Nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm as well as preparation method and application thereof

Through one-step calcination, nitrogen, oxygen and sulfur co-doped porous carbon and compounded with polypropylene, the capacity attenuation problem of lithium-sulfur batteries is solved, high energy density and long cycle stability is achieved, process flow is simplified and production costs are reduced .

CN119050598APending Publication Date: 2024-11-29SHAANXI UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411362554.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the process of preparing porous carbon materials is complex, there are few types of doped elements and low specific surface area, resulting in faster attenuation of lithium-sulfur battery capacity.

Method used

Acemeth is used as the carbon, nitrogen, oxygen and sulfur source, and a porous carbon co-doped with nitrogen, oxygen and sulfur is formed by one step of calcination, and is compounded with polypropylene to form a porous carbon/polypropylene composite membrane, using its rich pore channels. The structure and high specific surface area inhibit the shuttle effect of polysulfides.

Benefits of technology

It significantly improves the electrochemical performance and cycle stability of lithium-sulfur batteries, extends the battery life, and reduces production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050598A_ABST
    Figure CN119050598A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and relates to a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm as well as a preparation method and application thereof. The preparation method comprises the following steps: preparing nitrogen, oxygen and sulfur heteroatom co-doped porous carbon by a one-step acesulfame potassium carbonization method; a polypropylene diaphragm is coated with the porous carbon to obtain the composite membrane, and the composite membrane has excellent polysulfide adsorption and catalysis performance. The preparation method is simple in technological process, low in production cost and energy consumption and easy for large-scale production. The porous carbon prepared by the method has rich macropore, mesopore and micropore structures and has a relatively large specific surface area; nitrogen, oxygen and sulfur heteroatoms provide adsorption and catalytic active sites; the prepared porous carbon / polypropylene composite diaphragm has excellent battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm and a preparation method and application thereof. Background Art

[0002] With the further development of the times, electric drive equipment has put forward further requirements on the performance of batteries. In particular, the rapid development of new energy electric vehicles has placed high demands on the capacity and energy density of power batteries. However, the lithium batteries currently carried by new energy electric vehicles have gradually exposed shortcomings such as poor endurance and heavy weight. Therefore, it is urgent to develop power batteries with high energy density and capacity.

[0003] Since the advent of lithium-sulfur batteries in the 1960s, they have been widely used due to their high theoretical capacity (1675 mAh g -1 ) and energy density (2600Wh kg -1 ) has always attracted much attention and has become a star battery for future electric vehicles to achieve ultra-long cruising. Lithium-sulfur battery is a battery system established in an organic electrolyte with metallic lithium as the negative electrode and sulfur material as the positive electrode. However, due to the combination of elemental sulfur and solid Li 2 S 2 / Li 2 S is an insulator, which reduces the reaction kinetics and the utilization rate of active materials, resulting in a faster capacity decay; secondly, the sulfur positive electrode expands in volume during the charge and discharge process, destroying the electrode structure and affecting the cycle stability; the most serious is the "shuttle effect" caused by lithium polysulfides that are easily soluble in organic electrolytes, which not only reduces the cycle life of lithium-sulfur batteries, but also causes corrosion and self-discharge behavior of the lithium metal negative electrode of lithium-sulfur batteries. Inhibiting the shuttling of polysulfides is the key to achieving high-performance lithium-sulfur batteries. The diaphragm is the only channel for polysulfides to diffuse, and the most direct way to prevent the shuttle effect is to design an ideal diaphragm that can not only ensure the diffusion of lithium ions, but also block the diffusion of polysulfides generated by the positive electrode, achieving high utilization of active materials and high energy density.

[0004] After searching, the invention patent CN112510170 A discloses a nitrogen-sulfur dual-doped porous carbon material that serves as both a sulfur host and a modified diaphragm material. This method uses citric acid and urea as nitrogen and carbon sources to form a gel in a mixed solvent, then heats the gel at high temperature to evaporate it, grinds the evaporated porous carbon precursor, and calcines it under hydrogen sulfide and inert gas to obtain nitrogen-sulfur dual-doped porous carbon. In addition to the cumbersome process and complex preparation process, this method uses a highly toxic acidic gas called hydrogen sulfide. In addition, the prepared carbon material has poor polarity and cannot effectively adsorb polysulfides. The nitrogen-sulfur dual-doped porous carbon has a low specific surface area, resulting in a rapid decay of the battery capacity.

[0005] In summary, the existing technology for preparing porous carbon has problems such as complex preparation method, few types of doping elements, low specific surface area, etc., which will lead to rapid capacity decay when applied to lithium-sulfur batteries. Summary of the invention

[0006] The purpose of the present invention is to provide a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm and its preparation method and application. Acesulfame potassium is used to simultaneously provide carbon, nitrogen, oxygen and sulfur sources without the need for other pore-forming activators and doping reagents. Nitrogen, oxygen and sulfur co-doped porous carbon is formed by one-step calcination. The porous carbon has a wide pore size distribution and a large specific surface area. The porous carbon / polypropylene composite diaphragm is prepared to solve the problem of rapid battery capacity decay.

[0007] The present invention is achieved through the following technical solutions:

[0008] A method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm, comprising:

[0009] Acesulfame potassium is used for carbonization reaction under a protective atmosphere to obtain a hierarchical porous carbon precursor co-doped with nitrogen, oxygen and sulfur atoms;

[0010] The hierarchical porous carbon precursor is washed and dried to obtain porous carbon;

[0011] The porous carbon is mixed with Ketjen black, a binder and a solvent, and ground into a slurry to obtain a diaphragm modification material;

[0012] The polypropylene diaphragm is coated with the diaphragm modification material to obtain a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm.

[0013] Furthermore, the acesulfame potassium needs to be pre-treated by ball milling for 20-40 minutes before carbonization.

[0014] Further, the protective atmosphere is nitrogen or argon;

[0015] The carbonization temperature is 850-950° C., and the carbonization time is 3-6 hours.

[0016] Furthermore, the cleaning is a two-step process of washing with dilute hydrochloric acid and washing with water until the surface is neutral; the drying temperature is 50-110° C., and the drying time is 6-20 hours.

[0017] Furthermore, the porous carbon contains micropores, mesopores and macropores at the same time, and the specific surface area is greater than 300m 2 g -1 ;

[0018] The diameter of micropores is <2nm, the diameter of mesopores is 2-50nm, and the diameter of macropores is >50nm.

[0019] Further, the method of coating the polypropylene diaphragm with the diaphragm modifying material is specifically as follows:

[0020] The membrane modification material is evenly applied to one side of the polypropylene membrane and vacuum dried;

[0021] The vacuum drying specifically includes: drying in a vacuum environment, the drying temperature is 50-60° C., and the drying time is 10-24 hours.

[0022] Furthermore, the binder is polyvinylidene fluoride and the solvent is N-methylpyrrolidone;

[0023] The mass ratio of porous carbon, Ketjen black and polyvinylidene fluoride is (7-9):(0.5-2):(0.5-1).

[0024] Furthermore, the thickness of the membrane modifying material after drying is 10-20 μm.

[0025] The invention also discloses a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm prepared by the preparation method.

[0026] The present invention also discloses the use of the nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm as a lithium-sulfur battery diaphragm in the preparation of a lithium-sulfur battery. When the diaphragm is used for the lithium-sulfur battery, the discharge capacity of the lithium-sulfur battery is greater than 1500 mAh g at a current density of 0.2C. -1 ;

[0027] At a high current density of 1C, the discharge capacity of the lithium-sulfur battery after 500 cycles is >800mAh g -1 capacity.

[0028] Compared with the prior art, the present invention has the following beneficial technical effects:

[0029] The invention discloses a method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm. The method comprises the following steps: firstly, a nitrogen, oxygen and sulfur heteroatom co-doped porous carbon is prepared by a one-step carbonization method of acesulfame potassium. 4 H 4 KNO 4 The molecular structure of S is rich in carbon, nitrogen, oxygen, sulfur and potassium. During the carbonization process, some potassium-containing groups decompose into SO 2 , CO 2 and K 2 O, and at the same time, the carbon atoms in the carbon skeleton are 2 and K 2O reacts to generate CO gas, thereby promoting the formation of micropores and mesopores in the carbon skeleton; the residual inorganic impurities in the carbon skeleton can be cleaned to obtain a continuous macroporous structure. Nitrogen, oxygen, and sulfur atoms are embedded in the carbon skeleton structure in situ to form a stable three-type heteroatom co-doping, which can adsorb lithium polysulfide and accelerate the electrochemical transformation kinetics of lithium polysulfide. Compared with the existing method of preparing porous carbon using template pore-forming agents and activators, the carbonization of acesulfame potassium belongs to a self-activation and self-template strategy, which avoids the waste and non-recyclability of template agents and activators.

[0030] Afterwards, the porous carbon material is mixed with Ketjen black, an adhesive and a solvent to obtain a membrane modification material; the membrane modification material is used to coat a modified polypropylene membrane to obtain a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane. Since the porous carbon material has a rich pore structure, it can provide a transmission channel for lithium ions. The porous carbon material can also fix lithium polysulfide by physical adsorption and chemical adsorption, reducing its shuttling between the positive and negative electrodes; Ketjen black has good electrical conductivity, which can enhance the electronic conductivity of the electrode, thereby promoting the transmission process of lithium ions. The high conductivity of Ketjen black helps to maintain the stability of the electrochemical properties of the electrode and reduce the impact of lithium polysulfide shuttling on battery performance; the adhesive can firmly bond the porous carbon material and Ketjen black to the polypropylene membrane to ensure the stability of the lithium ion transmission channel. The bonding effect can also ensure the integrity of the coating layer and prevent lithium polysulfide from shuttling through the gaps in the coating layer; the solvent enables the various components to be evenly mixed, creating a good microscopic environment for lithium ion transmission, making the effect of inhibiting lithium polysulfide shuttling more significant.

[0031] The preparation method of the present invention has a simple process flow, is easy to operate, does not require the use of additional templates and activators, has low production costs and energy consumption, is easy to mass produce, and has the value of commercial-scale production.

[0032] Furthermore, acesulfame potassium needs to be pre-treated by ball milling for 20-30 minutes before high-temperature carbonization. Ball milling subjects the powder to multiple forces such as impact, shear and compression, causing it to pre-react in advance, which is beneficial to the formation of porous carbon.

[0033] Furthermore, the carbonization temperature of acesulfame potassium is 850-950°C, and the carbonization time is 4-6 hours. Too low a carbonization temperature will reduce the degree of graphitization, thereby reducing conductivity; too high a carbonization temperature will cause the loss of doping atoms, reduce the doping amount and increase energy consumption.

[0034] Furthermore, HCl and H 2 O washes the inorganic impurities remaining in the carbon skeleton to obtain a continuous macroporous structure.

[0035] Furthermore, the thickness of the membrane modification material after drying is 10-20 μm. When the coating layer has a certain thickness, the mixed material can inhibit the shuttle effect of lithium polysulfide. If the coating layer is too thick, it will hinder the transmission of lithium ions, because the excessively thick coating layer will increase the path length of lithium ion diffusion and reduce the migration rate of lithium ions; if the coating layer is too thin, it is difficult to fully exert the inhibitory effect on the shuttle effect of lithium polysulfide.

[0036] The present invention also discloses a porous carbon / polypropylene composite diaphragm obtained by adopting the above-mentioned preparation method, which can be applied to the diaphragm of a lithium-sulfur battery, can greatly improve the electrochemical performance of the lithium-sulfur battery, and has a significant improvement in capacity performance and cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is the X-ray diffraction (XRD) spectrum of nitrogen, oxygen, and sulfur co-doped porous carbon (NOSAKC) prepared in Example 1;

[0038] Figure 2 This is an X-ray photoelectron spectrum (XPS) diagram of the NOSAKC material prepared in Example 1;

[0039] Figure 3 This is a scanning electron microscope (SEM) image of the NOSAKC material prepared in Example 1;

[0040] Figure 4 This is a transmission electron microscope (TEM) image of the NOSAKC material prepared in Example 1;

[0041] Figure 5a This is the BET graph obtained from the nitrogen adsorption test of the NOSAKC material prepared in Example 1;

[0042] Figure 5b This is the pore size distribution diagram obtained by nitrogen adsorption test of the NOSAKC material prepared in Example 1;

[0043] Figure 6 This is a cross-sectional SEM image of the porous carbon / polypropylene composite diaphragm prepared in Example 1;

[0044] Figure 7 The cycling performance of the porous carbon / polypropylene composite separator and pure polypropylene separator prepared in Example 1 at 1C in a lithium-sulfur battery;

[0045] Figure 8 The rate performance of the porous carbon / polypropylene composite separator and pure polypropylene separator prepared in Example 1 in lithium-sulfur batteries. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solution and advantages of the present invention more clear, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, not all embodiments.

[0047] The detailed description of the embodiments of the present invention provided in the following drawings is not intended to limit the scope of the invention claimed for protection, but merely represents a selected embodiment of the present invention. Based on the drawings and embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0048] The present invention discloses a method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm, comprising:

[0049] Acesulfame potassium is used for carbonization reaction under a protective atmosphere to obtain a hierarchical porous carbon precursor co-doped with nitrogen, oxygen and sulfur atoms;

[0050] The hierarchical porous carbon precursor is washed and dried to obtain porous carbon;

[0051] The porous carbon is mixed with Ketjen black, a binder and a solvent, and ground into a slurry to obtain a diaphragm modification material;

[0052] The polypropylene diaphragm is coated with the diaphragm modification material to obtain a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm.

[0053] Acesulfame potassium is used as a raw material as a source of carbon, nitrogen, oxygen and sulfur, and a graded porous carbon doped with a large amount of nitrogen, oxygen and sulfur atoms is obtained through a one-step pyrolysis method; the graded porous carbon is coated on a polypropylene diaphragm to obtain a composite membrane, which has excellent polysulfide adsorption and catalytic properties and is suitable for lithium-sulfur batteries.

[0054] The preparation method has a simple process flow, low production cost and energy consumption, and is easy to mass produce. The porous carbon prepared by the present invention has a rich macropore, mesopore and micropore structure, and has a large specific surface area; nitrogen, oxygen, and sulfur atoms provide adsorption and catalytic active sites, showing excellent battery performance.

[0055] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0056] Example 1

[0057] The present invention discloses a method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm, comprising the following steps:

[0058] (1) After 10 g of acesulfame potassium was ball-milled for 20 min, it was placed in a corundum porcelain boat and then transferred to a tubular furnace. Argon was used as a protective gas, and the temperature was raised from room temperature to 900 ° C and calcined for 3 h. The temperature was naturally cooled to room temperature to obtain a graded porous carbon precursor co-doped with nitrogen, oxygen, and sulfur atoms.

[0059] (2) Then the graded porous carbon precursor is ground and poured into dilute hydrochloric acid and stirred for 2 hours to completely remove inorganic impurities; finally, centrifuged, repeatedly washed with deionized water until the pH reaches 7, and vacuum dried at 80°C for 12 hours to obtain nitrogen-, oxygen-, and sulfur-doped porous carbon.

[0060] (3) adding porous carbon, Ketjen black and PVDF in a mass ratio of 8:1:1 to N-methylpyrrolidone and mixing evenly to obtain a membrane modification material;

[0061] (4) The membrane modification material is uniformly coated on the surface of the polypropylene membrane and vacuum dried at 50°C for 12 hours to obtain a composite membrane, which is labeled as NOSAKC / PP.

[0062] In a glove box, lithium-sulfur batteries were assembled using NOSAKC / PP as a separator, with the side of the composite separator containing the active material NOSAKC facing the positive electrode, and the battery performance could then be tested.

[0063] The XRD pattern of NOSAKC in this Example 1 is as follows Figure 1 As shown, there are two main peaks in the diffraction pattern of NOSAKC material, at 24.6° and 44° respectively, and the characteristic peak at 2θ=24.6° corresponds to the (002) crystal plane of carbon.

[0064] The XPS pattern of NOSAKC in this Example 1 is as follows Figure 2 As shown, nitrogen, oxygen and sulfur atoms have been successfully incorporated into porous carbon.

[0065] The NOSAKC material prepared in Example 1 was subjected to SEM analysis. Figure 3 As shown, it can be observed that there are abundant macroporous structures on the surface of NOSAKC material.

[0066] The NOSAKC material prepared in Example 1 was subjected to TEM analysis. Figure 4 As shown, it can be observed that NOSAKC material has abundant pore cross-linking.

[0067] The specific surface area and pore distribution of NOSAKC in Example 1 are as follows: Figure 5a and Figure 5b As shown, NOSAKC material has a large specific surface area of ​​336.7 m 2 g -1And rich micropore, mesopore and macropore structure. The diameter of micropore is <2nm, the diameter of mesopore is 2~50nm, and the diameter of macropore is >50nm.

[0068] The cross-sectional SEM of NOSAKC / PP in Example 1 is as follows: Figure 6 As shown, the thickness of the coating is 18 μm.

[0069] The assembled battery is subjected to long cycle stability test and rate test. Figure 7 The battery with the composite separator shown in the figure was subjected to a constant current charge and discharge long cycle test at a current density of 1C. It can be seen that after 500 cycles, there is still 817 mAh g -1 The capacity of the battery is 99.8%.

[0070] Depend on Figure 8 The rate performance test results of the battery containing the composite separator shown in the figure show that the discharge specific capacities of the battery at 0.2C, 0.3C, 0.5C, 1C, 2C and 3C are 1598.5, 1360.2, 1224.3, 1022.6, 851.3 and 713.5 mAh g -1 The battery performance of the composite diaphragm is significantly improved compared with that of the pure polypropylene diaphragm.

[0071] Example 2

[0072] The present invention discloses a method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm, comprising the following steps:

[0073] (1) After 10 g of acesulfame potassium was ball-milled for 30 min, it was placed in a corundum porcelain boat and then transferred to a tubular furnace. Argon was used as a protective gas, and the temperature was raised from room temperature to 950 ° C and calcined for 5 h. The temperature was naturally cooled to room temperature to obtain a graded porous carbon precursor co-doped with nitrogen, oxygen, and sulfur atoms.

[0074] (2) The graded porous carbon precursor is then ground and poured into hydrochloric acid and stirred thoroughly to completely remove inorganic impurities; finally, it is centrifuged and washed with deionized water until the pH reaches 7, and then vacuum dried at 110°C for 18 hours to obtain nitrogen-, oxygen-, and sulfur-doped porous carbon, which is recorded as NOSAKC.

[0075] (3) NOSAKC, Ketjen black and PVDF were added to N-methylpyrrolidone in a mass ratio of 7:2:1 and mixed evenly to obtain a membrane modification material;

[0076] (4) The membrane modification material was uniformly coated on the surface of the polypropylene membrane and vacuum dried at 60°C for 20 hours to obtain a composite membrane, which was labeled as NOSAKC / PP. The coating thickness of NOSAKC was 15 μm.

[0077] The obtained NOSAKC / PP separator was assembled into a lithium-sulfur battery, and the assembled battery was subjected to a long cycle stability test and a rate test. The discharge capacity at a current density of 0.2C was 1523mAh g -1 At a high current density of 1C, the battery has a discharge capacity of 810 mAh g after 500 cycles. -1 .

[0078] Example 3

[0079] The present invention discloses a method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm, comprising the following steps:

[0080] (1) After 10 g of acesulfame potassium was ball-milled for 40 min, it was placed in a corundum porcelain boat and then transferred to a tubular furnace. Nitrogen was used as a protective gas, the temperature was raised from room temperature to 850 ° C and calcined for 6 h, and then naturally cooled to room temperature to obtain a porous carbon precursor co-doped with nitrogen, oxygen, and sulfur atoms.

[0081] (2) The hierarchical porous carbon precursor is then ground and poured into hydrochloric acid and stirred thoroughly to completely remove inorganic impurities; finally, the mixture is centrifuged and washed with deionized water until the pH reaches 7, and then vacuum dried at 100°C for 20 hours to obtain nitrogen-, oxygen-, and sulfur-doped hierarchical porous carbon, which is denoted as NOSAKC.

[0082] (3) NOSAKC, Ketjen black and PVDF were added with N-methylpyrrolidone in a mass ratio of 9:0.5:0.5 and mixed evenly to obtain a membrane modification material;

[0083] (4) The membrane modification material was evenly coated on the surface of the polypropylene membrane and vacuum dried at 60°C for 24 hours to obtain a modified membrane, which was labeled as NOSAKC / PP. The coating thickness of NOSAKC was 10 μm.

[0084] The obtained NOSAKC / PP separator was assembled into a lithium-sulfur battery, and the assembled battery was subjected to a long cycle stability test and a rate test. The discharge capacity at a current density of 0.2C was 1531 mAh g -1 At a high current density of 1C, the battery has a discharge capacity of 814 mAh g after 500 cycles. -1 .

[0085] Example 4

[0086] The present invention discloses a method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm, comprising the following steps:

[0087] (1) After 10 g of acesulfame potassium was ball-milled for 30 min, it was placed in a corundum porcelain boat and then transferred to a tubular furnace. Nitrogen was used as a protective gas, the temperature was raised from room temperature to 850 ° C and calcined for 5 h, and then naturally cooled to room temperature to obtain a porous carbon precursor co-doped with nitrogen, oxygen, and sulfur atoms.

[0088] (2) The hierarchical porous carbon precursor is then ground and poured into hydrochloric acid and stirred thoroughly to completely remove inorganic impurities; finally, it is centrifuged and washed with deionized water until the pH reaches 7, and then vacuum dried at 50°C for 20 hours to obtain nitrogen-, oxygen-, and sulfur-doped hierarchical porous carbon, which is denoted as NOSAKC.

[0089] (3) NOSAKC, Ketjen black and PVDF were added to N-methylpyrrolidone in a mass ratio of 9:2:1 and mixed evenly to obtain a membrane modification material;

[0090] (4) The membrane modification material was evenly coated on the surface of the polypropylene membrane and vacuum dried at 60°C for 24 hours to obtain a modified membrane, which was labeled as NOSAKC / PP. The coating thickness of NOSAKC was 20 μm.

[0091] The obtained NOSAKC / PP separator was assembled into a lithium-sulfur battery, and the assembled battery was subjected to a long cycle stability test and a rate test. The discharge capacity at a current density of 0.2C was 1556 mAh g -1 At a high current density of 1C, the battery has a discharge capacity of 810 mAh g after 500 cycles. -1 .

[0092] The present invention provides a method for preparing hierarchical porous carbon doped with three kinds of heteroatoms with a simple process. The porous carbon obtained by one-step pyrolysis has a large number of macropores, mesopores and micropores, as well as rich nitrogen, oxygen and sulfur heteroatom doping. The heteroatoms doped in situ have a strong chemical adsorption effect on polysulfides, effectively inhibiting the shuttle effect of polysulfides. In addition, the hierarchical porous carbon skeleton structure not only effectively limits the shuttle effect, but also has good lithium affinity and electrolyte wettability, which is conducive to the rapid conduction of electrons and ions. The polar porous carbon is applied to the modification of the diaphragm for lithium-sulfur batteries, which can greatly improve the capacity and cycle stability of lithium-sulfur batteries, and can still show excellent cycle stability under low E / S ratio.

[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane, characterized in that: include: Acesulfame potassium is used for carbonization reaction under a protective atmosphere to obtain a hierarchical porous carbon precursor co-doped with nitrogen, oxygen and sulfur atoms; The hierarchical porous carbon precursor is washed and dried to obtain porous carbon; The porous carbon is mixed with Ketjen black, a binder and a solvent, and ground into a slurry to obtain a diaphragm modification material; The polypropylene diaphragm is coated with the diaphragm modification material to obtain a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm.

2. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The acesulfame potassium needs to be pre-treated by ball milling for 20-40 minutes before carbonization.

3. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The protective atmosphere is nitrogen or argon; The carbonization temperature is 850-950° C., and the carbonization time is 3-6 hours.

4. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The cleaning comprises two steps of washing with dilute hydrochloric acid and washing with water until the mixture is neutral; the drying temperature is 50-110° C., and the drying time is 6-20 hours.

5. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The porous carbon contains micropores, mesopores and macropores at the same time, with a specific surface area of ​​>300m 2 g -1 ; The diameter of micropores is <2nm, the diameter of mesopores is 2-50nm, and the diameter of macropores is >50nm.

6. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The method of coating the polypropylene diaphragm with the diaphragm modifying material is specifically as follows: The membrane modification material is evenly applied to one side of the polypropylene membrane and vacuum dried; The vacuum drying specifically includes: drying in a vacuum environment, the drying temperature is 50-60° C., and the drying time is 10-24 hours.

7. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The adhesive is polyvinylidene fluoride, and the solvent is N-methylpyrrolidone; The mass ratio of porous carbon, Ketjen black and polyvinylidene fluoride is (7-9):(0.5-2):(0.5-1).

8. The method for preparing a nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane according to claim 1, characterized in that: The thickness of the membrane modification material after drying is 10-20 μm.

9. A nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite membrane prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the nitrogen, oxygen and sulfur co-doped porous carbon / polypropylene composite diaphragm as claimed in claim 9 as a lithium-sulfur battery diaphragm in the preparation of lithium-sulfur batteries, characterized in that: When applied to lithium-sulfur battery separators, the discharge capacity of lithium-sulfur batteries is >1500mAh g at a current density of 0.2C. -1 ; At a high current density of 1C, the discharge capacity of the lithium-sulfur battery after 500 cycles is >800mAh g -1 capacity.

Citation Information

Patent Citations

  • Nitrogen and sulfur double-doped porous carbon lithium-sulfur battery positive electrode material as well as preparation method and application thereof

    CN112510170A