Negative electrode material and preparation method and application thereof
By blending hard carbon with graphite and building a MoOx-MoyN modification layer, the problems of fast charging and long cycle stability of traditional graphite anode materials are solved, and the high energy density and long life of lithium-ion batteries are achieved.
Patent Information
- Application Number
- CN202411219683.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional graphite anode materials exhibit poor fast charging capabilities and poor electrochemical stability of long cycle interfaces under fast charging conditions, resulting in challenges in lithium-ion batteries in terms of high power density and long cycle life.
A matrix blended with hard carbon and graphite was used, and a MoOx-MoyN modified material layer was constructed on its surface. Randomly embedded MoO2 and Mo2N nanocrystals were formed by simple crystallization and partial topological nitriding methods, thereby improving Li+ diffusion rate and electron conduction ability. , alleviate the problems of solvent coembedding and lithium extraction.
It significantly improves the rate performance and cycle stability of the material, achieves the stability of the Li+ fast conduction and electrolyte interface, and extends the fast charging capability and cycle life of lithium-ion batteries.
Smart Images

Figure BDA0005022645010000171 
Figure BDA0005022645010000181
Abstract
Description
Technical Field
[0001] The present invention relates to the field of batteries, and in particular to a negative electrode material and a preparation method and application thereof. Background Art
[0002] Since Sony first launched lithium-ion batteries in the 1990s, graphite carbon (Gr) and its derived composites have been used as the mainstream negative electrode materials for lithium-ion batteries (LIBs), and it is generally believed that the negative electrode material determines the fast charging performance and power density of LIBs.
[0003] Theoretically, graphite (Gr) has a high enough Li + Diffusion coefficient (D Li+ >2×10 -10 cm 2 s -1 ), supporting full lithiation within 10 min (equivalent to charging at a 6C rate). During the charge / discharge process, graphite shows a well-defined voltage plateau at low potentials (<0.2 V relative to Li / Li+), as well as relatively high initial and subsequent cycle Coulombic efficiencies. These properties make graphite an attractive material for achieving high energy density lithium-ion batteries. While the low redox potential of graphite promotes higher battery energy density, it also raises concerns when graphite anodes are subjected to fast charging conditions. During fast charging, high current densities can lead to large anode polarization due to transport and kinetic limitations. These limitations can vary spatially throughout the thickness / volume of the anode, resulting in spatially inhomogeneous charging currents. From a more microscopic perspective, in fact, at high charging rates, the presence of edge structural imperfections on the Gr surface, such as atomic-scale defects, lattice distortion, dangling bonds, and unexpected chemical functionalization, may block reversible Li + Diffusion into the bulk, thus affecting the electrochemical performance. At the same time, in conventional vinyl carbonate electrolytes, Li + Strong interactions with the solvent at the anode / electrolyte interface lead to slow desolvation and may even induce solvent co-intercalation into the Gr interlayer at high charge rates. As a result, exfoliation along the (002) plane and parasitic solvent reduction reactions may occur on the Gr surface, which will lead to Li + The loss of transport pathways and the formation of a thick, organic-rich solid electrolyte interphase SEI, which in turn leads to the obstruction of charge transfer at the Gr / electrolyte interface, significantly increases the interfacial resistance and large voltage hysteresis. In addition, due to the large negative electrode polarization during the fast charging process of lithium-ion batteries, lithium dendrites may form at the Gr negative electrode, causing battery short circuit and thermal runaway, and reducing the cycle life. Therefore, Gr remains challenging in achieving high power density and long cycle life.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] In order to solve the problem that traditional graphite negative electrode materials have poor fast charging capability and poor long-cycle interface electrochemical stability, the present invention provides a negative electrode material and a preparation method and application thereof. The negative electrode material is improved on the basis of traditional graphite negative electrode materials, and the obtained negative electrode material has good fast charging capability and long-cycle interface electrochemical stability.
[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0007] One aspect of the present invention relates to a negative electrode material, comprising: a substrate and a modification material layer disposed on the surface of the substrate;
[0008] Wherein, the matrix comprises: hard carbon and graphite covering the hard carbon;
[0009] The chemical formula of the modifying material in the modifying material layer is MoO x -Mo y N, x is between 2 and 3, and y is between 1 and 2.
[0010] Compared with traditional graphite negative electrode materials, the negative electrode material has good fast charging performance and long-cycle interface electrochemical stability.
[0011] Another aspect of the present invention also relates to a method for preparing the negative electrode material, comprising the following steps:
[0012] (a) subjecting a mixed solution containing aqueous ammonia, hard carbon and formaldehyde to a first reaction and collecting a precipitate;
[0013] (b) subjecting the dispersion containing the precipitate and graphite to a first drying treatment and calcining to obtain the matrix;
[0014] (c) subjecting the mixed solution containing ammonium heptamolybdate and the substrate to a second drying treatment and a first annealing treatment; subjecting the product obtained by the first annealing treatment to a second annealing treatment under an atmosphere of ammonia and hydrogen;
[0015] (d) Cooling and passivating the product obtained by the second annealing treatment under a nitrogen and oxygen atmosphere to obtain the negative electrode material.
[0016] The method for preparing the negative electrode material has relatively simple production steps, low raw material prices, and can achieve large-scale production. The method can be used to obtain negative electrode materials with excellent electrochemical properties.
[0017] Another aspect of the present invention also relates to a negative electrode plate, comprising the negative electrode material or the negative electrode material prepared by the negative electrode material preparation method.
[0018] Another aspect of the present invention also relates to a secondary battery, comprising the negative electrode plate.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The negative electrode material provided by the present invention comprises a modified material layer which modifies a matrix of a graphite and hard carbon mixture. The graphite and hard carbon materials are mixed to significantly improve the rate performance of the material, achieving a compromise and balance between energy density and power performance. The modified material layer has high ionic conductivity and low Li + Diffusion energy barrier, which helps to form Li between graphite / electrolyte + It conducts quickly and has a low desolvation energy barrier, which can prevent the co-embedding of solvent molecules, effectively alleviating failure problems such as electrolyte reduction side reactions, structural exfoliation, and lithium precipitation on the graphite surface during fast charging and long cycles. The modified layer has a high Young's modulus and can withstand the accumulated internal stress and volume expansion caused by the violent movement of lithium ions, significantly improving the transmission dynamics, and achieving fast charging performance and long cycle life for the graphite negative electrode. The modified material layer can reduce parasitic solvent reduction reactions, effectively solving the problems of interface side reactions and lithium precipitation of the Gr negative electrode under fast charging conditions, significantly improving the fast charging capability of the Gr negative electrode while taking into account the long cycle life. The modified material layer has a high electron work function, which proves that it can alleviate the decomposition and fracture of the electrolyte interface and has excellent electron blocking ability in fast charging mode.
[0021] (2) The method for preparing the negative electrode material provided by the present invention has relatively simple production steps, low raw material prices, and can achieve large-scale production. The method can be used to obtain negative electrode materials with excellent electrochemical properties. The method is relatively simple and can be produced continuously, laying a foundation for the preparation of fast-charging graphite negative electrodes. DETAILED DESCRIPTION
[0022] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0023] One aspect of the present invention relates to a negative electrode material, comprising: a substrate and a modification material layer disposed on the surface of the substrate;
[0024] Wherein, the matrix comprises: hard carbon and graphite covering the hard carbon;
[0025] The chemical formula of the modifying material in the modifying material layer is MoO x -Mo y N, x is between 2 and 3, and y is between 1 and 2.
[0026] The negative electrode material is improved based on the traditional negative electrode material, and a composite material in which graphite is coated on the outside of hard carbon is used as a matrix, and a modified material layer is formed on the surface of the matrix. Compared with the traditional graphite negative electrode material, the negative electrode material has good fast charging performance and long cycle interface electrochemical stability.
[0027] The present invention mixes hard carbon with graphite to achieve a compromise between long cycle and fast charging performance. The hard carbon material has a large interlayer spacing and a randomly arranged crystal structure. + The diffusion coefficient in hard carbon is significantly higher than that in graphite, making it suitable as anode material for fast-charging and power-type batteries. At the same time, hard carbon materials have micropores and good compatibility with electrolytes, so the reaction kinetics are good. As a fast-charging material, the voltage platform of hard carbon is conducive to Li + Rapid embedding, not easy to precipitate lithium, good safety performance. Therefore, mixing hard carbon with graphite is beneficial to improve the overall kinetic performance of the negative electrode.
[0028] The present invention constructs MoO x -Mo y N modified nanomaterial layer fundamentally solves the structural stability problem of graphite materials. The solvent adsorption energy (Ea) of the modified material is low, which can promote Li + The desolvation process improves the solvent repellency and effectively alleviates the Li + The continuous exfoliation of the Gr structure caused by solvent co-intercalation, the high Young's modulus of the modified material layer, and the strong modified material layer can withstand the accumulated internal stress and volume expansion caused by the violent movement of lithium ions, ensuring long-term cycle durability. In addition, the modified material has a high electronic work function, which can alleviate the decomposition and fracture of the electrolyte interface under fast charging conditions and block the leakage of electrons from the negative electrode to the electrolyte layer. + channels, reducing internal stress, and blocking solvent molecule co-intercalation as well as valence electron leakage, which are very important for establishing a stable electrode / electrolyte interface for long-life and fast-charging LIBs.
[0029] Furthermore, the mass ratio of the hard carbon to the graphite is 10-50:50-90, including but not limited to 10:90, 20:80, 30:70, 40:60 or 50:50. The matrix composed of hard carbon and graphite in a certain ratio is conducive to improving the cycle stability and fast charging ability of the negative electrode material.
[0030] Furthermore, the thickness of the modified material layer is 500nm to 1μm, including but not limited to any point value of 500μm, 550μm, 600μm, 650μm, 700μm, 750μm, 800μm, 850μm, 900μm, 950μm or 1μm, or a range value between any two of them.
[0031] The present invention does not specifically limit the specific type of hard carbon, and conventional hard carbon in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the hard carbon includes but is not limited to: resin carbon, and the resin carbon includes but is not limited to: at least one of phenolic resin, epoxy resin or o-aminophenol.
[0032] This negative electrode material can be used not only in lithium-ion batteries, but also in sodium-ion batteries, potassium-ion batteries and all-solid-state batteries, with a wide range of applications. At the same time, the production steps are relatively simple, the raw material price is low, and it is expected to achieve large-scale production.
[0033] Another aspect of the present invention also relates to a method for preparing the negative electrode material, comprising the following steps:
[0034] (a) subjecting a mixed solution containing aqueous ammonia, hard carbon and formaldehyde to a first reaction and collecting a precipitate;
[0035] (b) subjecting the dispersion containing the precipitate and graphite to a first drying treatment and calcining to obtain the matrix;
[0036] (c) subjecting the mixed solution containing ammonium heptamolybdate and the substrate to a second drying treatment and a first annealing treatment; subjecting the product obtained by the first annealing treatment to a second annealing treatment under an atmosphere of ammonia and hydrogen;
[0037] (d) Cooling and passivating the product obtained by the second annealing treatment under a nitrogen and oxygen atmosphere to obtain the negative electrode material.
[0038] The preparation method of the negative electrode material uses a simple crystallization and partial topological nitridation method to form MoO on the surface of the graphite and hard carbon mixed material. x -Mo y The N-modified layer has randomly embedded MoO2 and Mo2N nanocrystals in the layer, which can achieve fast charging and long cycle performance of the graphite negative electrode.
[0039] The preparation method of the negative electrode material provides a structural domain of hard carbon and graphite mixed, which is a region with a cross-linked structure formed during the calcination of graphite and hard carbon, increasing the graphite interlayer spacing, reducing the edge effect of graphite, and improving the long cycle performance of graphite. The hard carbon material has a large interlayer spacing and a randomly arranged crystal structure. + The diffusion coefficient in hard carbon is significantly higher than that in graphite, making it suitable as anode material for fast-charge and power-type batteries. Mixing the two in a certain ratio can, to a certain extent, balance long cycle and fast-charge performance. Furthermore, the new dual-phase MoOx-Mo is coated on the surface of the mixed material by simple crystallization and topological nitridation. y N modified layer, which fundamentally solves the structural stability problem of graphite materials, not only promotes Li + The desolvation process improves the solvent repellency and effectively alleviates the Li + The continuous exfoliation of the Gr structure caused by solvent co-intercalation can also withstand the accumulated internal stress and volume expansion caused by the violent movement of lithium ions, ensuring long-term cycle durability.
[0040] The preparation method of the negative electrode material is to heat and mix a certain volume of NH3·H2O in water and ethanol. Then, add the hard carbon and formaldehyde solution to the mixed solvent and stir under heating conditions. The precipitate is separated by centrifugation, washed and dried to obtain a brown-yellow polymer powder. Then, the polymer powder and graphite are dispersed in water, mixed with ethanol, and stirred under heating conditions until the solvent is completely evaporated. Then, the dried sample is transferred to a high-temperature tube furnace for calcination to obtain a mixed material Gr@HC of graphite and hard carbon. Subsequently, a certain proportion of (NH4)6Mo7O 24 4H2O powder was dissolved in deionized water, and Gr@HC powder was added to the solution under continuous stirring. The obtained mixed solution was dried to form AMT@Gr@HC powder. MoO x @Gr@HC powder. Subsequently, NH3 / H2 mixed gas was introduced into a tube furnace for secondary annealing. After the powder obtained by the secondary annealing was cooled to room temperature, it was passivated in N2 / O2 mixed gas to obtain MoO x -Mo y The three-dimensional structure of N-modified graphite and hard carbon mixed negative electrode can form Li between mixed carbon material / electrolyte. + It quickly conducts and blocks the co-embedding of solvent molecules, improves the material / charge transfer kinetics, and cleverly enables the graphite negative electrode to have both fast charging performance and long cycle life.
[0041] The first annealing treatment forms MoO2 on the substrate surface, the second annealing treatment forms MoO2 and Mo2N on the substrate surface, and MoO x -Mo y N.
[0042] Furthermore, the temperature of the first reaction is 75-85°C, including but not limited to any one of 75°C, 77°C, 79°C, 81°C, 83°C or 85°C or a range between any two of them.
[0043] Furthermore, the time of the first reaction is 4 to 6 hours, including but not limited to any one of 4 hours, 5 hours or 6 hours or a range between any two of them.
[0044] Furthermore, the temperature of the first drying treatment is 70-80°C, including but not limited to any point value of 70°C, 72°C, 74°C, 76°C, 78°C or 80°C or a range value between any two of them.
[0045] Further, the calcination temperature is 800-1300° C., including but not limited to any point value of 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1150° C., 1200° C., 1250° C. or 1300° C. or any range value between two of them. After calcination at a certain temperature, the formed matrix material has good stability.
[0046] Furthermore, the heating rate of the calcination is 1-3°C / min, including but not limited to any one of 1°C / min, 2°C / min or 3°C / min or a range between any two of them.
[0047] Furthermore, the calcination time is 2 to 5 hours, including but not limited to any one of 2 hours, 3 hours, 4 hours or 5 hours or a range between any two of them.
[0048] Furthermore, the calcination is carried out under the protection of an inert atmosphere, which includes but is not limited to argon.
[0049] Furthermore, the molar ratio of the aqueous ammonia to the formaldehyde is 1:1 to 3, including but not limited to 1:1, 1:2 or 1:3.
[0050] Furthermore, the molar ratio of the ammonium heptamolybdate to the matrix is 1:(1-5), including but not limited to 1:1, 1:2, 1:3, 1:4 or 1:5.
[0051] Furthermore, the temperature of the second drying treatment is 75-85°C, including but not limited to any point value of 75°C, 77°C, 79°C, 81°C, 83°C or 85°C, or a range value between any two of them.
[0052] Furthermore, the time of the second drying treatment is 10 to 14 hours, including but not limited to any one of 10 hours, 11 hours, 12 hours, 13 hours or 14 hours or a range between any two of them.
[0053] Further, the temperature of the first annealing treatment is 250-400°C, including but not limited to any point value of 250°C, 280°C, 300°C, 330°C, 350°C, 380°C or 400°C or a range value between any two of them.
[0054] Furthermore, the time of the first annealing treatment is 1 to 3 hours, including but not limited to any one of 1 hour, 2 hours or 3 hours or a range between any two of them.
[0055] Furthermore, the heating rate of the first annealing treatment is 4-6°C / min, including but not limited to any point value of 4°C / min, 5°C / min or 6°C / min or a range value between any two of them.
[0056] Furthermore, the first annealing treatment is performed under an inert atmosphere.
[0057] Further, the temperature of the second annealing treatment is 480-800°C, including but not limited to any point value of 480°C, 490°C, 500°C, 510°C, 520°C, 550°C, 580°C, 600°C, 630°C, 650°C, 680°C, 700°C, 730°C, 750°C, 780°C or 800°C, or the range value between any two of them.
[0058] Furthermore, the time of the second annealing treatment is 1 to 3 hours, including but not limited to any one of 1 hour, 2 hours or 3 hours or a range between any two of them.
[0059] Furthermore, the heating rate of the second annealing treatment is 1-3°C / min, including but not limited to any one of 1°C / min, 2°C / min or 3°C / min or a range between any two of them.
[0060] Furthermore, when the second annealing treatment is performed, the volume ratio of ammonia to hydrogen is 90-99:1-10, including but not limited to 90:10, 93:7, 95:5, 97:3 or 99:1.
[0061] Furthermore, the passivation time is 1 to 3 hours, including but not limited to any one of 1 hour, 2 hours or 3 hours or a range between any two of them.
[0062] Furthermore, during the passivation, the volume ratio of nitrogen to oxygen is 90-99:1-10, including but not limited to 90:10, 93:7, 95:5, 97:3 or 99:1.
[0063] Another aspect of the present invention also relates to a negative electrode plate, comprising the negative electrode material or the negative electrode material prepared by the negative electrode material preparation method.
[0064] Another aspect of the present invention also relates to a secondary battery, comprising the negative electrode plate.
[0065] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0066] Example 1
[0067] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0068] (1) Dissolve 0.6 mL of NH3·H2O in water and mix with ethanol in a volume ratio of 1:1, and stir at 40°C for 30 min;
[0069] (2) adding phenolic resin and 37 wt % formaldehyde solution into a mixed solvent and stirring at 80° C. for 5 hours; the molar ratio of ammonia water to formaldehyde is 1:1;
[0070] (3) separating the precipitate by centrifugation, washing it three times with water and ethanol, and then drying it at 80° C. for 12 hours to obtain a brown-yellow polymer powder;
[0071] (4) dispersing phenolic resin powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of phenolic resin to graphite of 10:90, and stirring at 75° C. until the solvent is completely evaporated;
[0072] (5) The dried sample was transferred to a high temperature tube furnace and heated to 800 °C at a heating rate of 1 °C min -1 , and maintained for 2 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0073] (6) (NH4)6Mo7O 24·4H2O powder was dissolved in deionized water, and Gr@HC was added to the solution under continuous stirring. (NH4)6Mo7O 24 The molar ratio of 4H2O to Gr@HC was 1:3, and the resulting mixed solution was dried at 80 °C for 12 h to form AMT@Gr@HC powder;
[0074] (7) The prepared powder was heated at 5 °C min under argon flow. -1 The MoO was annealed in a tube furnace at a heating rate of 1 h and an annealing temperature of 370 °C to form x @Gr@HC powder;
[0075] (8) A mixed gas of NH3 and H2 with a volume ratio of 95:5 was introduced into a tube furnace and annealed at 500°C for 1.5 h with a heating rate of 2°C min -1 , at this time MoO is formed x -Mo y N@Gr@HC powder;
[0076] (9) After the obtained powder was cooled to room temperature, it was passivated in a mixed gas of N2 and O2 with a volume ratio of 95:5 for 2 hours.
[0077] Example 2
[0078] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0079] (1) to (4) are the same as in Example 1;
[0080] (5) The dried sample was transferred to a high temperature tube furnace and heated to 900 °C at a heating rate of 1 °C min -1 , and maintained for 3 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0081] (6)~(9) are the same as in Example 1.
[0082] Example 3
[0083] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0084] (1) Same as Example 1;
[0085] (2) adding o-aminophenol and 37% formaldehyde solution into a mixed solvent and stirring at 80° C. for 5 hours; the molar ratio of ammonia water to formaldehyde is 1:2;
[0086] (3) Same as Example 1;
[0087] (4) dispersing o-aminophenol powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of o-aminophenol to graphite of 20:80, and stirring at 75° C. until the solvent is completely evaporated;
[0088] (5) The dried sample was transferred to a high temperature tube furnace and heated to 1000 °C at a heating rate of 1 °C min -1 , kept for 4 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0089] (6)~(9) are the same as in Example 1.
[0090] Example 4
[0091] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0092] (1) Same as Example 1;
[0093] (2) adding o-aminophenol and 37 wt % formaldehyde solution into a mixed solvent and stirring at 80° C. for 5 hours; the molar ratio of ammonia water to formaldehyde is 1:3;
[0094] (3) Same as Example 1;
[0095] (4) dispersing o-aminophenol powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of o-aminophenol to graphite of 30:70, and stirring at 75° C. until the solvent is completely evaporated;
[0096] (5) The dried sample was transferred to a high temperature tube furnace and heated to 1100 °C at a heating rate of 1 °C min -1 , kept for 4 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0097] (6)~(9) are the same as in Example 1.
[0098] Example 5
[0099] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0100] (1) Same as Example 1;
[0101] (2) adding epoxy resin and 37 wt % formaldehyde solution into a mixed solvent and stirring at 80° C. for 5 hours; the molar ratio of ammonia water to formaldehyde is 1:1.5;
[0102] (3) Same as Example 1;
[0103] (4) dispersing epoxy resin powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of epoxy resin to graphite of 40:60, and stirring at 75°C until the solvent is completely evaporated;
[0104] (5) The dried sample was transferred to a high temperature tube furnace and heated to 1200 °C at a heating rate of 1 °C min -1 , kept for 4 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0105] (6)~(9) are the same as in Example 1.
[0106] Example 6
[0107] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0108] (1) Same as Example 1;
[0109] (2) adding epoxy resin and 37 wt % formaldehyde solution into a mixed solvent and stirring at 80° C. for 5 hours; the molar ratio of ammonia water to formaldehyde is 1:2.5;
[0110] (3) Same as Example 1;
[0111] (4) dispersing epoxy resin powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of epoxy resin to graphite of 50:50, and stirring at 75°C until the solvent is completely evaporated;
[0112] (5) The dried sample was transferred to a high temperature tube furnace and heated to 1300 °C at a heating rate of 1 °C min -1 , kept for 4 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0113] (6)~(9) are the same as in Example 1.
[0114] Example 7
[0115] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0116] (1) Same as Example 1;
[0117] (2) adding phenolic resin and 37 wt % formaldehyde solution into a mixed solvent and stirring at 85° C. for 4 hours; the molar ratio of ammonia water to formaldehyde is 1:2;
[0118] (3) separating the precipitate by centrifugation, washing it three times with water and ethanol, and then drying it at 80° C. for 12 hours to obtain a brown-yellow polymer powder;
[0119] (4) dispersing phenolic resin powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of phenolic resin to graphite of 10:90, and stirring at 75° C. until the solvent is completely evaporated;
[0120] (5) The dried sample was transferred to a high temperature tube furnace and heated to 1300 °C at a heating rate of 2 °C min -1 , maintained for 5 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0121] (6) (NH4)6Mo7O 24 ·4H2O powder was dissolved in deionized water, and Gr@HC was added to the solution under continuous stirring. (NH4)6Mo7O 24 The molar ratio of 4H2O to Gr@HC was 1:5, and the resulting mixed solution was dried at 80 °C for 12 h to form AMT@Gr@HC powder;
[0122] (7) The prepared powder was heated at 4 °C min under argon flow. -1 The MoO was annealed in a tube furnace at a heating rate of 400 °C for 3 h. x @Gr@HC powder;
[0123] (8) A mixed gas of NH3 and H2 with a volume ratio of 99:1 was introduced into a tube furnace and annealed at 520 °C for 1 h with a heating rate of 3 °C min -1 , at this time MoO is formed x -Mo y N@Gr@HC powder;
[0124] (9) After the obtained powder was cooled to room temperature, it was passivated in a mixed gas of N2 and O2 with a volume ratio of 90:10 for 1 hour.
[0125] Example 8
[0126] The method for preparing the negative electrode material provided in this embodiment comprises the following steps:
[0127] (1) Same as Example 1;
[0128] (2) adding phenolic resin and 37 wt % formaldehyde solution into a mixed solvent and stirring at 75° C. for 6 hours; the molar ratio of ammonia water to formaldehyde is 1:3;
[0129] (3) separating the precipitate by centrifugation, washing it three times with water and ethanol, and then drying it at 80° C. for 12 hours to obtain a brown-yellow polymer powder;
[0130] (4) dispersing phenolic resin powder and graphite in water, mixing with ethanol in a volume ratio of 1:1, and a mass ratio of phenolic resin to graphite of 10:90, and stirring at 75° C. until the solvent is completely evaporated;
[0131] (5) The dried sample was transferred to a high temperature tube furnace and heated to 1250 °C at a heating rate of 3 °C min -1 , kept for 4 hours to obtain the carbon material Gr@HC, under the protection of argon;
[0132] (6) (NH4)6Mo7O 24 ·4H2O powder was dissolved in deionized water, and Gr@HC was added to the solution under continuous stirring. (NH4)6Mo7O 24 The molar ratio of 4H2O and Gr@HC was 1:1, and the resulting mixed solution was dried at 80 °C for 12 h to form AMT@Gr@HC powder;
[0133] (7) The prepared powder was heated at 6 °C min under argon flow. -1 The MoO was annealed in a tube furnace at a heating rate of 250 °C for 2 h. x @Gr@HC powder;
[0134] (8) A mixed gas of NH3 and H2 with a volume ratio of 90:10 was introduced into a tube furnace and annealed at 480 °C for 3 h with a heating rate of 1 °C min -1 , at this time MoO is formed x -Mo y N@Gr@HC powder;
[0135] (9) After the obtained powder was cooled to room temperature, it was passivated in a mixed gas of N2 and O2 with a volume ratio of 99:1 for 3 hours.
[0136] Example 9
[0137] The only difference between this embodiment and embodiment 1 is that the mass ratio of phenolic resin to graphite is 5:95.
[0138] Example 10
[0139] The only difference between this embodiment and embodiment 1 is that in step 5, the sample is heated to 1400°C.
[0140] Embodiment 11
[0141] The only difference between this embodiment and embodiment 1 is that the heating rate in step 5 is 5° C. / min.
[0142] Example 12
[0143] The difference between this embodiment and embodiment 1 is that, in step 6, (NH4)6Mo7O 24 The molar ratio of 4H2O to Gr@HC is 1:8.
[0144] Embodiment 13
[0145] The only difference between this embodiment and embodiment 1 is that the heating rate in step 7 is 2°C min -1 .
[0146] Embodiment 14
[0147] The only difference between this embodiment and embodiment 1 is that the annealing temperature in step 7 is 200°C.
[0148] Embodiment 15
[0149] The only difference between this embodiment and embodiment 1 is that the annealing temperature in step 8 is 450°C.
[0150] Example 16
[0151] The only difference between this embodiment and embodiment 1 is that, in step 8, the volume ratio of NH3 and H2 is 50:50.
[0152] Comparative Example 1
[0153] The method for preparing the negative electrode material provided in this comparative example comprises the following steps:
[0154] (NH4)6Mo7O 24 ·4H2O powder was dissolved in deionized water, and Gr was added to the solution under continuous stirring. (NH4)6Mo7O 24 The molar ratio of 4H2O and Gr was 1:3; the obtained mixed solution was dried at 80°C for 12 hours to form AMT@Gr powder. -1 The MoOx@Gr powder was annealed in a tube furnace for 1 h at 370 °C with a heating rate of 2 °C min-1. Then, NH3 / H2 (95:5) mixed gas was introduced into the tube furnace and annealed at 500 °C for 1.5 h with a heating rate of 2 °C min-1. -1 The powder was cooled to room temperature and then passivated in a N2 / O2 (95:5) mixed gas for 2 hours.
[0155] Comparative Example 2
[0156] The method for preparing the negative electrode material provided in this comparative example comprises the following steps:
[0157] (NH4)6Mo7O 24·4H2O powder was dissolved in deionized water, and HC was added to the solution under continuous stirring. (NH4)6Mo7O 24 The molar ratio of 4H2O to HC was 1:3. The obtained mixed solution was dried at 80 °C for 12 h to form AMT@HC powder. Next, the prepared powder was heated at 5 °C min under an argon flow. -1 The MoOx@HC powder was annealed in a tube furnace for 1 h at 370 °C at a heating rate of 2 °C min-1. Then, NH3 / H2 (95:5) mixed gas was introduced into the tube furnace and annealed at 500 °C for 1.5 h at a heating rate of 2 °C min-1. -1 The powder was cooled to room temperature and then passivated in a N2 / O2 (95:5) mixed gas for 2 hours.
[0158] Comparative Example 3
[0159] The method for preparing the negative electrode material provided in this comparative example comprises the following steps:
[0160] 0.6 mL of NH3·H2O was dissolved in water and mixed with ethanol in a volume ratio of 1:1 and stirred at 40 °C for 30 min. Then, o-aminophenol and 37% formaldehyde solution were added to the mixed solvent and stirred at 80 °C for 5 h. The precipitate was separated by centrifugation, washed three times with water and ethanol, and then dried at 80 °C for 12 h to obtain a brown-yellow powder. Then, the polymer powder and 70% asphalt were dispersed in water and mixed with ethanol in a certain volume ratio and stirred at 75 °C until the solvent was completely evaporated. Then, the dried sample was transferred to a high-temperature tube furnace. Then, the sample was heated to 1300 °C with a heating rate of 1 °C min -1 , and kept for 4 hours to obtain the carbon material Gr@HC. The whole process was carried out under the protection of Ar atmosphere.
[0161] Comparative Example 4
[0162] The method for preparing the negative electrode material provided in this comparative example is different from that in Example 1 only in that step 9 is omitted.
[0163] Experimental example
[0164] The negative electrode materials, conductive carbon (carbon black) and binder PVDF prepared in each embodiment and comparative example were mixed in a weight ratio of 80:10:10. The obtained slurry was stirred for 12 hours and then coated on copper foil. The coated copper foil was heated at 80°C under vacuum for 12 hours. The obtained electrode was cut into circular sheets with a diameter of 12 mm. The mass loading of the half-cell negative electrode was controlled at 0.32-0.54 mgcm -2 The area capacity of the negative electrode half-cell is controlled at 0.95 mAh cm-2 .
[0165] For the half-cell (CR2025) assembly, the negative electrode prepared above was used as the working electrode, while the lithium metal electrode was used as the counter electrode. The battery was assembled in a glove box filled with argon (H2O, O2 < 0.1ppm). The electrolyte was 1M LiPF6 dissolved in EC, DMC and EMC in a volume ratio of 1:1, and the amount used was 50μL.
[0166] The electrochemical performance of the half-cell was tested, and the results are shown in Table 1.
[0167] Table 1 Electrochemical properties of negative electrode materials
[0168]
[0169]
[0170] It can be seen from Table 1 that the negative electrode material provided by the present invention has cycle stability and fast charging performance.
[0171] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A negative electrode material, characterized in that: include: A substrate and a modification material layer disposed on the surface of the substrate; Wherein, the matrix comprises: hard carbon and graphite covering the hard carbon; The chemical formula of the modifying material in the modifying material layer is MoO x -Mo y N, x is between 2 and 3, and y is between 1 and 2.
2. The negative electrode material according to claim 1, characterized in that Includes at least one of the following technical features: (1) The mass ratio of the hard carbon to the graphite is 10-50:50-90; (2) The thickness of the modified material layer is 500 nm to 1 μm; (3) The hard carbon comprises at least one of phenolic resin, epoxy resin or o-aminophenol.
3. The method for preparing the negative electrode material according to claim 1 or 2, characterized in that: The following steps are involved: (a) subjecting a mixed solution containing aqueous ammonia, hard carbon and formaldehyde to a first reaction and collecting a precipitate; (b) subjecting the dispersion containing the precipitate and graphite to a first drying treatment and calcining to obtain the matrix; (c) subjecting the mixed solution containing ammonium heptamolybdate and the substrate to a second drying treatment and a first annealing treatment; subjecting the product obtained by the first annealing treatment to a second annealing treatment under an atmosphere of ammonia and hydrogen; (d) Cooling and passivating the product obtained by the second annealing treatment under a nitrogen and oxygen atmosphere to obtain the negative electrode material.
4. The method for preparing the negative electrode material according to claim 3, characterized in that: Includes at least one of the following technical features: (1) The molar ratio of the aqueous ammonia to the formaldehyde is 1:1 to 3; (2) The temperature of the first reaction is 75-85°C; (3) The time of the first reaction is 4 to 6 hours.
5. The method for preparing the negative electrode material according to claim 3, characterized in that: Includes at least one of the following technical features: (1) The calcination temperature is 800-1300° C.; (2) The heating rate of the calcination is 1 to 3°C / min; (3) The calcination time is 2 to 5 hours.
6. The method for preparing the negative electrode material according to claim 3, characterized in that: Includes at least one of the following technical features: (1) The molar ratio of the ammonium heptamolybdate to the matrix is 1:(1-5); (2) The temperature of the first annealing treatment is 250-400° C.; (3) The first annealing treatment time is 1 to 3 hours; (4) The heating rate of the first annealing treatment is 4 to 6°C / min.
7. The method for preparing the negative electrode material according to claim 3, characterized in that: Includes at least one of the following technical features: (1) The temperature of the second annealing treatment is 480-800° C.; (2) The second annealing treatment time is 1 to 3 hours; (3) The heating rate of the second annealing treatment is 1 to 3°C / min; (4) During the second annealing treatment, the volume ratio of ammonia gas to hydrogen gas is 90-99:1-10.
8. The method for preparing the negative electrode material according to claim 3, characterized in that: Includes at least one of the following technical features: (1) The passivation time is 1 to 3 hours; (2) During the passivation, the volume ratio of nitrogen to oxygen is 90-99:1-10.
9. A negative electrode plate, characterized in that: The invention comprises the negative electrode material according to claim 1 or 2 or the negative electrode material prepared by the method for preparing the negative electrode material according to any one of claims 3 to 8.
10. A secondary battery, characterized in that: Including the negative electrode sheet as described in claim 9.
Citation Information
Cited By
Negative electrode material, preparation method therefor, and use thereof
WO2026045528A1