Power transistor for industrial printing control system and manufacturing method thereof

Through the epitaxial plane process, ion implantation process and other technical means, the structure and process of power transistors are optimized, the oscillation and heating problems at high current frequency are solved, the reliability and stability of the product are improved, and high current gain and fast Switching speed.

CN119050135APending Publication Date: 2024-11-29WUXI KEC SEMICON CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411143161.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing power transistors with high current and high frequency are prone to oscillation and heating problems when used with load, which affects the reliability and stability of the product.

Method used

Adopt epitaxial plane process, ion implantation process, back multi-layer metal process and surface PSG+SI3N4 process, combined with TO-3PML insulated high-thermal conductivity full-inclusive packaging, optimize the control of base area depth, emission area depth and resistance increase ring, and improve ohmic contact and Thermal resistance.

Benefits of technology

It effectively solves the contradiction between saturation voltage drop and current capability, improves product reliability and stability, reduces heating problems, and enhances current gain and switching speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050135A_ABST
    Figure CN119050135A_ABST
Patent Text Reader

Abstract

The invention provides a power transistor for an industrial printing control system and a manufacturing method thereof, the power transistor comprises a chip, the chip comprises a substrate, a metal layer is arranged on the back of the substrate, a high-resistance layer region is arranged on the front of the substrate, a base region is arranged on the front of the high-resistance layer region, an emitter region and a resistance increasing ring are arranged on the front of the base region, and a second metal layer is arranged on the front of the emitter region; a first metal layer is arranged on the front surface of the base region except the part connected with the emitter region, and an insulating medium layer covers the outermost layer of the front surface of the substrate. According to the power transistor for the industrial printing control system and the manufacturing method of the power transistor, an epitaxial plane process is adopted, so that the contradiction between saturation voltage drop and current capability is solved; an ion implantation process is adopted to solve the control problem of a light boron base region; a back multi-layer metal process is adopted, so that good ohmic contact and thermal resistance are ensured; a surface PSG + SI3N4 process is adopted, so that the reliability and the stability of the product are ensured; tO-3PML insulating high-thermal-conductivity full-package packaging is adopted, so that the insulating application of the product is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a power transistor used in an industrial printing control system and a manufacturing method thereof. Background Art

[0002] Power transistors with high power, low saturation voltage drop and high hFE have a wide range of applications, such as printers, inverters, automotive electronic devices, DC converters, drives, etc. They have a large market demand and a very broad prospect. In these applications, the products are required to have high current, fast switching speed, low saturation voltage drop and high current gain. However, during the use of the domestically produced products with high current, high frequency, low saturation voltage drop and high gain, customers have reported that when the products are used with load and the load is gradually increased, obvious oscillations and severe heating will occur, which affects the reliability of the products.

[0003] The present invention aims at the problem and develops a power transistor pair 2SA1746 and 2SC4131 for industrial printing control system to meet the requirements of application manufacturers, especially the scale of industrial printing control system and 3D printing. The epitaxial planar process is adopted to solve the contradiction between saturation voltage drop and current capacity; the ion implantation process is adopted to solve the control problem of the light boron base area; the back multi-layer metal process is adopted to ensure good ohmic contact and thermal resistance; the surface PSG+SI3N4 process is adopted to ensure the reliability and stability of the product; the TO-3PML insulation high thermal conductivity full package is adopted to ensure the insulation application of the product. In particular, the control of base area depth, doping concentration and diffusion process, emission area depth, emission area expansion, phosphor lithography and other process controls have been well optimized. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a power transistor for an industrial printing control system and a method for manufacturing the same.

[0005] The technical solution adopted by the present invention is:

[0006] A power transistor for an industrial printing control system, wherein: the power transistor comprises a chip, the chip comprises a substrate, a metal layer is arranged on the back of the substrate, a high resistance layer region is arranged on the front of the substrate, a base region is arranged on a front side of the high resistance layer region away from the substrate, an emitter region and a resistance increasing ring arranged around the periphery of the emitter region are arranged on the front side of the base region, a second metal layer is arranged on the front side of the emitter region, a first metal layer is arranged on the front side of the base region except for a portion connected to the emitter region, an insulating dielectric layer is covered on the outermost layer of the front side of the substrate, and the first metal layer and the second metal layer except for a portion connected to the emitter region are isolated from the substrate by an insulating dielectric layer.

[0007] Preferably, the power transistor for an industrial printing control system, wherein: the substrate is a P+ type substrate, the high resistance layer region is a P- high resistance layer region, the base region is an N-type base region, and the emitter region is a P+ type emitter region; the thickness of the P+ type substrate is 240um±20um, and the thickness of the metal layer is 2.0-2.5um; the thickness of the P- high resistance layer region is 10um, the width of the N-type base region is 4.5-5.0um, the thickness of the first metal layer and the second metal layer is 4.5-5.2um, the depth of the P+ type emitter region is 2-3um, and the thickness of the insulating dielectric layer is 2-2.5um.

[0008] Preferably, the power transistor for an industrial printing control system, wherein: the substrate is an N+ type substrate, the high resistance layer region is an N- high resistance layer region, the base region is a P-type base region, and the emitter region is an N+ type emitter region; the thickness of the N+ type substrate is 231-240um, the thickness of the N- high resistance layer region is 14-18um, the depth of the P-type base region is 10-15um, the depth of the N+ emitter region is 5-7um, the thickness of the insulating dielectric layer is 2-4um, and the thickness of the first metal layer and the second metal layer is 4.5-5.2um.

[0009] Preferably, the power transistor for industrial printing control system, wherein: the insulating dielectric layer is a three-layer structure, a silicon dioxide layer in contact with the substrate, a PSG layer in the middle, and a Si3N4 layer on the surface; the back metal layer is a three-layer structure, a titanium layer in contact with the substrate, a nickel layer in the middle, and a silver layer on the bottom; the power transistor also includes a lead frame, solder, leads and an epoxy resin layer, the chip is arranged on the lead frame, solder and leads are arranged between the chip and the lead frame, and an epoxy resin layer is arranged on the periphery of the lead frame.

[0010] The present invention also provides a method for manufacturing a power transistor for an industrial printing control system, which comprises the following steps:

[0011] Step S1. Field oxidation: providing a silicon epitaxial wafer, inserting the silicon epitaxial wafer into a boat and pushing the silicon epitaxial wafer into a heating furnace for heating so that an oxide layer is formed on the silicon epitaxial wafer, thereby obtaining a first silicon epitaxial wafer;

[0012] Step S2. Photolithography base area: the first silicon epitaxial wafer is coated by a coating machine, and then development, hardening, etching, and wet stripping are performed in sequence to obtain a second silicon epitaxial wafer;

[0013] Step S3. Injection oxidation: insert the second silicon epitaxial wafer into the oxidation boat and send it into the diffusion furnace, and form the second silicon epitaxial wafer into a thickness of Oxide layer;

[0014] Step S4. Phosphorus implantation in the base region: Phosphorus ions are implanted into the second silicon epitaxial wafer after the oxidation in step S3 by an ion implanter;

[0015] Step S5. Base region re-diffusion: inserting the second silicon epitaxial wafer into which phosphorus has been implanted in the base region in step S4 into a diffusion boat and sending it into a diffusion furnace, and heat treating it in a nitrogen atmosphere to obtain a third silicon epitaxial wafer;

[0016] Step S6. Photolithography of the emission area: the third silicon epitaxial wafer is coated by a coating machine, followed by development, hardening, etching, and wet stripping in sequence;

[0017] Step S7. Coating photoresist: The third silicon epitaxial wafer after the photolithography emission area treatment in step S6 is coated by a coating machine, and then dried, oxidized, and rinsed in sequence to obtain a fourth silicon epitaxial wafer, and the resistance is controlled to be 4.5±1Ω, thereby forming a high resistance layer region on the surface of the fourth silicon epitaxial wafer;

[0018] Step S8. Boron re-expansion of the emitter region: the fourth silicon epitaxial wafer processed in step S7 is sent into a diffusion furnace for heat treatment in an oxygen and nitrogen atmosphere, and the heat temperature is controlled to be 1050±10°C, so that an emitter region is formed on the front side of the base region of the fourth silicon epitaxial wafer, and a resistance-increasing ring is formed around the emitter region;

[0019] Step S9. Phosphorus filling photolithography: the fourth silicon epitaxial wafer processed in step S8 is subjected to a coating machine, and then subjected to development, hardening, etching, and wet stripping treatments in sequence;

[0020] Step S10. Phosphorus supplementation diffusion oxidation: The diffusion furnace is heated to 1050±10°C, and nitrogen gas carrying a phosphorus source is introduced into the diffusion furnace for t1 time after the temperature is maintained. Then, the fourth silicon epitaxial wafer after phosphorus supplementation photolithography is inserted into an oxidation boat and sent into the diffusion furnace for oxidation under an oxygen atmosphere. The thickness of the oxide layer is controlled to be

[0021] Step S11. Photolithography of lead holes: The fourth silicon epitaxial wafer processed in step S10 is subjected to a coating machine, and then subjected to pre-baking, film hardening, and wet stripping in sequence to obtain a fifth silicon epitaxial wafer;

[0022] Step S12. Vaporizing aluminum on the front side: Vapor-depositing an aluminum film with a thickness of 4.5-5.2 um on the fifth silicon epitaxial wafer through a high vacuum electron beam evaporation station;

[0023] Step S13. Photolithography of aluminum: The fifth silicon epitaxial wafer processed in step S12 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence;

[0024] Step S14. Surface aluminum evaporation: The fifth silicon epitaxial wafer processed in step S13 is subjected to surface aluminum evaporation in a nitrogen atmosphere to form a second metal layer on the front side of the emitter region, and a first metal layer is formed on the front side of the base region except for the portion connected to the emitter region;

[0025] Step S15. Deposition of protective layer: Covering the outermost layer of the front side of the fifth silicon epitaxial wafer processed in step S14 with an insulating dielectric layer;

[0026] Step S16. Bonding area photolithography: The fifth silicon epitaxial wafer processed in step S15 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence;

[0027] Step S17. Heat treatment: heat-treating the fifth silicon epitaxial wafer processed in step S16 in a nitrogen atmosphere; then thinning the ninth silicon epitaxial wafer to control the thickness of the ninth silicon epitaxial wafer to 260±10 um, to obtain the sixth silicon epitaxial wafer;

[0028] Step S18. Back metallization: The sixth silicon epitaxial wafer is subjected to Ti-Ni-Ag evaporation through an electron beam evaporation station, thereby forming a metal layer on the back of the sixth silicon epitaxial wafer to obtain a chip;

[0029] Step S19. Saw blade: saw the chip into individual dies;

[0030] Step S20. Finished product: The tube core is sequentially mounted, bonded, plastic-sealed, electroplated and cut to obtain a power transistor for an industrial printing control system.

[0031] Preferably, the method for manufacturing a power transistor for an industrial printing control system, wherein: the heating in step S1 is specifically: introducing oxygen and heating to 1150±15°C, controlling the oxygen flow rate to 5-6L / min, then introducing a mixture of oxygen and hydrogen and maintaining it for 80 minutes, and finally introducing oxygen and maintaining it for 40 minutes, controlling the oxide layer thickness to 0.6-0.7μm.

[0032] Preferably, the method for manufacturing a power transistor for an industrial printing control system, wherein: the base region photolithography in step S2, the emitter region photolithography in step S6, and the phosphorus-filling photolithography in step S9 all specifically include the following steps:

[0033] S21. Spinning glue: Spinning glue on the first silicon epitaxial wafer or the third silicon epitaxial wafer or the fourth silicon epitaxial wafer by a spinner, controlling the speed to 6000-7000rpm, the spin time to 30-40s, the pre-baking temperature to 100±5℃, the time to 25-30min, the exposure to mask the B area, ultraviolet exposure, and the exposure time to 6-8s;

[0034] S22. Development: Immerse the first silicon epitaxial wafer, the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after the coating in a developing liquid for 6-8 minutes;

[0035] S23. Hard film: heat treating the first silicon epitaxial wafer or the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after development, controlling the heat treatment temperature to 130±8°C for 30-40min;

[0036] S24. Etching: treating the first silicon epitaxial wafer, the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after hardening in an etching solution for 6-8 minutes, and controlling the temperature of the etching solution to be 38±2°C;

[0037] S25. Wet degumming: Degumming the first silicon epitaxial wafer, the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after corrosion in a degumming solution for 6-8 minutes, and then rinsing with water for 10-12 times to obtain a second silicon epitaxial wafer. The degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4.

[0038] Preferably, the method for manufacturing a power transistor for an industrial printing control system, wherein: the heat treatment in step S5 is specifically as follows: when the temperature of the diffusion furnace reaches 800±5°C, the second silicon epitaxial wafer is sent into the constant temperature zone of the diffusion furnace, the nitrogen flow rate is controlled to 4-6L / min, and then the temperature is increased for 35min-40min to the temperature of 1100±5°C, and then annealing is performed for 30-50min at a nitrogen flow rate of 4-6L / min, and finally the temperature is increased for 30-40min to the temperature of 1170°C±5°C for diffusion for 140-160min, and H2 and O2 are introduced for oxidation at the same time, and then the temperature is reduced to 800°C to take the second silicon epitaxial wafer out of the diffusion furnace, and it is naturally cooled to obtain a third silicon epitaxial wafer.

[0039] Preferably, in the method for manufacturing a power transistor for an industrial printing control system, the step of coating the photoresist in step S7 specifically comprises the following steps:

[0040] Step S71: Spreading the third silicon epitaxial wafer through a spreader, controlling the speed of the spreader to be 6000-7000 rpm, and the spread time to be 32-40 s;

[0041] Step S72: pre-baking: pre-baking the third silicon epitaxial wafer after the coating at 90-100°C for 1 hour;

[0042] Step S73. Oxidation: insert the third silicon epitaxial wafer after pre-baking into a boat, put it into a diffusion furnace, and oxidize it at 1050°C-1100°C for 90-120min while introducing N2, H2 and O2;

[0043] Step S74. Rinse: Treat the oxidized third silicon epitaxial wafer in the etching solution for 1.5-2 minutes, rinse 10-12 times, and then spin dry.

[0044] Preferably, the method for manufacturing a power transistor for an industrial printing control system, wherein: in step S10, t1 is 1.35-1.75h, the oxidation time is 10-15min, and the oxidation temperature is 1050±10°C; in step S14, the temperature of surface aluminum vaporization is 480-515°C, and the time is 20-30min; in step S17, the temperature of heat treatment is 395-405°C, and the time is 20-30min;

[0045] Step S20: loading the film includes the following specific steps:

[0046] Step S201. Place the lead frame into the loading mechanism of the high-speed automatic chip loader, and insert high-temperature soft solder 20 at the chip mounting position on the lead frame. Control the compressed air pressure in the high-speed automatic chip loader to be 0.35-0.6MPa, and the vacuum degree to be -80 to -100KPa. The high-speed automatic chip loader includes 8 temperature zones, and the controlled temperatures are: 300℃±5℃, 375℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 380℃±5℃, 320℃±5℃, and introduce hydrogen and nitrogen mixed gas to control the total flow rate of the mixed gas to be: 15-25L / min;

[0047] Step S202. Automatically pick up the chip into the solder on the lead frame through a suction nozzle;

[0048] Step S203: The lead frame with the chip mounted on it automatically enters the material box through the tinning, lamination, shaping, core mounting and cooling zone of the chip mounting machine track.

[0049] Advantages of the present invention:

[0050] The power transistor for industrial printing control system of the present invention and the manufacturing method thereof adopt an epitaxial planar process to solve the contradiction between saturation voltage drop and current capacity; adopt an ion implantation process to solve the control problem of the light boron base area; adopt a back-side multi-layer metal process to ensure good ohmic contact and thermal resistance; adopt a surface PSG+SI3N4 process to ensure product reliability and stability; adopt a TO-3PML insulating high thermal conductivity full package to ensure the insulation application of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a cross-sectional view of the chip of the present invention.

[0052] Figure 2 It is a front view of a power transistor used in an industrial printing control system according to the present invention.

[0053] Figure 3 It is a side view of the power transistor used in the industrial printing control system of the present invention. DETAILED DESCRIPTION

[0054] The present invention will be further described below in conjunction with specific drawings and embodiments.

[0055] A method for manufacturing a power transistor for an industrial printing control system, comprising the following steps:

[0056] Step S1. Field oxidation: Provide a silicon epitaxial wafer, the resistivity of the silicon epitaxial wafer is 7.6-8.4Ω.cm, and the thickness is 14-15um. Since too high a resistivity will increase the saturation voltage drop of the product, too low a resistivity will affect the breakdown voltage of the product, the overall thickness of the chip = 465±20um, insert the silicon epitaxial wafer into a boat and push it into a heating furnace for heating so that an oxide layer is formed on the silicon epitaxial wafer, and obtain a first silicon epitaxial wafer;

[0057] The heating in step S1 is specifically as follows: dry oxygen is introduced and the temperature is raised to 1150±15°C, the heating time is 4h, the oxygen flow rate is controlled at 5-6L / min, when the temperature rises to 1150±15°C, wet oxygen (oxygen + hydrogen mixture, O2 flow rate is 4000±400ml / min, H2 flow rate is 4700±470ml / min) is then introduced, and maintained for 80min, and finally dry oxygen is introduced and maintained for 40min, the thickness of the oxide layer is controlled to be 0.6-0.7μm, effectively ensuring the required breakdown voltage.

[0058] Step S2. Photolithography base area: the first silicon epitaxial wafer is coated by a coating machine, and then development, hardening, etching, and wet stripping are performed in sequence to obtain a second silicon epitaxial wafer;

[0059] Step S2. Photolithography of the base region specifically includes the following steps:

[0060] S21. Spreading glue: Select HFJ220 spread glue agent and add a spread glue machine, pass the first silicon epitaxial wafer through the spread glue machine, control the speed to 6000-7000rpm, the spread glue time is 30-40s, the pre-baking temperature is 100±5℃, the time is 25-30min, the exposure is masked with the B area plate, ultraviolet exposure, and the exposure time is controlled to be 6-8s;

[0061] S22. Development: The first silicon epitaxial wafer after the coating is immersed in the HFJ2200 developer liquid for 6-8 minutes to ensure high-quality development effect;

[0062] S23. Hardening: The first silicon epitaxial wafer after development is subjected to heat treatment, and the heat treatment temperature is controlled to be 130±8°C for 30-40 minutes. In this process, the high temperature treatment can remove the remaining solvent in the photoresist, enhance the adhesion of the photoresist to the silicon wafer surface, and improve the corrosion resistance of the photoresist in the subsequent etching and ion implantation processes. At the same time, the photoresist will soften at high temperature to form a molten state similar to glass at high temperature, which will make the surface of the photoresist smooth under the action of surface tension and reduce defects (such as pinholes) in the photoresist layer;

[0063] S24. Etching: The first silicon epitaxial wafer after hardening is treated in an etching solution for 6-8 min, the temperature of the etching solution is controlled to be 38 ± 2 ° C, the etching solution comprises a mixture of HF (concentration 42%), NH4F (concentration 96%) and deionized water, HF: NH4F: deionized water = 1 mL: 2 g: 3.3 mL, the temperature is controlled at 38 ± 2 ° C, the time is 6-8 min, and the rinse is 10-12 times;

[0064] S25. Wet degumming: degumming the first silicon epitaxial wafer after etching in a degumming solution for 6-8 minutes, and then rinsing with water 10-12 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4;

[0065] Step S3. Injection oxidation: insert the second silicon epitaxial wafer into the oxidation boat and send it into the diffusion furnace, and form the second silicon epitaxial wafer into a thickness of The oxidation layer was formed by controlling the oxygen flow rate at 4 L / min and the oxidation time at 10 min.

[0066] Step S4. Phosphorus implantation in the base region: Phosphorus ions are implanted into the second silicon epitaxial wafer after the oxidation in step S3 through an ion implanter. The ion implanter sets the energy and number of ions to be implanted, and the second silicon epitaxial wafer is implanted with accurately measured phosphorus ions. The implantation metering is 2.7E13. The advantages of ion implantation include less pollution and good uniformity of implantation within the wafer, between wafers, and between batches.

[0067] Step S5. Base region re-diffusion: inserting the second silicon epitaxial wafer into which phosphorus has been implanted in the base region in step S4 into a diffusion boat and sending it into a diffusion furnace, and heat treating it in a nitrogen atmosphere to obtain a third silicon epitaxial wafer;

[0068] The heat treatment in step S5 is specifically as follows: when the temperature of the diffusion furnace reaches 800±5℃, the second silicon epitaxial wafer is sent into the constant temperature zone of the diffusion furnace, the nitrogen flow rate is controlled at 4-6L / min, and then the temperature is increased for 35min-40min to the temperature of 1100±5℃, and then annealing is performed for 30-50min at a nitrogen flow rate of 4-6L / min, and finally the temperature is increased for 30-40min to the temperature of 1170℃±5℃ for diffusion for 140-160min, and H2 and O2 are introduced for oxidation at the same time, and then the temperature is reduced to 800℃ to take the second silicon epitaxial wafer out of the diffusion furnace, and it is naturally cooled to obtain a third silicon epitaxial wafer.

[0069] Step S6. Photolithography of the emission area: the third silicon epitaxial wafer is coated by a coating machine, followed by development, hardening, etching, and wet stripping in sequence;

[0070] Step S6: photolithography of the emission area specifically includes the following steps:

[0071] S21. Spreading glue: Spread the third silicon epitaxial wafer by a glue machine, control the speed to 6000-7000rpm, the glue time to 30-40s, the pre-bake temperature to 100±5℃, the time to 25-30min, the exposure to the B area mask, ultraviolet exposure, control the exposure time to 6-8s;

[0072] S22. Development: Immerse the third silicon epitaxial wafer after the coating in the developing liquid for 6-8 minutes;

[0073] S23. Hard film: The third silicon epitaxial wafer after development is heat treated, and the heat treatment temperature is controlled to be 130±8°C and the time is 30-40min;

[0074] S24. Etching: The third silicon epitaxial wafer after hardening is treated in an etching solution for 6-8 minutes, and the temperature of the etching solution is controlled to be 38±2°C; the etching solution includes HF (concentration 42%): NH4F (concentration 96%): deionized water = 1mL: 2g: 3.3mL, the etching time is 6-8min, and the washing is performed 10-12 times;

[0075] S25. Wet degumming: degumming the third silicon epitaxial wafer after etching in a degumming solution for 6-8 minutes, and then rinsing with water 10-12 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4;

[0076] Since the base current generates a voltage drop when passing through the base resistor, the bias voltages in different areas of the transistor emitter junction are not equal. There is an EXP relationship between the emitter current and the emitter junction bias voltage, so as long as the emitter bias voltage is slightly different, the emitter current will change greatly. When the operating current of the transistor is large, the voltage drop generated by the base current passing through the base resistor is also large, which makes the distribution of the emitter current on the emitter junction extremely uneven. In practice, the distribution of the emitter is that the closer to the base contact, the greater the current, and the current drops quickly to a very small value at a distance from the base. This emitter edge collection effect can also be considered as the base resistor self-bias effect. The current edge collection effect makes the entire emitter junction only effective near the edge of the base contact. The emitter region doping adopts high-concentration CSD diffusion to improve the injection efficiency. During ion implantation, the emitter junction depth is controlled to 2-2.5um, the chip surface state is improved, and the injection efficiency is improved. From the process point of view, it is guaranteed that the product has a higher characteristic frequency, faster switching speed, extremely high current gain, and uniformity of the diffusion parameter hFE.

[0077] Step S7. Coating photoresist: The third silicon epitaxial wafer after the photolithography emission area treatment in step S6 is coated by a coating machine, and then dried, oxidized, and rinsed in sequence to obtain a fourth silicon epitaxial wafer, and the resistance is controlled to be 4.5±1Ω, thereby forming a high resistance layer region 2 on the surface of the fourth silicon epitaxial wafer;

[0078] The photoresist coating process specifically comprises the following steps:

[0079] Step S71. Spreading glue: Select HFJ220 glue agent and add it to the glue machine, pass the fourth silicon epitaxial wafer through the glue machine, control the speed to 6000-7000rpm, the glue time is 30-40s, and evenly coat the glue agent on the front of the fourth silicon epitaxial wafer;

[0080] Step S72: pre-baking: placing the fourth silicon epitaxial wafer in a clean oven and drying it at 90°C-100°C for 1 hour to ensure that the solvent of the latex source is fully volatilized;

[0081] Step S73. Oxidation: insert the fourth silicon epitaxial wafer into a boat and place it into a diffusion furnace, oxidize it at 1050°C-1100°C for 90-120min, and introduce N2, H2 and O2 at the same time; the flow rate of N2 is 4000±400ml / min, the flow rate of O2 is 4000±400ml / min, and the flow rate of H2 is 4700±470ml / min;

[0082] Step S74. Rinse: Place the fourth silicon epitaxial wafer in a rinse solution of HF (concentration 42%): NH4F (concentration 96%): deionized water = 1 mL: 2 g: 3.3 mL for rinsing, control the temperature to 38 ± 2 ° C, the time to 1.5-2 min, rinse 10-12 times, then spin dry, and inspect, and measure the resistance of the fourth silicon epitaxial wafer to be 4.5 ± 1Ω;

[0083] Step S8. Boron expansion of the emitter region: The fourth silicon epitaxial wafer processed in step S7 is sent to a diffusion furnace for heat treatment in an oxygen and nitrogen atmosphere. The pipeline nitrogen flow rate is controlled to be 5L / min, the oxygen flow rate is 2L / min, and the heat temperature is controlled to be 1050±10°C. After heating for 4h to reach 1050±10°C, nitrogen is introduced for a time of t=1.55±0.2h, the nitrogen is turned off, the temperature is kept constant for 15 minutes, the temperature is lowered to 700°C, taken out, and sent to the inspection Xj=2-2.5um oxide layer thickness: An emitter region 4 is formed on the front of the base region 3 of the fourth silicon epitaxial wafer, and a resistance-increasing ring 5 is formed around the emitter region 4; the resistance-increasing ring 5 is independent of the emitter junction and the base region lead hole, does not participate in the conduction, and forms isolation, thereby blocking the lateral flow of the base region injection current. The base region current cannot flow directly to the emitter junction surface, but flows evenly under the emitter junction, thereby weakening the emitter current edge collection effect when the transistor is working at a large current, reducing the current concentration of the emitter junction, improving the product heating problem, and improving the controllability of the product;

[0084] Step S9. Phosphorus filling photolithography: the fourth silicon epitaxial wafer processed in step S8 is subjected to a coating machine, and then subjected to development, hardening, etching, and wet stripping treatments in sequence;

[0085] Step S9 phosphor-filling lithography specifically includes the following steps:

[0086] S21. Spreading glue: Spread the fourth silicon epitaxial wafer by a glue machine, control the speed to 6000-7000rpm, the glue time is 30-40s, the pre-bake temperature is 100±5℃, the time is 25-30min, the exposure is masked with a B-area plate, ultraviolet exposure, and the exposure time is controlled to be 6-8s;

[0087] S22 development: the fourth silicon epitaxial wafer after the coating is immersed in the developing liquid for 6-8min;

[0088] S23. Hardening: The fourth silicon epitaxial wafer after development is heat treated, and the temperature of the heat treatment is controlled to be 130±8℃, and the time is 30-40min. In this process, the high temperature treatment can remove the remaining solvent in the photoresist, enhance the adhesion of the photoresist to the surface of the silicon wafer, and improve the corrosion resistance of the photoresist in the subsequent etching and ion implantation processes. At the same time, the photoresist will soften at high temperature, forming a molten state similar to glass at high temperature, which will make the surface of the photoresist smooth under the action of surface tension and reduce defects (such as pinholes) in the photoresist layer;

[0089] S24. Etching: The fourth silicon epitaxial wafer after hardening is treated in an etching solution for 6-8 minutes, and the temperature of the etching solution is controlled to be 38±2°C; the etching solution includes HF (concentration 42%): NH4F (concentration 96%): deionized water = 1mL: 2g: 3.3mL, the etching time is 6-8min, and the washing is performed 10-12 times;

[0090] S25. Wet degumming: Degumming the fourth silicon epitaxial wafer after etching in a degumming solution for 6-8 minutes, and then rinsing with water for 10-12 times to obtain a second silicon epitaxial wafer. The degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4.

[0091] Step S10. Phosphorus supplementation diffusion oxidation: The temperature of the constant temperature zone of the diffusion furnace is raised to 1050±10°C for about 30 minutes. After the constant temperature, nitrogen carrying a phosphorus source is introduced into the diffusion furnace for 1.35-1.75 hours, the nitrogen is turned off, and the temperature is kept constant for 15 minutes. Then, the fourth silicon epitaxial wafer that has undergone phosphorus supplementation lithography is inserted into an oxidation boat and sent into the diffusion furnace for oxidation in an oxygen atmosphere. The oxidation time is 10-15 minutes, the oxygen flow rate is controlled at 4L / min, the oxidation temperature is 1050±10°C, and the thickness of the oxide layer is controlled to be

[0092] Step S11. Photolithography of lead holes: The fourth silicon epitaxial wafer processed in step S10 is subjected to a coating machine, and then subjected to pre-baking, film hardening, and wet stripping in sequence to obtain a fifth silicon epitaxial wafer;

[0093] Step S11 of photolithography of lead holes specifically includes the following steps:

[0094] S110. Spreading glue: BN308 glue is selected as a spreader and added to a spreader, and the fourth silicon epitaxial wafer is spread by a spreader, and the speed is controlled to be 3000rpm and the spread time is 40s;

[0095] S111. Pre-baking: pre-baking the fourth silicon epitaxial wafer after the coating, controlling the temperature at 100±5°C for 25-30min, masking the lead frame, and exposing to ultraviolet light for 6-9s;

[0096] S112. Hard film: The fourth silicon epitaxial wafer after pre-baking was heat treated, and the heat treatment temperature was controlled to be 140±5°C for 30-40min; the window SiO2 was etched with HF (concentration 42%): NH4F (concentration 96%): deionized water = 1mL: 2g: 3.3mL, the temperature was controlled to be 38±2°C, the time was 6-8min, and the rinse was performed 10-12 times;

[0097] S113. Wet degumming: degumming the etched fourth silicon epitaxial wafer in a degumming solution for 6-8 minutes, and then rinsing with water 10-12 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is 98% concentrated sulfuric acid and 35% hydrogen peroxide in a volume ratio of 1:4;

[0098] Step S12. Front aluminum evaporation: The fifth silicon epitaxial wafer is evaporated into an aluminum film with a thickness of 4.5-5.2um by a high vacuum electron beam evaporation table; pre-evacuation is performed according to the equipment operating procedures. When the pressure reaches below 2Mpa, the extraction valve is closed and the high valve is opened. The vacuum chamber is controlled to a pressure of 4*10 -3 Mpa, temperature control 180℃, time 30min, turn off the baking power; when the vacuum reaches 2*10 -3 Mpa, delay 2-3 minutes, turn on the high-voltage current aluminum source for pre-melting: control 0.4A slow steaming for 4min, 0.6A, 30-40 minutes, the thickness of the aluminum layer is controlled moderately, which greatly reduces the damage to the product in the subsequent packaging bonding process, and even causes crater problems, reduces the contact resistance between the bonding wire and the aluminum layer on the chip surface, and improves the bonding strength between the aluminum wire and the chip aluminum layer.

[0099] Step S13. Photolithography of aluminum: The fifth silicon epitaxial wafer processed in step S12 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence;

[0100] Step S13 of photolithography of aluminum specifically includes the following steps:

[0101] S130. Spreading glue: BN308 glue is selected as a spreader and added to a spreader, and the fourth silicon epitaxial wafer is spread by a spreader, and the speed is controlled to be 3000rpm and the spread time is 40s;

[0102] S131 pre-baking: pre-baking the fifth silicon epitaxial wafer after the coating, controlling the temperature at 100±5°C for 25-30min, masking the lead hole plate, and exposing to ultraviolet light for 6-9s;

[0103] S132. Hard film: The fifth silicon epitaxial wafer after pre-baking was heat treated, and the heat treatment temperature was controlled to be 140±5°C for 30-40min; the window SiO2 was etched with HF (concentration 42%): NH4F (concentration 96%): deionized water = 1mL: 2g: 3.3mL, the temperature was controlled to be 38±2°C, the time was 6-8min, and the rinse was performed 10-12 times;

[0104] S133. Wet degumming: degumming the fourth silicon epitaxial wafer after etching in a degumming solution for 6-8 minutes, and then rinsing with water 10-12 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is 98% concentrated sulfuric acid and 35% hydrogen peroxide in a volume ratio of 1:4;

[0105] Step S14. Surface aluminum evaporation: The fifth silicon epitaxial wafer processed in step S13 is subjected to surface aluminum evaporation in a nitrogen atmosphere to form a second metal layer 8 on the front side of the emitter region 4, and a first metal layer 7 is formed on the front side of the base region 3 except for the portion connected to the emitter region 4; the surface aluminum evaporation temperature in step S14 is 480-515°C, the time is 20-30min, and the nitrogen flow rate is controlled to be 5L / min;

[0106] Step S15. Deposition of protective layer: Covering the outermost layer of the front side of the fifth silicon epitaxial wafer processed in step S14 with the insulating dielectric layer 6;

[0107] The insulating dielectric layer is SiO2+phosphosilicate glass PSG+Si3N4, with a thickness of about 2-3um; although SiO2 is very stable in mechanical, chemical and electrical aspects and has a good passivation effect, SiO2 has poor masking ability for alkaline metal ions such as Na+ and K+. Phosphosilicate glass PSG has the function of extracting, fixing and blocking sodium ions, which can significantly weaken the influence of mobile ions such as sodium on the surface properties of semiconductors and reduce leakage current. The outermost layer is the Si3N4 layer, which has a tight structure, low pinhole density, and is difficult for gas and water vapor to penetrate. It has a strong masking ability, which can weaken the influence of impurities on the outer surface of the dielectric layer, has good chemical stability, and has a strong sodium resistance. It has high hardness and provides mechanical protection for metal interconnects and terminal metals.

[0108] Step S16. Bonding area photolithography: The fifth silicon epitaxial wafer processed in step S15 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence;

[0109] Step S16: the bonding area photolithography specifically includes the following steps:

[0110] S160. Spreading glue: BN308 glue is selected as a spreader and added to a spreader, and the fourth silicon epitaxial wafer is spread by a spreader, and the speed is controlled to be 3000rpm and the spread time is 40s;

[0111] S161. Pre-baking: pre-baking the fifth silicon epitaxial wafer after the coating, controlling the temperature at 100±5°C for 25-30min, masking the lead frame, and exposing to ultraviolet light for 6-9s;

[0112] S162. Hard film: Heat-treat the fifth silicon epitaxial wafer after pre-baking, control the heat treatment temperature to 140±5°C, and the time to 30-40min; etch the window SiO2, use HF (concentration 42%): NH4F (concentration 96%): deionized water = 1mL: 2g: 3.3mL, control the temperature to 75±2°C, the time to 6-8min, and rinse 10-12 times;

[0113] S163. Wet degumming: degumming the etched fourth silicon epitaxial wafer in a degumming solution for 6-8 minutes, and then rinsing with water 10-12 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is 98% concentrated sulfuric acid and 35% hydrogen peroxide in a volume ratio of 1:4;

[0114] Step S17. Heat treatment: heat treat the fifth silicon epitaxial wafer treated in step S16 in a nitrogen atmosphere; then reduce the thickness of the ninth silicon epitaxial wafer to 260±10um to obtain the sixth silicon epitaxial wafer; the heat treatment temperature in step S17 is 395-405°C, the time is 20-30min, and the nitrogen flow rate is controlled to 5L / min;

[0115] Step S18. Back metallization: The sixth silicon epitaxial wafer is subjected to Ti-Ni-Ag evaporation through an electron beam evaporation station, thereby forming a metal layer 9 on the back of the sixth silicon epitaxial wafer to obtain a chip;

[0116] Ti-Ni-Ag was deposited on the electron beam evaporation table according to the equipment operation card. The thickness of Ti is The thickness of Ni is The thickness of Ag is 1-1.5um, and the total thickness is controlled at 2-2.5um to ensure good ohmic contact and thermal resistance, especially forming a very good alloy layer together with high-temperature soft solder, ensuring very low thermal resistance and high reliability of this device. Ink dot screening is used to screen defective chips, and the test instrument JUNO automatic test bench is used to test parameters such as VEBO, VCEO, VCBO, IEBO, ICBO, and hFE.

[0117] Step S19. Saw blade: saw the chip into individual dies;

[0118] Step S20. Finished product: The tube core is sequentially mounted, bonded, and plastic-sealed to obtain a power transistor for an industrial printing control system.

[0119] Step S20: loading the film includes the following specific steps:

[0120] Step S201. Place the lead frame 10 into the loading mechanism of the high-speed automatic chip loader, and insert high-temperature soft solder 20 at the chip mounting position on the lead frame. The high-temperature soft solder 20 includes 92.5 lead, 5 tin and 2.5 silver. The compressed air pressure in the high-speed automatic chip loader is controlled to be 0.35-0.6MPa, and the vacuum degree is -80 to -100KPa. The high-speed automatic chip loader includes 8 temperature zones, and the controlled temperatures are: 300℃±5℃, 375℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 380℃±5℃, 320℃±5℃, and hydrogen and nitrogen mixed gas is introduced to control the total flow rate of the mixed gas to be: 15-25L / min;

[0121] Step S202. Automatically pick up the chip 30 into the solder 20 on the lead frame 10 through a suction nozzle;

[0122] Step S203. The lead frame with the loaded chip is automatically put into the material box through the cooling zone of the chip loading machine track, tinning, film pressing, shaping, core loading, and cooling process. This process is fully matched to ensure that the overall chip void rate is less than 5% and the single chip void rate is less than 2%, ensuring good transient thermal resistance VBE and high reliability of the product.

[0123] Bonding involves the following steps:

[0124] S204. Place the lead frame 10 with the chip 30 on the feeding mechanism of the automatic ultrasonic bonding machine for bonding. The lead wire 40 is 99.99% high-purity aluminum wire with a diameter of 300um, 1 E pole and 1 B pole;

[0125] (1) Wedge blade: YH-153-12mil, wire nozzle specification: YH-7200-W12; (2) Control the ultrasonic power, pressure, and time of the bonding machine. The parameter settings are shown in Table 1.

[0126] Table 1

[0127] Solder point location Power Pressure F Time T One solder joint (chip) 700±50 450±20 120±10 Two solder joints (lead frame) 800±50 500±30 120±20

[0128] (3) Control of solder joint length: 375-750um; solder joint width: 300-500um; (4) Control of bonding wire tension F: 400-600N; control of solder joint core thrust: 800-1200; the angle between the bonding point and the aluminum wire is greater than 90°, and the height of the bonding arch wire is controlled to be less than 3.5mm. The well-bonded product has no cold solder joints, no craters, and no twisting of the aluminum wire, which fully guarantees the product's ability to pass large currents and can reduce the product's Vce (sat) saturation voltage drop parameters. At the same time, the solder joint and the chip are fully and effectively connected, ensuring that the solder joint is not broken or loose after the reliability test, further ensuring the high reliability of the product.

[0129] Plastic packaging includes the following specific steps:

[0130] Step S205: The bonded product is further encapsulated with epoxy resin 50. The epoxy resin is KHG400 produced by Soienohem, Φ48mm, 108g / piece, an environmentally friendly plastic encapsulation material specially used for encapsulating fully encapsulated high-power devices, with high thermal conductivity and high reliability. The main control parameters are shown in Table 2;

[0131] Table 2

[0132]

[0133]

[0134] (1) After the plastic encapsulation material is taken out of the cold storage, it is warmed up for 24 hours, with a temperature of 23±2℃ and a relative humidity of 50±15%; (2) Temperature control of the injection molding press: the upper mold setting temperature is 185±5℃, and the lower mold setting temperature is 185±5℃; high-frequency preheating time: 27±2s, transfer time: 20s±2s, injection time: 50s±5s, injection pressure: 4-8MPa, in-mold curing time: 150-180s, post-curing process is 175, and post-curing time is 6-8h; TO-3PML plastic encapsulation mold, 80 cavities; the appearance of the product after plastic encapsulation is complete, without voids, bubbles, corners, or pinholes. By using halogen-free and environmentally friendly materials with high thermal conductivity and low water absorption, and adopting the preferred injection molding process, the product's appearance size and high thermal conductivity of the product are ensured, laying a high reliability foundation for the application of device products in high temperature environments.

[0135] The electroplating cutting process specifically includes the following steps:

[0136] Step S206: electroplating high-purity tin Sn, controlling the thickness of the tin layer to 5-15um, using high-speed line electroplating to ensure uniform thickness of the product tin layer, ensuring the product's 260°C, 10s wave soldering process, ensuring the product's high-reliability process adaptability, and controlling the cutting force to 6±1Mpa to prevent excessive force from causing stress that affects the reliability of the chip.

[0137] Example 1

[0138] like Figure 1-3, a power transistor for an industrial printing control system, wherein: the power transistor includes a chip 30, the chip 30 includes a substrate 1, a metal layer 9 is arranged on the back of the substrate 1, a high resistance layer area 2 is arranged on the front of the substrate 1, a base area 3 is arranged on a front side of the high resistance layer area 2 away from the substrate 1, an emitter area 4 and a resistance increasing ring 5 arranged around the periphery of the emitter area 4 are arranged on the front side of the base area 3, a second metal layer 8 is arranged on the front side of the emitter area 4, a first metal layer 7 is arranged on the front side of the base area 3 except for the part connected to the emitter area 4, the outermost layer on the front side of the substrate is covered with an insulating dielectric layer 6, and the first metal layer 7 and the second metal layer 8 except for the part connected to the emitter area 4 are isolated from the substrate by the insulating dielectric layer 6.

[0139] The substrate 1 is a P+ type substrate, the high resistance layer region 2 is a P- high resistance layer region, the base region 3 is an N-type base region, and the emitter region 4 is a P+ type emitter region; the thickness of the P+ type substrate 1 is 240um±20um, and the thickness of the metal layer 9 is 2.0-2.5um; the thickness of the P- high resistance layer region 2 is 10um, the width of the N-type base region 3 is 4.5-5.0um, the thickness of the first metal layer 7 and the second metal layer 8 is 4.5-5.2um, the depth of the P+ type emitter region 4 is 2-3um, and the thickness of the insulating dielectric layer 6 is 2-2.5um.

[0140] The substrate 1 is an N+ type substrate, the high resistance layer region 2 is an N- high resistance layer region, the base region 3 is a P-type base region, and the emitter region 4 is an N+ type emitter region; the thickness of the N+ type substrate 1 is 231-240um, the thickness of the N- high resistance layer region is 14-18um, the depth of the P-type base region is 10-15um, the depth of the N+ emitter region is 5-7um, the thickness of the insulating dielectric layer 6 is 2-4um, and the thickness of the first metal layer 7 and the second metal layer 8 is 4.5-5.2um.

[0141] The insulating dielectric layer 6 is a three-layer structure, wherein a silicon dioxide layer is in contact with the substrate 1, a PSG layer is in the middle, and a Si3N4 layer is on the surface; the back metal layer 9 is a three-layer structure, wherein a titanium layer is in contact with the substrate, a nickel layer is in the middle, and a silver layer is on the bottom; the power transistor further comprises a lead frame 10, solder 20, leads 40, and an epoxy resin layer 50, wherein the chip 30 is arranged on the lead frame 10, solder 20 and leads 40 are arranged between the chip 30 and the lead frame 10, and an epoxy resin layer 50 is arranged on the periphery of the lead frame 10.

[0142] Example 2

[0143] A method for manufacturing a power transistor for an industrial printing control system, comprising the following steps:

[0144] Step S1. Field oxidation: Provide a silicon epitaxial wafer, the resistivity of the silicon epitaxial wafer is 7.6-8.4Ω.cm, and the thickness is 14-15um. Since too high a resistivity will increase the saturation voltage drop of the product, too low a resistivity will affect the breakdown voltage of the product, the overall thickness of the chip = 465±20um, insert the silicon epitaxial wafer into a boat and push it into a heating furnace for heating so that an oxide layer is formed on the silicon epitaxial wafer, and obtain a first silicon epitaxial wafer;

[0145] The heating in step S1 is specifically as follows: oxygen is introduced and the temperature is raised to 1150°C, the heating time is 4 hours, the oxygen flow rate is controlled to 5L / min, when the temperature rises to 1150°C, then a mixture of oxygen and hydrogen is introduced and maintained for 80 minutes, and finally oxygen is introduced and maintained for 40 minutes, the thickness of the oxide layer is controlled to be 0.6μm, the flow rate of O2 is 4000ml / min, and the flow rate of H2 is 4700ml / min, which effectively ensures the breakdown voltage.

[0146] Step S2. Photolithography base area: the first silicon epitaxial wafer is coated by a coating machine, and then development, hardening, etching, and wet stripping are performed in sequence to obtain a second silicon epitaxial wafer;

[0147] Step S2. Photolithography of the base region specifically includes the following steps:

[0148] S21. Spreading glue: Select HFJ220 spread glue agent and add a spread glue machine, spread the first silicon epitaxial wafer through the spread glue machine, control the speed to 6500rpm, the spread glue time is 35s, the pre-baking temperature is 100°C, the time is 25min, the exposure is masked with the B area plate, ultraviolet exposure, and the exposure time is controlled to 7s;

[0149] S22 Development: The first silicon epitaxial wafer after the coating is immersed in the HFJ2200 developer liquid for 8 minutes to ensure high-quality development effect;

[0150] S23. Hardening: The first silicon epitaxial wafer after development is subjected to heat treatment, and the heat treatment temperature is controlled to be 130° C. for 35 minutes. In this process, the high temperature treatment can remove the remaining solvent in the photoresist, enhance the adhesion of the photoresist to the silicon wafer surface, and improve the corrosion resistance of the photoresist in the subsequent etching and ion implantation processes. At the same time, the photoresist will soften at high temperature to form a molten state similar to glass at high temperature, which will make the photoresist surface smooth under the action of surface tension and reduce defects (such as pinholes) in the photoresist layer;

[0151] S24. Etching: The first silicon epitaxial wafer after hardening was treated in an etching solution for 6 min, the temperature of the etching solution was controlled to be 38 ° C, the etching solution included a mixture of HF (concentration 42%), NH4F (concentration 96%) and deionized water, HF: NH4F: deionized water = 1mL: 2g: 3.3mL, controlled temperature: 38 ° C, time 8min, rinse 10 times;

[0152] S25. Wet degumming: the first silicon epitaxial wafer after etching is degummed in a degumming solution for 8 minutes, and then rinsed with water 10 times to obtain a second silicon epitaxial wafer, the degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4;

[0153] Step S3. Injection oxidation: insert the second silicon epitaxial wafer into the oxidation boat and send it into the diffusion furnace, and form the second silicon epitaxial wafer into a thickness of The oxidation layer was formed by controlling the oxygen flow rate at 4 L / min and the oxidation time at 10 min.

[0154] Step S4. Phosphorus implantation in the base region: Phosphorus ions are implanted into the second silicon epitaxial wafer after the oxidation in step S3 through an ion implanter. The ion implanter sets the energy and number of ions to be implanted, and the second silicon epitaxial wafer is implanted with accurately measured phosphorus ions. The implantation metering is 2.7E13. The advantages of ion implantation include less pollution and good uniformity of implantation within the wafer, between wafers, and between batches.

[0155] Step S5. Base region re-diffusion: inserting the second silicon epitaxial wafer into which phosphorus has been implanted in the base region in step S4 into a diffusion boat and sending it into a diffusion furnace, and heat treating it in a nitrogen atmosphere to obtain a third silicon epitaxial wafer;

[0156] The heat treatment in step S5 is specifically as follows: when the temperature of the diffusion furnace reaches 800°C, the second silicon epitaxial wafer is sent into the constant temperature zone of the diffusion furnace, the nitrogen flow rate is controlled at 4.5L / min, and then the temperature is raised to 1100°C for 35min, and then annealing is performed at a nitrogen flow rate of 6L / min for 35min, and finally the temperature is raised to 1170°C for 30min and diffusion is performed for 150min, while H2 and O2 are introduced for oxidation, and then the temperature is reduced to 800°C, the second silicon epitaxial wafer is taken out of the diffusion furnace, and naturally cooled to obtain a third silicon epitaxial wafer.

[0157] Step S6. Photolithography of the emission area: the third silicon epitaxial wafer is coated by a coating machine, followed by development, hardening, etching, and wet stripping in sequence;

[0158] Step S6: photolithography of the emission area specifically includes the following steps:

[0159] S21. Spreading glue: Spread the third silicon epitaxial wafer through the glue machine, control the speed to 6500rpm, the glue time is 30s, the pre-baking temperature is 100°C, the time is 25min, the exposure is masked with the B area version, ultraviolet exposure, and the exposure time is controlled to 6s;

[0160] S22. Development: Immerse the third silicon epitaxial wafer after the coating in the developing liquid for 8 minutes;

[0161] S23. Hard film: The developed third silicon epitaxial wafer is heat treated, and the heat treatment temperature is controlled to be 130±5°C and the time is 35min;

[0162] S24. Etching: The third silicon epitaxial wafer after hardening was treated in an etching solution for 6 min, and the temperature of the etching solution was controlled to be 38 ° C; the etching solution included HF (concentration 42%): NH4F (concentration 96%): deionized water = 1 mL: 2 g: 3.3 mL, the etching time was 7 min, and the solution was rinsed 10 times;

[0163] S25. Wet degumming: the third silicon epitaxial wafer after etching is degummed in a degumming solution for 6 minutes, and then rinsed with water 12 times to obtain a second silicon epitaxial wafer, the degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4;

[0164] Since the base current generates a voltage drop when passing through the base resistor, the bias voltages in different areas of the transistor emitter junction are not equal. There is an EXP relationship between the emitter current and the emitter junction bias voltage, so as long as the emitter bias voltage is slightly different, the emitter current will change greatly. When the operating current of the transistor is large, the voltage drop generated by the base current passing through the base resistor is also large, which makes the distribution of the emitter current on the emitter junction extremely uneven. In practice, the distribution of the emitter is that the closer to the base contact, the greater the current, and the current drops quickly to a very small value at a distance from the base. This emitter edge collection effect can also be considered as the base resistor self-bias effect. The current edge collection effect makes the entire emitter junction only effective near the edge close to the base contact. The emitter region doping adopts high-concentration CSD diffusion to improve the injection efficiency. During ion implantation, the emitter junction depth is controlled to 2um, the chip surface state is improved, and the injection efficiency is improved. From the process point of view, it is guaranteed that the product has a higher characteristic frequency, a faster switching speed, and a very high current gain as well as the uniformity of the diffusion parameter hFE.

[0165] Step S7. Coating photoresist: The third silicon epitaxial wafer after the photolithography emission area treatment in step S6 is coated by a coating machine, and then dried, oxidized, and rinsed in sequence to obtain a fourth silicon epitaxial wafer, and the resistance is controlled to be 4.5±1Ω, thereby forming a high resistance layer region 2 on the surface of the fourth silicon epitaxial wafer;

[0166] The photoresist coating process specifically comprises the following steps:

[0167] Step S71. Spreading glue: Select HFJ220 glue agent and add it to a glue machine, pass the fourth silicon epitaxial wafer through the glue machine, control the speed to 6000rpm, the glue time to 30s, and evenly coat the glue agent on the front of the fourth silicon epitaxial wafer;

[0168] Step S72. Pre-baking: placing the fourth silicon epitaxial wafer in a clean oven and drying it at 90° C. for 1 hour to ensure that the solvent of the latex source is fully volatilized;

[0169] Step S73. Oxidation: insert the fourth silicon epitaxial wafer into a boat and place it into a diffusion furnace, and oxidize it at 1050°C for 90 minutes, while introducing N2, H2 and O2; the flow rate of N2 is 4000ml / min, the flow rate of O2 is 4000ml / min, and the flow rate of H2 is 4700ml / min;

[0170] Step S74. Rinse: put the fourth silicon epitaxial wafer into a rinse solution of HF (concentration 42%): NH4F (concentration 96%): deionized water = 1 mL: 2 g: 3.3 mL for rinsing, control the temperature to 38°C, the time to 2 min, rinse 10 times, then spin dry, and inspect, and measure the resistance of the fourth silicon epitaxial wafer to be 4.5±1Ω;

[0171] Step S8. Boron expansion of the emitter region: The fourth silicon epitaxial wafer processed in step S7 is sent to a diffusion furnace for heat treatment in an oxygen and nitrogen atmosphere. The pipeline nitrogen flow rate is controlled to be 5L / min, the oxygen flow rate is 2L / min, and the heat temperature is controlled to be 1050°C. After heating for 4h to reach 1050°C, nitrogen is introduced for a time of t=1.5h, the nitrogen is turned off, the temperature is kept constant for 15 minutes, the temperature is lowered to 700°C, taken out, and sent to the inspection Xj=2.2um oxide layer thickness: An emitter region 4 is formed on the front of the base region 3 of the fourth silicon epitaxial wafer, and a resistance-increasing ring 5 is formed around the emitter region 4; the resistance-increasing ring 5 is independent of the emitter junction and the base region lead hole, does not participate in the conduction, and forms isolation, thereby blocking the lateral flow of the base region injection current. The base region current cannot flow directly to the emitter junction surface, but flows evenly under the emitter junction, thereby weakening the emitter current edge collection effect when the transistor is working at a large current, reducing the current concentration of the emitter junction, improving the product heating problem, and improving the controllability of the product;

[0172] Step S9. Phosphorus filling photolithography: the fourth silicon epitaxial wafer processed in step S8 is subjected to a coating machine, and then subjected to development, hardening, etching, and wet stripping treatments in sequence;

[0173] Step S9 phosphor-filling lithography specifically includes the following steps:

[0174] S21. Spreading glue: Spread the fourth silicon epitaxial wafer through the glue machine, control the speed to 6500rpm, the glue time is 35s, the pre-baking temperature is 100°C, the time is 25min, the exposure is masked with the B area version, ultraviolet exposure, and the exposure time is controlled to 8s;

[0175] S22. Development: The fourth silicon epitaxial wafer after the coating is immersed in the developing liquid for 8 minutes;

[0176] S23. Hardening: The fourth silicon epitaxial wafer after development is heat treated, and the temperature of the heat treatment is controlled to be 130°C and the time is 30 minutes. In this process, the high temperature treatment can remove the remaining solvent in the photoresist, enhance the adhesion of the photoresist to the silicon wafer surface, and improve the corrosion resistance of the photoresist in the subsequent etching and ion implantation process. At the same time, the photoresist will soften at high temperature to form a molten state similar to glass at high temperature, which will make the surface of the photoresist smooth under the action of surface tension and reduce defects in the photoresist layer (such as pinholes);

[0177] S24. Etching: The fourth silicon epitaxial wafer after hardening was treated in an etching solution for 6 min, and the temperature of the etching solution was controlled to be 38 ± 2 ° C; the etching solution included HF (concentration 42%): NH4F (concentration 96%): deionized water = 1 mL: 2 g: 3.3 mL, the etching time was 7 min, and the solution was rinsed 10 times;

[0178] S25. Wet degumming: Degumming the fourth silicon epitaxial wafer after etching in a degumming solution for 8 minutes, and then rinsing it with water for 10 times to obtain a second silicon epitaxial wafer. The degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:4.

[0179] Step S10. Phosphorus supplementation diffusion oxidation: The temperature of the constant temperature zone of the diffusion furnace is raised to 1050°C for about 30 minutes. After the constant temperature, nitrogen carrying a phosphorus source is introduced into the diffusion furnace for 1.5 hours, the nitrogen is turned off, and the temperature is kept constant for 15 minutes. Then, the fourth silicon epitaxial wafer that has undergone phosphorus supplementation lithography is inserted into an oxidation boat and sent into the diffusion furnace for oxidation under an oxygen atmosphere. The oxidation time is 12 minutes, the oxygen flow rate is controlled at 4L / min, the oxidation temperature is 1050°C, and the thickness of the oxide layer is controlled to be

[0180] Step S11. Photolithography of lead holes: The fourth silicon epitaxial wafer processed in step S10 is subjected to a coating machine, and then subjected to pre-baking, film hardening, and wet stripping in sequence to obtain a fifth silicon epitaxial wafer;

[0181] Step S11 of photolithography of lead holes specifically includes the following steps:

[0182] S110. Spreading glue: BN308 glue is selected as a spreader and added to a spreader, and the fourth silicon epitaxial wafer is spread by a spreader, and the speed is controlled to be 3000rpm and the spread time is 40s;

[0183] S111. Pre-baking: pre-baking the fourth silicon epitaxial wafer after the coating, controlling the temperature to 100°C, the time to 25min, masking the lead frame, and exposing to ultraviolet light for 8s;

[0184] S112. Hard film: The fourth silicon epitaxial wafer after pre-baking was heat treated, and the heat treatment temperature was controlled to be 140°C for 30 min; the window SiO2 was etched with HF (concentration 42%): NH4F (concentration 96%): deionized water = 1 mL: 2 g: 3.3 mL, the temperature was controlled to be 38°C, the time was 8 min, and rinsed 10 times;

[0185] S113. Wet degumming: degumming the etched fourth silicon epitaxial wafer in a degumming solution for 6 minutes, and then rinsing with water 10 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is 98% concentrated sulfuric acid and 35% hydrogen peroxide in a volume ratio of 1:4;

[0186] Step S12. Front aluminum evaporation: The fifth silicon epitaxial wafer is evaporated into an aluminum film with a thickness of 4.6um by a high vacuum electron beam evaporation table; pre-evacuation is performed according to the equipment operating procedures. When the pressure reaches below 2Mpa, the extraction valve is closed and the high valve is opened. The vacuum chamber is controlled to a pressure of 4*10 -3 Mpa, temperature control 180℃, time 30min, turn off the baking power; when the vacuum reaches 2*10 -3 Mpa, delay for 2 minutes, turn on the high-voltage current aluminum source for pre-melting: control 0.4A slow steaming for 4min, 0.6A, 30 minutes, the thickness of the aluminum layer is controlled moderately, which greatly reduces the damage to the product in the subsequent packaging bonding process, and even causes crater problems, reduces the contact resistance between the bonding wire and the aluminum layer on the chip surface, and improves the bonding strength between the aluminum wire and the chip aluminum layer.

[0187] Step S13. Photolithography of aluminum: The fifth silicon epitaxial wafer processed in step S12 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence;

[0188] Step S13 of photolithography of aluminum specifically includes the following steps:

[0189] S130. Spreading glue: BN308 glue is selected as a spreader and added to a spreader, and the fourth silicon epitaxial wafer is spread by a spreader, and the speed is controlled to be 3000rpm and the spread time is 40s;

[0190] S131 pre-baking: pre-baking the fifth silicon epitaxial wafer after the coating, controlling the temperature to 100°C, the time to 25min, the lead frame masking, ultraviolet exposure, the time to 8s;

[0191] S132. Hard film: The fifth silicon epitaxial wafer after pre-baking was heat treated, and the heat treatment temperature was controlled to be 140±3°C for 30 min; the window SiO2 was etched with HF (concentration 42%): NH4F (concentration 96%): deionized water = 1 mL: 2 g: 3.3 mL, the temperature was controlled to be 38°C, the time was 8 min, and rinsed 10 times;

[0192] S133. Wet degumming: degumming the fourth silicon epitaxial wafer after etching in a degumming solution for 6 minutes, and then rinsing with water 10 times to obtain a second silicon epitaxial wafer, the degumming solution is 98% concentrated sulfuric acid and 35% hydrogen peroxide in a volume ratio of 1:4;

[0193] Step S14. Surface aluminum evaporation: The fifth silicon epitaxial wafer processed in step S13 is subjected to surface aluminum evaporation in a nitrogen atmosphere to form a second metal layer 8 on the front side of the emitter region 4, and a first metal layer 7 is formed on the front side of the base region 3 except for the portion connected to the emitter region 4; the surface aluminum evaporation temperature in step S14 is 500°C, the time is 30 minutes, and the nitrogen flow rate is controlled to be 5L / min;

[0194] Step S15. Deposition of protective layer: Covering the outermost layer of the front side of the fifth silicon epitaxial wafer processed in step S14 with the insulating dielectric layer 6;

[0195] The insulating dielectric layer is SiO2+phosphosilicon glass PSG+Si3N 4, Thickness 2.5um; Although SiO2 is very stable in mechanical, chemical and electrical aspects and has a good passivation effect, SiO2 has poor masking ability for alkaline metal ions such as Na+ and K+. Phosphorus silicon glass PSG has the function of extracting, fixing and blocking sodium ions, which can significantly weaken the influence of mobile ions such as sodium on the surface properties of semiconductors and reduce leakage current. The outermost layer is the Si3N4 layer, which has a tight structure, low pinhole density, and is difficult for gas and water vapor to penetrate. It has a strong masking ability and can weaken the influence of impurities on the outer surface of the dielectric layer. It has good chemical stability and strong sodium resistance. It has high hardness and provides mechanical protection for metal interconnects and terminal metals.

[0196] Step S16. Bonding area photolithography: The fifth silicon epitaxial wafer processed in step S15 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence;

[0197] Step S16: the bonding area photolithography specifically includes the following steps:

[0198] S160. Spreading glue: BN308 glue is selected as a spreader and added to a spreader, and the fourth silicon epitaxial wafer is spread by a spreader, and the speed is controlled to be 3000rpm and the spread time is 40s;

[0199] S161 pre-baking: pre-baking the fifth silicon epitaxial wafer after the coating, controlling the temperature to 100°C, the time to 30min, the lead hole masking, ultraviolet exposure, the time to 8s;

[0200] S162. Hard film: The fifth silicon epitaxial wafer after pre-baking was heat treated, and the heat treatment temperature was controlled to be 140°C for 30 min; the window SiO2 was etched with HF (concentration 42%): NH4F (concentration 96%): deionized water = 1mL: 2g: 3.3mL, the temperature was controlled to be 75°C, the time was 8 min, and rinsed 10 times;

[0201] S163. Wet degumming: degumming the etched fourth silicon epitaxial wafer in a degumming solution for 6 minutes, and then rinsing with water 10 times to obtain a second silicon epitaxial wafer, wherein the degumming solution is 98% concentrated sulfuric acid and 35% hydrogen peroxide in a volume ratio of 1:4;

[0202] Step S17. Heat treatment: heat treat the fifth silicon epitaxial wafer treated in step S16 in a nitrogen atmosphere; then reduce the thickness of the ninth silicon epitaxial wafer to 265um to obtain the sixth silicon epitaxial wafer; the heat treatment temperature in step S17 is 400°C, the time is 25min, and the nitrogen flow rate is controlled to 5L / min;

[0203] Step S18. Back metallization: The sixth silicon epitaxial wafer is subjected to Ti-Ni-Ag evaporation through an electron beam evaporation station, thereby forming a metal layer 9 on the back of the sixth silicon epitaxial wafer to obtain a chip;

[0204] Ti-Ni-Ag was deposited on the electron beam evaporation table according to the equipment operation card. The thickness of Ti was The thickness of Ni is The thickness of Ag is 1.3um, and the total thickness is controlled at 2.0um to ensure good ohmic contact and thermal resistance, especially forming a very good alloy layer together with high-temperature soft solder, ensuring very low thermal resistance and high reliability of this device. Ink dot screening of defective chips, testing instrument JUNO automatic test bench, testing VEBO, VCEO, VCBO, IEBO, ICBO, hFE and other parameters.

[0205] Step S19. Saw blade: saw the chip into individual dies;

[0206] Step S20. Finished product: The tube core is sequentially mounted, bonded, and plastic-sealed to obtain a power transistor for an industrial printing control system.

[0207] Step S20: loading the film includes the following specific steps:

[0208] Step S201. Place the lead frame 10 into the loading mechanism of the high-speed automatic chip loader, and insert high-temperature soft solder 20 at the chip mounting position on the lead frame. The high-temperature soft solder 20 includes 92.5% lead, 5% tin and 2.5% silver. The compressed air pressure in the high-speed automatic chip loader is controlled to be 0.4MPa, and the vacuum degree is -80KPa. The high-speed automatic chip loader includes 8 temperature zones, and the controlled temperatures are: 300°C, 375°C, 385°C, 385°C, 385°C, 385°C, 380°C, and 320°C, and a hydrogen-nitrogen mixed gas is introduced to control the total flow rate of the mixed gas to be: 19L / min;

[0209] Step S202. Automatically pick up the chip 30 into the solder 20 on the lead frame 10 through a suction nozzle;

[0210] Step S203. The lead frame with the loaded chip is automatically put into the material box through the cooling zone of the chip loading machine track, tinning, film pressing, shaping, core loading, and cooling process. This process is fully matched to ensure that the overall chip void rate is less than 5% and the single chip void rate is less than 2%, ensuring good transient thermal resistance VBE and high reliability of the product.

[0211] Bonding involves the following steps:

[0212] S204. The lead frame 10 with the chip 30 is placed in the feeding mechanism of the automatic ultrasonic bonding machine for bonding. The lead wire 40 is 99.99% high-purity aluminum wire with a diameter of 300um, 1 E pole and 1 B pole;

[0213] (1) Wedge blade: YH-153-12mil, wire nozzle specification: YH-7200-W12; (2) Control the ultrasonic power, pressure, and time of the bonding machine. The parameter settings are shown in Table 3.

[0214] Table 3

[0215] Solder point location Power Pressure F Time T One solder joint (chip) 650 450 120 Two solder joints (lead frame) 800 500 120

[0216] (3) Control of solder joint length: 737um; width of solder joint: 365um; (4) Control of bonding wire tension F: 456N; thrust control of solder joint core: 1118N; the direction of bonding point and aluminum wire is greater than 90°, and the height of bonding arch wire is controlled at 2.78mm. The bonded product has no cold solder joints, no craters, and no twisting of aluminum wire, which fully guarantees the product's ability to pass large currents and can reduce the product's Vce (sat) saturation voltage drop parameters. At the same time, the solder joint and the chip are fully and effectively connected, ensuring that the solder joint is not broken or loose after the reliability test, further ensuring the high reliability of the product.

[0217] Plastic packaging includes the following specific steps:

[0218] Step S205: The bonded product is further encapsulated with epoxy resin 50. The epoxy resin is KHG400 produced by Soienohem, Φ48mm, 108g / piece, an environmentally friendly plastic encapsulation material specially used for encapsulating fully encapsulated high-power devices, with high thermal conductivity and high reliability. The main control parameters are shown in Table 4;

[0219] Table 4

[0220]

[0221]

[0222] (1) After the plastic encapsulation material is taken out of the cold storage, it is warmed up for 24 hours, the temperature is 23±2℃, and the relative humidity is 50±15%; (2) Injection molding press temperature control: upper mold setting temperature 185℃, lower mold setting temperature 185℃; high frequency preheating time: 27s, transfer time: 20s, injection time: 50s, injection pressure: 6MPa, mold curing time: 180s, oven post-curing temperature 175, post-curing time 6h; TO-3PML plastic encapsulation mold, 80 cavities; the appearance of the product after plastic encapsulation is complete, without voids, bubbles, corners, or pinholes. By using halogen-free environmentally friendly materials with high thermal conductivity and low water absorption, and adopting the preferred injection molding process, the product's appearance size and high thermal conductivity are ensured, laying a high reliability foundation for the application of device products in high temperature environments. The insulation voltage test is implemented and all are >2500V, ensuring the insulation application of the product.

[0223] The electroplating cutting process specifically includes the following steps:

[0224] Step S206: electroplating high-purity tin Sn, controlling the thickness of the tin layer to 12um, using high-speed line electroplating to ensure uniform thickness of the product tin layer, ensuring the product's 260°C, 10s wave soldering process, ensuring the product's high-reliability process adaptability, and controlling the cutting force to 6Mpa to prevent excessive force from causing stress that affects the reliability of the chip.

[0225] Step S21. Testing:

[0226] The chip is tested on the discrete device test system JUNO. The discrete device test system JUNO model is DTS-1000. The controlled environment temperature is 18-24℃ and the humidity is 40-70%.

[0227] Setting up test conditions

[0228] VEBO:>6V, V(BR)CEO:>50V IC=25mA, VCBO:>70V, ICBO:<10uA, VCB=70V, VEBO:<10uA, VEB=6V, hFE1:>150(Ic=1A, Vce=5V), hFE2:>50(Ic=5A, Vce=5V), Vce(sat):<0.5(Ic=5A, Ib=80mA), Vbe(sat):<1.2(Ic=5A, Ib=80mA), During the test, VEBO and VCBO were tested at 50uA, 100uA, 500uA, and 1mA respectively, and the ratio requirement of 95% was added to prevent pipeline breakdown and leakage products from affecting the reliability of the product. The test results are shown in Tables 5 and 6.

[0229] Table 5 PNP test data table

[0230]

[0231] Table 6 NPN test data table

[0232]

[0233]

[0234] It can be seen from Tables 5 and 6 above that in this method, the contradiction between the saturation voltage drop and the current capability is solved by using the epitaxial planar process, while ensuring that the breakdown voltage of the PNP type product, VCE: 76-80V, the VCESAT parameter is between 0.3-0.4V, and the breakdown voltage of the NPN type, VCE: 87-92.28, the VCESAT parameter is between 0.17-0.30V, which is far below the standard requirements of the product.

[0235] During ion implantation, the emitter junction depth is controlled at 2um, which improves the surface state of the chip and the implantation efficiency. By using the surface PSG+SI3N4 process, the IEBO and ICBO leakage currents of the product are very low, at the pA and nA levels, ensuring high product reliability.

[0236] By solving the control problem of the light boron base area, the product is guaranteed to have a higher characteristic frequency, faster switching speed, extremely high current gain and uniformity of diffusion parameter hFE. The product P-type HFE parameters are 220-243, and N-type HFE parameters are 261-267.

[0237] The back-side multi-layer metal process is used to ensure good ohmic contact and thermal resistance, especially to form a very good alloy layer together with high-temperature soft solder. The transient thermal resistance DVbe value is 60mV, ensuring very low thermal resistance and high reliability of this device.

[0238] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A power transistor for an industrial printing control system, characterized in that: The power transistor comprises a chip (30), wherein the chip (30) comprises a substrate (1), a metal layer (9) being arranged on the back side of the substrate (1), a high resistance layer region (2) being arranged on the front side of the substrate (1), a base region (3) being arranged on a front side of the high resistance layer region (2) away from the substrate (1), an emitter region (4) and a resistance increasing ring (5) arranged around the periphery of the emitter region (4) being arranged on the front side of the base region (3), a second metal layer (8) being arranged on the front side of the emitter region (4), a first metal layer (7) being arranged on the front side of the base region (3) except for a portion connected to the emitter region (4), the outermost layer on the front side of the substrate being covered with an insulating dielectric layer (6), and the first metal layer (7) and the second metal layer (8) except for a portion connected to the emitter region (4) being isolated from the substrate by the insulating dielectric layer (6).

2. The power transistor for industrial printing control system according to claim 1, characterized in that: The substrate (1) is a P+ type substrate, the high resistance layer region (2) is a P- type high resistance layer region, the base region (3) is an N- type base region, and the emitter region (4) is a P+ type emitter region; the thickness of the P+ type substrate (1) is 240um±20um, and the thickness of the metal layer (9) is 2.0-2.5um; the thickness of the P- type high resistance layer region (2) is 10um, the width of the N- type base region (3) is 4.5-5.0um, the thickness of the first metal layer (7) and the second metal layer (8) is 4.5-5.2um, the depth of the P+ type emitter region (4) is 2-3um, and the thickness of the insulating dielectric layer (6) is 2-2.5um.

3. The power transistor for industrial printing control system according to claim 1, characterized in that: The substrate (1) is an N+ type substrate, the high resistance layer region (2) is an N- high resistance layer region, the base region (3) is a P-type base region, and the emitter region (4) is an N+ type emitter region; the thickness of the N+ type substrate (1) is 231-240 um, the thickness of the N- high resistance layer region is 14-18 um, the depth of the P-type base region is 10-15 um, the depth of the N+ emitter region is 5-7 um, the thickness of the insulating dielectric layer (6) is 2-4 um, and the thickness of the first metal layer (7) and the second metal layer (8) are 4.5-5.2 um.

4. The power transistor for industrial printing control system according to claim 1, characterized in that: The insulating dielectric layer (6) is a three-layer structure, wherein the silicon dioxide layer is in contact with the substrate (1), the middle layer is a PSG layer, and the surface layer is a Si3N4 layer; the back metal layer (9) is a three-layer structure, wherein the titanium layer is in contact with the substrate, the middle layer is a nickel layer, and the bottom layer is a silver layer; the power transistor further comprises a lead frame (10), solder (20), bonding wires (40), and an epoxy resin layer (50); the chip (30) is arranged on the lead frame (10), solder (20) and bonding wires (40) are arranged between the chip (30) and the lead frame (10), and the lead frame (10) is sealed by the epoxy resin layer (50).

5. The method for manufacturing a power transistor for an industrial printing control system according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1. Field oxidation: providing a silicon epitaxial wafer, inserting the silicon epitaxial wafer into a boat and pushing the silicon epitaxial wafer into a heating furnace for heating so that an oxide layer is formed on the silicon epitaxial wafer, thereby obtaining a first silicon epitaxial wafer; Step S2. Photolithography base area: the first silicon epitaxial wafer is coated by a coating machine, and then development, hardening, etching, and wet stripping are performed in sequence to obtain a second silicon epitaxial wafer; Step S3. Injection oxidation: insert the second silicon epitaxial wafer into the oxidation boat and send it into the diffusion furnace, so that the second silicon epitaxial wafer forms an oxide layer with a thickness of 400±50Å under an oxygen atmosphere; Step S4. Phosphorus implantation in the base region: Phosphorus ions are implanted into the second silicon epitaxial wafer after the oxidation in step S3 by an ion implanter; Step S5. Base region re-diffusion: inserting the second silicon epitaxial wafer into which phosphorus has been implanted in the base region in step S4 into a diffusion boat and sending it into a diffusion furnace, and heat treating it in a nitrogen atmosphere to obtain a third silicon epitaxial wafer; Step S6. Photolithography of the emission area: the third silicon epitaxial wafer is coated by a coating machine, followed by development, hardening, etching, and wet stripping in sequence; Step S7. Coating photoresist: Spread the third silicon epitaxial wafer after the photolithography emission area treatment in step S6 through a photoresist machine, and then sequentially dry, oxidize, and rinse to obtain a fourth silicon epitaxial wafer, and control the resistance to be 4.5±1Ω, thereby forming a high resistance layer region (2) on the surface of the fourth silicon epitaxial wafer; Step S8. Boron re-expansion of the emitter region: the fourth silicon epitaxial wafer processed in step S7 is sent into a diffusion furnace for heat treatment in an oxygen and nitrogen atmosphere, and the heat temperature is controlled to be 1050±10° C., so that an emitter region (4) is formed on the front side of the base region (3) of the fourth silicon epitaxial wafer, and a resistance-increasing ring (5) is formed around the emitter region (4); Step S9. Phosphorus filling photolithography: the fourth silicon epitaxial wafer processed in step S8 is subjected to a coating machine, and then subjected to development, hardening, etching, and wet stripping treatments in sequence; Step S10. Phosphorus supplementation diffusion oxidation: the diffusion furnace is heated to 1050±10°C, and after constant temperature, nitrogen gas carrying a phosphorus source is introduced into the diffusion furnace for t1 time, and then the fourth silicon epitaxial wafer after phosphorus supplementation lithography is inserted into an oxidation boat and sent into the diffusion furnace for oxidation under an oxygen atmosphere, and the thickness of the oxide layer is controlled to be 2500±50Å; Step S11. Photolithography of lead holes: The fourth silicon epitaxial wafer processed in step S10 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal in sequence to obtain a fifth silicon epitaxial wafer; Step S12. Vaporizing aluminum on the front side: Vapor-depositing an aluminum film with a thickness of 4.5-5.2 um on the fifth silicon epitaxial wafer through a high vacuum electron beam evaporation station; Step S13. Photolithography of aluminum: The fifth silicon epitaxial wafer processed in step S12 is subjected to a coating machine for coating, and then subjected to pre-baking, film hardening, and wet coating removal treatments in sequence; Step S14. Surface aluminum vaporization: The fifth silicon epitaxial wafer processed in step S13 is subjected to surface aluminum vaporization in a nitrogen atmosphere to form a second metal layer (8) on the front surface of the emitter region (4), and a first metal layer (7) is formed on the front surface of the base region (3) except for the portion connected to the emitter region (4); Step S15. Deposition of protective layer: Covering the outermost layer of the front side of the fifth silicon epitaxial wafer processed in step S14 with an insulating dielectric layer (6); Step S16. Photolithography of the bonding area: the fifth silicon epitaxial wafer processed in step S15 is subjected to a coating machine, and then pre-baking, film hardening, and wet stripping are sequentially performed; Step S17. Heat treatment: heat treating the fifth silicon epitaxial wafer processed in step S16 in a nitrogen atmosphere; Then, the thickness of the ninth silicon epitaxial wafer is controlled to be 260±10 um to obtain the sixth silicon epitaxial wafer; Step S18. Back metallization: The sixth silicon epitaxial wafer is subjected to Ti-Ni-Ag evaporation through an electron beam evaporation station, thereby forming a metal layer (9) on the back of the sixth silicon epitaxial wafer to obtain a chip; Step S19. Saw blade: saw the chip into individual dies; Step S20. Finished product: The tube core is sequentially mounted, bonded, plastic-sealed, electroplated and cut to obtain a power transistor for an industrial printing control system.

6. The method for manufacturing a power transistor for an industrial printing control system according to claim 5, characterized in that: The heating in step S1 is specifically as follows: introducing oxygen and raising the temperature to 1150±15°C, controlling the oxygen flow rate to 5-6L / min, then introducing a mixture of oxygen and hydrogen and maintaining it for 80 minutes, and finally introducing oxygen and maintaining it for 40 minutes, controlling the oxide layer thickness to 0.6-0.7μm.

7. The method for manufacturing a power transistor for an industrial printing control system according to claim 5, characterized in that: The base region photolithography in step S2, the emitter region photolithography in step S6, and phosphorus filling photolithography in step S9 all specifically include the following steps: S21. Spreading glue: Spreading glue on the first silicon epitaxial wafer or the third silicon epitaxial wafer or the fourth silicon epitaxial wafer by a glue machine, controlling the speed to 6000-7000rpm, the glue spreading time to 30-40 s, the pre-baking temperature to 100±5℃, the time to 25-30min, the exposure to mask the B area plate, ultraviolet exposure, and controlling the exposure time to 6-8s; S22. Development: Immerse the first silicon epitaxial wafer, the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after the coating in a developing liquid for 6-8 minutes; S23. Hard film: heat treating the first silicon epitaxial wafer or the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after development, controlling the heat treatment temperature to 130±8°C for 30-40min; S24. Etching: treating the first silicon epitaxial wafer, the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after hardening in an etching solution for 6-8 minutes, and controlling the temperature of the etching solution to be 38±2°C; S25. Wet degumming: Degumming the first silicon epitaxial wafer, the third silicon epitaxial wafer or the fourth silicon epitaxial wafer after corrosion in a degumming solution for 6-8 minutes, and then rinsing with water for 10-12 times to obtain a second silicon epitaxial wafer. The degumming solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:

4.

8. The method for manufacturing a power transistor for an industrial printing control system according to claim 5, characterized in that: The heat treatment in step S5 is specifically as follows: when the temperature of the diffusion furnace reaches 800±5°C, the second silicon epitaxial wafer is sent into the constant temperature zone of the diffusion furnace, the nitrogen flow rate is controlled at 4-6L / min, and then the temperature is increased for 35min-40min to the temperature of 1100±5°C, and then annealing is performed for 30-50min at a nitrogen flow rate of 4-6L / min, and finally the temperature is increased for 30-40min to the temperature of 1170°C±5°C for diffusion for 140-160min, and H2 and O2 are introduced for oxidation at the same time, and then the temperature is reduced to 800°C to take the second silicon epitaxial wafer out of the diffusion furnace, and it is naturally cooled to obtain a third silicon epitaxial wafer.

9. The method for manufacturing a power transistor for an industrial printing control system according to claim 5, characterized in that: The step S7 of applying the photoresist specifically includes the following steps: Step S71: Spreading the third silicon epitaxial wafer through a spreader, controlling the speed of the spreader to be 6000-7000 rpm, and the spread time to be 32-40 s; Step S72: pre-baking: pre-baking the third silicon epitaxial wafer after the coating at 90-100°C for 1 hour; Step S73. Oxidation: insert the third silicon epitaxial wafer after pre-baking into a boat, put it into a diffusion furnace, and oxidize it at 1050°C-1100°C for 90-120min while introducing N2, H2 and O2; Step S74. Rinse: Treat the oxidized third silicon epitaxial wafer in the etching solution for 1.5-2 minutes, rinse 10-12 times, and then spin dry.

10. The method for manufacturing a power transistor for an industrial printing control system according to claim 5, characterized in that: In step S10, t1 is 1.35-1.75h, the oxidation time is 10-15min, and the oxidation temperature is 1050±10°C; in step S14, the surface aluminum vaporization temperature is 480-515°C, and the time is 20-30min; in step S17, the heat treatment temperature is 395-405°C, and the time is 20-30min; Step S20: loading the film includes the following specific steps: Step S201. Place the lead frame (10) into the loading mechanism of the high-speed automatic chip loader, and insert high-temperature soft solder (20) at the chip mounting position on the lead frame. Control the compressed air pressure in the high-speed automatic chip loader to be 0.35-0.6 MPa, and the vacuum degree to be -80~-100 KPa. The high-speed automatic chip loader includes 8 temperature zones, and the controlled temperatures are: 300℃±5℃, 375℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 385℃±5℃, 380℃±5℃, 320℃±5℃, and introduce hydrogen and nitrogen mixed gas, and control the total flow rate of the mixed gas to be: 15-25 L / min; Step S202. Automatically pick up the chip (30) into the solder (20) on the lead frame (10) through a suction nozzle; Step S203. The lead frame with the chip mounted on it passes through the track of the chip mounter, undergoes tinning, lamination, shaping, core loading, and cooling process, and then automatically enters the material box.

Citation Information

Cited By

  • Preparation method for improving saturation voltage drop of semiconductor device

    CN120417408A