburization. The full decarburization layer is a ferrite structure that grows vertically to the surface in a columnar shape. The metallographic appearance is a bright white band. Near the edge of the full decarburization layer, the reticular ferrite structure extends toward the center along the original austenite grain boundary, which is a partial decarburization layer.

[0004] The fatigue life of spring steel is inversely proportional to the depth of the surface decarburization layer. If there is a decarburization layer on the steel, during subsequent processing or quenching, the hardness and mechanical strength of the surface decarburization layer will be lower than those of normal parts. The expansion coefficients of different areas of the surface layer are different, which can easily lead to stress concentration and even microcracks, eventually causing the spring to fail and break. If a complete decarburization layer appears on the surface of the spring steel, the fatigue limit will be reduced by about 50%. Therefore, to increase the service life of the spring, it is necessary to start from the raw materials and find the influencing factors and prevention measures of spring steel decarburization. Many studies have been conducted in China on the formation of decarburization layer in spring steel, and the main research focuses on the heating of spring steel, while relatively few studies have been conducted on its rolling and slow cooling. Summary of the invention

[0005] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a decarburization method based on heating, rolling and slow cooling process, which can solve the above-mentioned problem.

[0006] To achieve the above object, the present invention provides the following technical solutions: A method for decarburization characteristics based on heating, rolling and slow cooling process, comprising the following specific steps: S1 Heating process: In the actual production process of 60Si2Mn spring steel, its surface decarburization mainly occurs during the heating process of the heating furnace;

[0007] S2 rolling process: the production process of the steel rolling mill, the φ25mm (round steel with a diameter of 25mm) produced on site was selected as the test object, the rolling program table is shown in Table 2, the temperature of the upper cooling bed is controlled, the sample is taken at the cooling bed, and the metallographic specimen is made after air cooling;

[0008] S3 slow cooling process: Keep the temperature of the upper cooling bed consistent, and control the opening degree of the cooling bed insulation cover to study the effect of the cooling rate on the cooling bed after rolling on the surface decarburization of 60Si2Mn spring steel.

[0009] Preferably, in the S1 heating process, factors such as room temperature billet feeding into the furnace, slightly positive pressure in the furnace, and residual oxygen content being controlled ≤1% throughout the whole process are kept unchanged, and the effects of soaking section temperature and soaking section time on surface decarburization of 60Si2Mn spring steel are studied.

[0010] Preferably, in the S1 heating process, the soaking section is below 1000°C.

[0011] Preferably, in the S1 heating process, the temperature in the soaking section is 1000-1250° C. and the heating time in the soaking section is 60-300 min.

[0012] Preferably, in the S1 heating process, sampling is performed at the flying shear, and metallographic specimens are prepared through processing steps such as wire cutting, mounting, grinding, polishing, and corrosion.

[0013] Preferably, the S2 rolling process studies the effect of the temperature of the cooling bed after rolling on the surface decarburization of 60Si2Mn spring steel.

[0014] Preferably, there is no complete decarburization on the surface of the 60Si2Mn continuous casting billet, and the total decarburization layer depth is 330-360um; there is local complete decarburization of 74um at the corners, and the total decarburization is 180-291um.

[0015] Preferably, the temperature of the soaking section is 1000-1250°C and the heating time in the soaking section is 60-300 minutes respectively. The test conditions are as follows: Figure 3 As shown, from Figure 3 It can be seen that when heated in the soaking section for 60 minutes, in the temperature range of 1000℃~1150℃, when the soaking section temperature increases, the depth of the decarburization layer increases. The reason is that the decarburization rate is greater than the oxidation rate. However, when the soaking section temperature exceeds 1150℃, the depth of the decarburization layer decreases with the increase of temperature.

[0016] Preferably, in the process of heating the 60Si2Mn spring steel from low temperature to high temperature, when the temperature rises to 1150°C, the depth of the decarburized layer on the surface of the spring steel reaches a maximum value of 48.1um, and with the increase of the heating time in the soaking section, all curves show an obvious increasing trend. At 120 minutes, when the soaking section temperature is 1200°C and 1250°C, the decarburized layer on the surface of the material quickly surpasses the sample with a soaking section temperature ≤1150°C. With the extension of the heating time and the increase of the heating temperature, the oxide scale on the surface of the spring steel becomes thick, loose and porous, and the residual oxygen in the heating furnace easily reacts with the C atoms in the steel, causing the decarburization rate of the steel to exceed the oxidation rate.

[0017] Preferably, for the samples with the soaking section temperature of 60min and the soaking section temperature of 1050°C, no complete decarburization layer was found when the upper cooling bed temperature was controlled. Only a partial decarburization layer was observed on the surface. The ferrite of the partial decarburization layer was distributed along the grain boundary. When the upper cooling bed temperature was controlled at 900°C, the decarburization layer temperature was 42um-45um, and when the upper cooling bed temperature was 800-700°C, the decarburization layer depth was similar, which were 26um-39um and 21um-25um respectively.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. This method based on the decarburization characteristics of heating, rolling and slow cooling processes can reduce the decarburization depth of 60Si2Mn spring steel and avoid production accidents. The optimal soaking section temperature in the heating furnace in this article is 60min, and the soaking section temperature is 1050℃. The decarburization layer depth and heating time are linearly fitted. With the increase of heating temperature, its slope gradually increases.

[0020] 2. This method based on the decarburization characteristics of heating, rolling and slow cooling process, in order to reduce the decarburization layer depth of 60Si2Mn spring steel, according to the calculation model, the heating temperature of the soaking section should be 1000℃. However, considering the actual situation on site, the soaking section temperature is 1050℃, which is conducive to controlling accidents on the production site and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0022] Figure 1 This is a rolling production process flow chart of the present invention;

[0023] Figure 2 This is a schematic diagram of the decarburization layer of the 60Si2Mn continuous casting billet of the present invention;

[0024] Figure 3 It is a schematic diagram of the curve of the change of the decarburized layer of 60Si2Mn spring steel with the soaking period time at different soaking period temperatures of the present invention;

[0025] Figure 4 Schematic diagram of the decarburization layer depth of 60Si2Mn spring steel under different rolling processes of the present invention;

[0026] Figure 5 This is the metallographic diagram of the sample with the best process route of the present invention. DETAILED DESCRIPTION

[0027] This section will describe in detail the specific embodiments of the present invention. The preferred embodiments of the present invention are shown in the accompanying drawings. The purpose of the accompanying drawings is to supplement the description of the text part of the specification with graphics, so that people can intuitively and vividly understand each technical feature and the overall technical solution of the present invention, but it cannot be understood as a limitation on the scope of protection of the present invention.

[0028] In the description of the present invention, it should be understood that descriptions involving orientations, such as up, down, front, back, left, right, etc., and orientations or positional relationships indicated are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0029] In the description of the present invention, "greater than", "less than", "exceed" etc. are understood as not including the number itself, and "above", "below", "within" etc. are understood as including the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0030] In the description of the present invention, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in the present invention based on the specific content of the technical solution.

[0031] See also Figure 1-5 The present invention provides a technical solution: a method for decarburization characteristics based on heating, rolling and slow cooling process. The production process of the steel rolling mill is: continuous casting billet - rough rolling - intermediate rolling - pre-finishing rolling - finishing rolling. The specific process flow chart is as follows Figure 1 As shown;

[0032] 0Si2Mn spring steel chemical composition;

[0033] The specific contents of each element of the chemical composition of 60Si2Mn spring steel are shown in Table 1 below;

[0034] Table 1 Chemical composition of 60Si2Mn

[0035]

[0036] Further, a method for decarburization characteristics based on heating, rolling and slow cooling process includes the following specific steps: S1 heating process: in the actual production process of 60Si2Mn spring steel, its surface decarburization mainly occurs during the heating process of the heating furnace;

[0037] Among them, factors such as room temperature billet entering the furnace, slightly positive pressure in the furnace, and residual oxygen content being controlled ≤1% throughout the whole process were kept unchanged, and the effects of soaking section temperature and soaking section time on the surface decarburization of 60Si2Mn spring steel were studied;

[0038] Among them, considering the actual rolling conditions on site, if the soaking section is lower than 1000℃, the rolling mill rolls will break and the grooves will not be wear-resistant during the rolling process, which will lead to serious production accidents;

[0039] The temperature of the soaking section is 1000-1250°C and the heating time in the soaking section is 60-300 minutes respectively.

[0040] Among them, the samples are taken from the flying shear, and metallographic specimens are made through wire cutting, mounting, grinding, polishing, corrosion and other processing procedures;

[0041] S2 rolling process: Figure 1 The production process of the steel rolling mill, φ25mm (round steel with a diameter of 25mm) produced on site was selected as the test object, the rolling program table is shown in Table 2, the temperature of the upper cooling bed is controlled, samples are taken at the cooling bed, and metallographic specimens are made after air cooling;

[0042] Among them, the effect of the temperature of the cooling bed after rolling on the surface decarburization of 60Si2Mn spring steel was studied.

[0043] S3 slow cooling process: Keep the temperature of the upper cooling bed consistent, and study the effect of the cooling rate on the cooling bed after rolling on the surface decarburization of 60Si2Mn spring steel by controlling the opening degree of the cooling bed insulation cover.

[0044] Table 2φ25mm rolling schedule

[0045]

[0046]

[0047] Furthermore, the influence of soaking temperature and soaking time on the surface decarburization of 60Si2Mn spring steel

[0048] Decarburization layer of 60Si2Mn continuous casting billet Figure 2 As shown, a: continuous casting billet plane, b: continuous casting billet corner from Figure 2We found that there was no complete decarburization on the surface of the 60Si2Mn continuous casting billet, and the total decarburization layer depth was 330-360um; there was local complete decarburization of 74um at the corner, and the total decarburization was 180-291um. In order to avoid the influence of the decarburization layer generated during the continuous casting of the billet on the test, all 60Si2Mn continuous casting billets were peeled;

[0049] The sample was heated at a temperature of 1000-1250°C in the soaking zone for 60-300 minutes. The test conditions are as follows: Figure 3 As shown, from Figure 3 It can be seen that when heated in the soaking section for 60 minutes, in the temperature range of 1000℃~1150℃, when the soaking section temperature increases, the depth of the decarburization layer increases. The reason is that the decarburization rate is greater than the oxidation rate. However, when the soaking section temperature exceeds 1150℃, the depth of the decarburization layer decreases with the increase of temperature. The main reason is that in the high-temperature soaking section (temperature>1150℃), the oxidation and decarburization reaction rates of the material surface are both relatively large. The rapid generation of iron oxide scale on the material surface slows down the decarburization reaction of the material, resulting in a decarburization rate that is slower than the oxidation rate. The decarburization layer generated by the decarburization reaction is partially oxidized and lost. After high-pressure water descaling, the iron oxide scale is removed, which reduces the depth of the decarburization layer of the material. Therefore, when the soaking section is kept warm for 60 minutes, in the process of heating the 60Si2Mn spring steel from low temperature to high temperature, when the temperature rises to 1150℃, the depth of the decarburized layer on the surface of the spring steel reaches a maximum value of 48.1um, and with the increase of the heating time in the soaking section, all curves show an obvious increasing trend. At 120 minutes, when the soaking section temperature is 1200℃ and 1250℃, the decarburized layer on the surface of the material quickly surpasses the sample with the soaking section ≤1150℃. With the extension of heating time and the increase of heating temperature, the oxide scale on the surface of the spring steel becomes thick, loose and porous, and the residual oxygen in the heating furnace easily reacts with the C atoms in the steel, causing the decarburization rate of the steel to exceed the oxidation rate.

[0050] In summary, in this experiment, the method for reducing the decarburization layer of 60Si2Mn spring steel billet is as follows: 1) the soaking section temperature is less than 1000℃; 2) the soaking section temperature is greater than 1200℃. Taking into account the actual production situation on site, when the soaking section temperature exceeds 1200℃, the decarburization layer depth is good in a short time, but the production organization is more difficult. After an accident on site, the decarburization layer will increase significantly with the increase of heating time, and there will even be a risk of furnace withdrawal. Too low heating temperature will increase the wear of the rolling groove on site and the production accidents of roll breakage. Therefore, in order to reduce the decarburization layer depth of 60Si2Mn spring steel, according to the experiment in this article, the best soaking section temperature in the heating furnace is 60min and the soaking section temperature is 1050℃.

[0051] Effect of rolling process on surface decarburization of 60Si2Mn spring steel;

[0052] The best heating process (soaking section temperature of 60min, soaking section temperature of 1050℃) was selected to study the effect of water penetration process after rolling on surface decarburization of 60Si2Mn spring steel. The temperature of the upper cooling bed was controlled at 900℃, 800℃, and 700℃. After the upper cooling bed, the samples were air-cooled. The sample analysis results are shown in the figure. Figure 4 As shown, a 900℃; b 800℃; c 700℃;

[0053] from Figure 4 It was found that when the upper cooling bed temperature was controlled at 1050℃ and the soaking section temperature was 60min, no complete decarburization layer was found. Only a partial decarburization layer was observed on the surface. The ferrite in the partial decarburization layer was distributed along the grain boundary. When the upper cooling bed temperature was controlled at 900℃, the decarburization layer temperature was 42um-45um. When the upper cooling bed temperature was 800-700℃, the decarburization layer depth was similar, which was 26um-39um and 21um-25um respectively.

[0054] Effect of Slow Cooling Process on Surface Decarburization of 60Si2Mn Spring Steel

[0055] The temperature of the soaking section of the heating process was selected as 60min, the temperature of the soaking section was 1050℃, and the temperature of the upper cooling bed of the rolling process was controlled as 700℃. By controlling the steel distribution method of the cooling bed and the opening degree of the cooling bed insulation cover, the influence of different slow cooling conditions on the surface decarburization layer of 60Si2Mn spring steel was studied. Table 3 shows the decarburization layer depth and hot-rolled hardness value of 60Si2Mn spring steel without slow cooling process. It can be found from Table 3 that the effect of the slow cooling rate of 0.5℃ / s-3.0℃ / s on the decarburization layer is negligible, but with the decrease of the slow cooling rate, its hot-rolled Brinell hardness gradually decreases. When the slow cooling process is 0.5℃ / s, the decarburization layer depth is 26um, and the hot-rolled Brinell hardness is 281HBW. Taking into account the actual application of customers, customers hope that the product processing hardness is low to reduce the wear of their tools. The cooling rate in the slow cooling process of 60Si2Mn spring steel is controlled to be less than 0.5℃ / s.

[0056] Table 3 shows the decarburization depth and hot rolling hardness of 60Si2Mn spring steel without slow cooling process

[0057]

[0058] Decarburization structure morphology of 60Si2Mn spring steel

[0059] The best process route samples of this experiment (heating process: soaking temperature for 60min, soaking temperature for 1050℃; rolling process: upper cooling bed temperature for 700℃; slow cooling process: cooling rate for 0.5℃ / s) were selected for metallographic analysis. Figure 5As shown in the figure, it is the metallographic diagram of the sample of the best process route, and its matrix structure is ferrite and pearlite. According to the research of Chen Yinli and others, when the carbon concentration on the surface of spring steel drops to the GS line, if the surface carbon concentration continues to decrease, it will enter the α+γ two-phase region. According to the phase law, during the decarburization process, the diffusion of carbon elements causes a sudden change in carbon concentration. Therefore, the result of decarburization is that a single ferrite phase appears on the surface, that is, complete decarburization occurs, while the original austenite area adjacent to the ferrite inside forms a partially decarburized structure. Figure 5 No complete decarburized layer structure was found. As the decarburized layer formed on the sample surface, the carbon concentration in the austenite gradually decreased from the surface to the inside and showed a linear change, accompanied by the generation of ferrite + pearlite.

[0060] Calculation Model of Decarburization Depth and Heating Time of 60Si2Mn Spring Steel

[0061] right Figure 3 The data in are linearly fitted. Table 4 shows the linear fitting relationship between the depth of decarburization layer and time at the same temperature, where y is the depth of decarburization layer um, and X is the soaking time min. From the fitting formula, the slope gradually increases with the increase of heating temperature. Therefore, in order to reduce the depth of decarburization layer of 60Si2Mn spring steel, according to the calculation model, the soaking temperature should be 1000℃. However, considering the actual situation on site, the soaking temperature is 1050℃, which is conducive to controlling accidents on the production site and improving production efficiency.

[0062]

[0063] Summarize

[0064] 1. Reduce the decarburization depth of 60Si2Mn spring steel and avoid production accidents. The optimal soaking temperature in the heating furnace is 60min and 1050℃. The decarburization depth and heating time are linearly fitted. With the increase of heating temperature, the slope gradually increases.

[0065] 2. Select the optimal heating process. When the upper cooling bed temperature is 800-700℃, the decarburization layer depths are similar, 26um-39um and 21um-25um respectively.

[0066] 3. With the decrease of slow cooling rate, the hot-rolled Brinell hardness gradually decreases. When the slow cooling process is 0.5℃ / s, the decarburization layer depth is 26um and the hot-rolled Brinell hardness is 281HBW.

[0067] 4. Select the best process route sample for this experiment (heating process: soaking section temperature is 60min, soaking section temperature is 1050℃; rolling process: upper cooling bed temperature is 700℃; slow cooling process: cooling rate is 0.5℃ / s). The matrix structure is ferrite and pearlite.

[0068] The embodiments of the present invention are described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the technical field without departing from the purpose of the present invention.

Claims

1. A decarburization method based on heating, rolling and slow cooling process, characterized in that: The following specific steps are included: S1 Heating process: In the actual production process of 60Si2Mn spring steel, surface decarburization mainly occurs during the heating process of the heating furnace; S2 rolling process: the production process of the steel rolling mill, the φ25mm (round steel with a diameter of 25mm) produced on site was selected as the test object, the rolling program table is shown in Table 2, the temperature of the upper cooling bed is controlled, the sample is taken at the cooling bed, and the metallographic specimen is made after air cooling; S3 slow cooling process: Keep the temperature of the upper cooling bed consistent, and control the opening degree of the cooling bed insulation cover to study the effect of the cooling rate on the cooling bed after rolling on the surface decarburization of 60Si2Mn spring steel.

2. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: In the S1 heating process, factors such as room temperature billet feeding into the furnace, slightly positive pressure in the furnace, and residual oxygen content being controlled ≤1% throughout the whole process are kept unchanged, and the effects of soaking section temperature and soaking section time on surface decarburization of 60Si2Mn spring steel are studied.

3. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: In the S1 heating process, the soaking stage is below 1000°C.

4. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: In the S1 heating process, the temperature of the soaking section is 1000-1250°C and the heating time in the soaking section is 60-300 minutes respectively.

5. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: In the S1 heating process, samples are taken at the flying shear, and metallographic samples are made through wire cutting, mounting, grinding, polishing, corrosion and other processing steps.

6. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: The S2 rolling process studies the effect of the temperature of the cooling bed after rolling on the surface decarburization of 60Si2Mn spring steel.

7. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: There is no complete decarburization on the surface of the 60Si2Mn continuous casting billet, and the total decarburization layer depth is 330-360um; there is local complete decarburization of 74um at the corner, and the total decarburization is 180-291um.

8. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: The temperature of the soaking section is 1000-1250°C, and the heating time in the soaking section is 60-300 minutes respectively. The test conditions are shown in Figure 3. It can be seen from Figure 3 that when heating in the soaking section for 60 minutes, within the temperature range of 1000°C to 1150°C, when the soaking section temperature increases, the depth of the decarburization layer increases. The reason is that the decarburization rate is greater than the oxidation rate. However, when the soaking section temperature exceeds 1150°C, the depth of the decarburization layer decreases with the increase of temperature.

9. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: In the process of heating the 60Si2Mn spring steel from low temperature to high temperature, when the temperature rises to 1150°C, the depth of the decarburization layer on the surface of the spring steel reaches a maximum value of 48.1um, and with the increase of the heating time in the soaking section, all curves show an obvious increasing trend. At 120 minutes, when the soaking section temperature is 1200°C and 1250°C, the decarburization layer on the surface of the material quickly surpasses the sample with the soaking section temperature ≤1150°C. With the extension of heating time and the increase of heating temperature, the iron oxide scale on the surface of the spring steel becomes thick, loose and porous, and the residual oxygen in the heating furnace easily reacts with the C atoms in the steel, causing the decarburization rate of the steel to exceed the oxidation rate.

10. The method for decarburization characteristics based on heating, rolling and slow cooling process according to claim 1, characterized in that: For the samples with the soaking section temperature of 60min and the soaking section temperature of 1050°C, no complete decarburization layer was found when the upper cooling bed temperature was controlled. Only a partial decarburization layer was observed on the surface. The ferrite in the partial decarburization layer was distributed along the grain boundary. When the upper cooling bed temperature was controlled at 900°C, the decarburization layer temperature was 42um-45um, and when the upper cooling bed temperature was 800-700°C, the decarburization layer depth was similar, which were 26um-39um and 21um-25um respectively.

Citation Information

Patent Citations

  • Manufacturing method of high-quality 60Si2Mn low-decarburization layer

    CN113699335A

  • Production method for eliminating full decarburization of Si-Cr series spring steel wire rod and prolonging fatigue life

    CN115870332A

  • Production method for improving depth of decarburized layer of hot-rolled 60Si2Mn spring round steel

    CN116024416A

  • Rolling method of spring steel with high fatigue performance

    CN116493424A

  • Production method of spring steel wire for automotive suspension

    CN116550750A

Cited By

  • 60Si2Mn spring steel hot-rolled wide coiled plate and preparation method thereof

    CN120885560A