Simple preparation method of piezoelectric film
The piezoelectric thin film prepared by the simplified gelation method solves the problems of complex preparation and high cost in the existing technology, and realizes high-quality, large-area, stable and uniform piezoelectric thin films with high sensitivity and high stability, which are suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202411263475.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
Existing piezoelectric thin film preparation methods are complex and costly, making it difficult to achieve large-scale production and application. Furthermore, the microstructure and piezoelectric properties of the thin films are difficult to control.
A simple gelation method is used, in which piezoelectric material powder with a particle size of less than 50 μm is mixed with PVA, and piezoelectric films are prepared by grinding, dissolving, coating and polarization. This method is applicable to a variety of piezoelectric materials and matrix materials.
It simplifies the preparation process, reduces costs, improves the uniformity and stability of the film, expands the application range, and possesses highly sensitive and stable piezoelectric properties, meeting the requirements of sustainable development.
Smart Images

Figure CN119053232A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of piezoelectric materials, and in particular relates to a method for preparing a piezoelectric film by a simple gel method. Background Art
[0002] In the field of piezoelectric materials, piezoelectric thin films, as an important functional material, have broad application prospects, especially in the fields of sensors, transducers, acoustic wave devices, etc. Traditional methods for preparing piezoelectric thin films include sputtering, chemical vapor deposition, solution spin coating, etc. These methods usually require complex equipment and processes, and are costly, which limits their promotion in large-scale production and application. Therefore, seeking a simple and low-cost method for preparing piezoelectric thin films has become one of the current research hotspots.
[0003] In recent years, the gel method has been widely studied as a simple and potential method for preparing thin films. The gel method is to dissolve polymer materials and other functional materials in a solvent to form a uniform solution, and then obtain the desired thin film material through methods such as coating, spin coating or casting and appropriate curing process. As a multiphase system, the gel contains a continuous and disordered three-dimensional structure in the solvent, which can stably disperse and fix the piezoelectric material powder, providing uniform support for the formation of the film. In the preparation process, it is necessary to select suitable matrix materials and piezoelectric material powders. The matrix material provides the basic structure and stability for the film, while the piezoelectric material powder gives the film piezoelectric properties. In the later stage of the preparation process, an appropriate curing process, such as drying or hot pressing, can solidify the gel system into a piezoelectric film. While curing, the matrix material forms a continuous phase and interacts with the piezoelectric material powder, so that the film also has piezoelectric properties. Compared with traditional methods, the gel method has the advantages of simple process, convenient operation and low cost.
[0004] In the preparation of piezoelectric films, selecting suitable polymer materials is a key step. Among them, soluble polymer materials such as polyvinyl alcohol (PVA) are widely used in the gel method. PVA has good water solubility and film-forming properties, and can be fully mixed with functional materials such as piezoelectric ceramic powder to form a uniform solution, and then prepared into a film. In addition, PVA also has good mechanical properties, chemical stability and biocompatibility, which can meet the needs of piezoelectric films in different application scenarios.
[0005] However, the gel preparation method of piezoelectric thin films still has some challenges and problems to be solved. For example, how to regulate the microstructure and piezoelectric properties of the film, how to improve the process stability and film quality of the film, etc. are the focus and difficulty of current research. The present invention optimizes the preparation process, improves the performance of the film, and provides a simple gel method for preparing piezoelectric thin films, which can prepare high-quality, large-area, stable and uniform, high-performance piezoelectric thin film materials. Summary of the invention
[0006] The present invention provides a simple preparation method of a piezoelectric film, aiming to simplify the existing process, reduce manufacturing costs, and improve stability and piezoelectricity. The piezoelectric film is prepared by grinding, mixing, and dissolving at high temperature using piezoelectric material powder and a mixed solution of PVA / PVOH as raw materials.
[0007] Preferably, the piezoelectric material is a powder with a particle size of less than 50 um, because the powder below 50 um has a higher degree of fusion with PVA and there will be no obvious granular phenomenon on the surface after film formation.
[0008] Preferably, if the piezoelectric material is a conventional ceramic ferroelectric material, the ceramic raw powder must first be fired into cooked powder in a high-temperature muffle furnace, and then the cooked powder must be ball-milled, dried, and repeatedly sieved through a 300-mesh sieve.
[0009] Preferably, the preparation process of the piezoelectric film mixed solution is as follows, wherein the piezoelectric material is selected from piezoelectric ceramic lead zirconate titanate (PZT):
[0010] (1) PZT cooked powder and PVA powder were weighed and mixed in a mass ratio of 4:1 and ground for 30 min to obtain PZT / PVA mixed powder;
[0011] (2) The mixed powder in step (1) is placed in a beaker, and deionized water is added to the beaker in a mass ratio of deionized water to PVA of 10:1. The mixture is magnetically stirred at 60°C for 2 hours to obtain a PZT / PVA mixed solution, which is then allowed to stand for about 4 hours to remove bubbles.
[0012] (3) applying the mixed solution obtained in step (2) by means of a tape casting machine;
[0013] (4) placing the sample obtained in step (3) into a drying machine and drying it at 60° C. for 4 h, then peeling off the PZT piezoelectric film from the cast plate along the edge;
[0014] (5) The PZT piezoelectric film obtained in step (4) was polarized for 15 min using a polarizer, and the polarization voltage was set to 1.5 kV.
[0015] Preferably, the preparation process of the mixed solution is also applicable to the preparation of zinc oxide piezoelectric thin films, molybdenum disulfide piezoelectric thin films, and hexagonal boron nitride piezoelectric thin films. Among them, two-dimensional materials such as molybdenum disulfide and hexagonal boron nitride do not need to be polarized.
[0016] It can be seen from the above technical solutions that the simple gel method for preparing piezoelectric thin films described in the present invention has certain advantages, which are as follows:
[0017] 1. This method is easy to operate and efficient, does not require complicated equipment and process flow, and can quickly prepare high-quality piezoelectric films.
[0018] 2. The characteristics of the gel ensure the uniform dispersion of the piezoelectric material powder in the solution, thereby improving the uniformity and stability of the film, while also ensuring good forming properties of the film
[0019] 3. The gel method is suitable for a variety of different types of piezoelectric materials and matrix materials, and can flexibly respond to different application requirements, expanding the application range of piezoelectric films.
[0020] 4. Environmentally friendly solvents and materials are used in the gel preparation process, which has little impact on the environment and meets the requirements of sustainable development.
[0021] 5. The prepared piezoelectric film has excellent piezoelectric properties and can realize the preparation of piezoelectric devices with high sensitivity and high stability.
[0022] 6. The process parameters in the gel preparation process are highly adjustable, which can achieve precise control of the various properties of the film to meet the needs of different application fields.
[0023] 7. Due to the relatively low preparation cost, this method is expected to reduce the preparation cost of the product and improve market competitiveness.
[0024] In summary, the simple gel method for preparing piezoelectric films has significant advantages in both technology and economy, and is expected to promote the widespread application of piezoelectric materials in various application fields and promote scientific and technological innovation and industrial development. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Attached Figure 1 This is the SEM morphology of the PZT powder in Example 1.
[0026] Attached Figure 2 This is an actual picture of the PZT thin film in Example 1.
[0027] Attached Figure 3 This is the SEM cross-sectional image of the PZT thin film in Example 1.
[0028] Attached Figure 4 This is a sensitivity curve diagram of the PZT film in Example 1.
[0029] Attached Figure 5 This is the hysteresis loop diagram of the ferroelectric test of the PZT thin film in Example 1.
[0030] Attached Figure 6 This is the PFM scanning morphology image of the PZT film in Example 1.
[0031] Attached Figure 7 This is the butterfly curve diagram of the PZT film in Example 1.
[0032] Attached Figure 8 This is the actual picture of the MoS2 film in Example 2.
[0033] Attached Fig. 9 This is the SEM morphology of the MoS2 film in Example 2.
[0034] Attached Fig.10 This is the sensitivity curve of the MoS2 film in Example 2.
[0035] Attached Fig.11 This is the PFM scanning morphology image of the MoS2 film in Example 2.
[0036] Attached Fig.12 This is the butterfly curve diagram of the MoS2 film in Example 2.
[0037] Attached Fig.13 This is the hysteresis loop diagram of the MoS2 film in Example 2.
[0038] Attached Fig.14 This is the actual picture of the ZnO thin film in Example 3.
[0039] Attached Fig.15 This is a sensitivity curve diagram of the ZnO film in Example 3.
[0040] Attached Fig.16 This is the PFM scanning morphology image of the ZnO film in Example 3.
[0041] Attached Fig.17 This is the butterfly curve diagram of the ZnO film in Example 3.
[0042] Attached Fig.18 This is the hysteresis loop diagram of the ZnO film in Example 3. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Example 1: This example discloses a simple method for preparing a piezoelectric film to prepare a PZT / PVA piezoelectric film. The preparation steps are as follows:
[0045] (1) Weigh 50g of PZT piezoelectric ceramic powder and place it in a crucible, and then put it into a muffle furnace for sintering. The sintering conditions are: heating to 550℃ at a rate of 10℃ / min and keeping it warm for 2h, then heating to 1210℃ at a rate of 10℃ / min and keeping it warm for 5h. After cooling, PZT powder is obtained. The obtained powder is repeatedly ground and sieved 5 times with a 300-mesh screen to obtain a finer PZT powder. The material shows obvious granularity in the SEM image, see the attached Figure 1 .
[0046] (2) Preparation of PZT / PVA piezoelectric film.
[0047] (21) Weigh the raw materials according to the mass ratio of PZT powder: PVA powder: deionized water = 4:1:10;
[0048] (22) 20.00 g of PZT powder and 5.00 g of PVA powder were mixed and ground for 30 min to obtain PZT / PVA mixed powder;
[0049] (23) The mixed powder in step (22) was placed in a beaker, and deionized water was added to the beaker. The mixture was magnetically stirred at 90° C. and 300 r / min for 1 h to obtain a PZT / PVA mixed solution, which was allowed to stand for about 4 h to remove bubbles.
[0050] (24) applying a knife coating to the mixed solution obtained in step (23) on a casting machine;
[0051] (25) Place the sample obtained in step (24) in a dryer and dry at 60°C for 4 h. Peel off the PZT piezoelectric film from the cast sheet along the edge. Figure 2 ;
[0052] (26) The PZT piezoelectric film obtained in step (25) was polarized by a polarizer with a polarization voltage of 1.5 KV and a polarization time of 15 min.
[0053] (3) The thickness of the prepared PZT piezoelectric film was measured by SEM electron microscope and its cross-sectional morphology was scanned. It was found that the PZT cooked powder was completely and evenly distributed in the PVA gel with a thickness of 73.15 μm. Figure 3 As shown; the film was prepared into a simple sensor, and the sensitivity of the PZT piezoelectric film was detected to be 206.5mV / g under the condition of 100 times charge magnification by the standard sensor test system, see the attached Figure 4 ; The hysteresis loop of the PZT film was tested by a ferroelectric tester. It can be seen that the PZT film has a large residual polarization intensity and has good ferroelectricity. Figure 5 ; PFM test shows that the film has more crystals in its microscopic morphology, see attached Figure 6(a), piezoelectric domains appear, see attached Figure 6 (b), and the piezoelectric coefficient d of the PZT piezoelectric film can be calculated through the butterfly curve 33 It is about 353 pm / V, indicating that the piezoelectric film has excellent piezoelectric properties.
[0054] Example 2: This example discloses a simple method for preparing a piezoelectric film to prepare a MoS2 / PVA piezoelectric film. The preparation steps are as follows:
[0055] (1) Weigh the raw materials according to the mass ratio of MoS2 powder: PVA powder: deionized water = 4:1:10.
[0056] (2) 8.00 g of MoS2 powder was mixed with 2.00 g of PVA powder and ground for 30 min to obtain MoS2 / PVA mixed powder.
[0057] (3) Place the mixed powder in step (2) into a beaker, and add 20 ml of deionized water into the beaker. Stir magnetically at 90°C and 300 r / min for 1 h to obtain a MoS2 / PVA mixed solution. Leave the solution for about 4 h to remove bubbles.
[0058] (4) The mixed solution obtained in step (3) is coated on a casting machine.
[0059] (5) Place the sample obtained in step (4) in a dryer and dry at 60°C for 4 h. Peel off the MoS2 piezoelectric film from the cast sheet along the edge. Figure 8 .
[0060] (6) The MOS2 / PVA piezoelectric film was scanned by SEM to measure the morphology and thickness of the MOS2 film, and the cross-sectional morphology of the MOS2 piezoelectric film was observed. It can be seen that the MOS2 powder has been completely and evenly distributed in the PVA gel, see Appendix Fig. 9 The thickness of the prepared film is 31.13 μm. The film is prepared into a simple sensor. Through the standard sensor test system, the sensitivity of the MOS2 piezoelectric film is detected to be 17.6 mV / g without adding amplification. See the attached Fig.10 ;Thin film tested by PFM, see attached Figure 11-13 It was observed that the film showed obvious unit cell growth, accompanied by the appearance of piezoelectric domains, and d 33 It is about 14.6 pm / V, and the hysteresis loop also shows good spontaneous polarization, indicating that the piezoelectric film prepared by the gel method has good piezoelectric properties.
[0061] Example 3: This example discloses a simple method for preparing a piezoelectric film to prepare a ZnO / PVA piezoelectric film. The preparation steps are as follows:
[0062] (1) Weigh the raw materials according to the mass ratio of ZnO powder: PVA powder: deionized water = 4:1:10.
[0063] (2) Mix 8.00 g of ZnO powder and 2.00 g of PVA powder in a certain proportion and grind them for 30 min to obtain a ZnO / PVA mixed powder.
[0064] (3) The mixed powder in step (2) was placed in a beaker, and 20 ml of deionized water was added to the beaker. The mixture was magnetically stirred at 90°C and 300 r / min for 1 h to obtain a ZnO / PVA mixed solution. The solution was allowed to stand for about 4 h to remove bubbles.
[0065] (4) The mixed solution obtained in step (3) is coated on a tape casting machine.
[0066] (5) Place the cast sheet after the casting in step (4) into a dryer and dry at 60°C for 4 h. Peel off the ZnO piezoelectric film from the cast sheet along the edge. Fig.14 .
[0067] (6) The prepared ZnO piezoelectric film was made into a simple sensor. The sensitivity of the ZnO piezoelectric film was detected to be 15.5 mV / g under 10 times voltage amplification by a standard sensor test system. Fig.15 ; Pass PFM test, as attached Figure 16-18 , it is observed that there is obvious growth of unit cells, accompanied by the appearance of piezoelectric domains, and d 33 It is about 175.8 pm / V, and the hysteresis loop shows good spontaneous polarization. It can be analyzed that the material is a single crystal piezoelectric material with excellent piezoelectric properties.
[0068] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A simple method for preparing a piezoelectric film, characterized in that: The piezoelectric film is prepared using piezoelectric material powder and solution PVA (polyvinyl alcohol) or PVOH (polyvinyl alcohol-polyvinyl ether) as raw materials through grinding, mixing and high-temperature dissolution.
2. The piezoelectric material according to claim 1 should be a powder with a particle size of less than 50 um, because the powder below 50 um has a higher degree of fusion with PVA and there will be no obvious granularity on the surface after film formation.
3. The piezoelectric material according to claim 1, if a traditional ceramic ferroelectric material such as PZT is selected, the ceramic raw powder must first be sintered into cooked powder in a high-temperature muffle furnace, and then the cooked powder must be ball-milled, dried and repeatedly sieved through a 300-mesh sieve.
4. The preparation process of the piezoelectric thin film mixed solution according to claim 1 is as follows, wherein the piezoelectric material is selected from piezoelectric ceramic lead zirconate titanate (PZT): (1) PZT cooked powder and PVA powder were weighed and mixed in a mass ratio of 4:1 and ground for 30 min to obtain PZT / PVA mixed powder; (2) The mixed powder in step (1) is placed in a beaker, and deionized water is added to the beaker in a mass ratio of deionized water to PVA of 10:
1. The mixture is magnetically stirred at 60°C for 2 hours to obtain a PZT / PVA mixed solution, which is then allowed to stand for about 4 hours to remove bubbles. (3) applying the mixed solution obtained in step (2) onto a casting plate through a casting machine, and casting the film according to the desired film thickness; (4) placing the sample obtained in step (3) into a drying machine and drying it at 60° C. for 4 h, then peeling off the PZT piezoelectric film from the cast plate along the edge; (5) The PZT piezoelectric film obtained in step (4) was polarized for 15 min using a polarizer, and the polarization voltage was set to 1.5 kV.
5. The preparation process of the piezoelectric material / polyvinyl alcohol mixed solution according to claim 4 is also applicable to the preparation of zinc oxide piezoelectric film, molybdenum disulfide piezoelectric film, and hexagonal boron nitride piezoelectric film. Two-dimensional materials such as molybdenum disulfide and hexagonal boron nitride do not require polarization.
Citation Information
Cited By
Flexible ferroelectric material, preparation method and application thereof
CN119613740A