Multi-layer TPO waterproof coiled material and preparation method thereof
By designing reasonable hierarchy and material components in multi-layer TPO waterproof coils, combining self-healing materials and antioxidants, the problems of aging and insufficient performance of traditional coils are solved, and higher waterproofing effect and service life are achieved , improves the energy efficiency and construction adaptability of the building.
Patent Information
- Application Number
- CN202411252028.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional waterproof coils are prone to aging and cracking during long-term use, resulting in a decrease in waterproofing effect. The existing multi-layer TPO waterproof coils lack performance in thermal insulation and self-healing.
A multi-layer TPO waterproof coil material is designed, including an upper surface protective layer, a functional layer, a thermal insulation layer and a bottom surface protective layer. By reasonably configuring the components of each layer of materials, self-healing materials, antioxidants, and ultraviolet rays are used. Absorbents, nanomaterials and optimized preparation processes to improve the overall performance of the coil.
It effectively improves the comprehensive performance of waterproof coils, including self-healing, weather resistance, mechanical properties, thermal insulation and wear resistance, extends service life, reduces building energy consumption, and improves production efficiency.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a multi-layer TPO waterproof coiled material and a preparation method thereof. Background Art
[0002] Traditional waterproof membranes are prone to aging and cracking during long-term use, resulting in reduced waterproofing effect. In order to improve the service life and waterproofing effect of waterproof membranes, researchers are constantly improving the materials and preparation processes of waterproof membranes. Multilayer TPO waterproof membranes have gradually become the mainstream product in the market due to their excellent physical properties, environmental performance and recyclability. However, the existing multilayer TPO waterproof membranes still need to be improved in terms of thermal insulation, self-healing and other aspects. Summary of the invention
[0003] In view of this, the present invention proposes a multi-layer TPO waterproof membrane and a preparation method thereof, aiming to solve the problem that traditional waterproof membranes in the current technology are prone to aging, cracking, etc. during long-term use, resulting in a decrease in waterproof effect.
[0004] On the one hand, the present invention provides a multi-layer TPO waterproof membrane, wherein the multi-layer TPO waterproof membrane comprises the following layers from top to bottom: The upper surface protective layer comprises the following components in parts by weight: 40-45 parts of ethylene-propylene rubber, 15-20 parts of polypropylene random copolymer, 0.8-1.5 parts of antioxidant, 0.5-0.9 parts of ultraviolet absorber, 7-15 parts of nanomaterial, 0.5-1 parts of organic tin catalyst and 0.5-1 parts of self-healing material; The reinforcing functional layer comprises the following components in parts by weight: 25 parts of ethylene-propylene rubber, 25 parts of polypropylene random copolymer, 5-10 parts of polyester fiber, 1-2 parts of low molecular weight polyethylene, 1-2 parts of toughening agent and 1-2 parts of plasticizer; The thermal insulation layer comprises the following components in parts by weight: 35-45 parts of foamed polypropylene, 20-25 parts of polyurethane, 10-15 parts of aluminum silicate fiber, 0.5-1 parts of barium carbonate and 5-10 parts of ceramic microbeads; Bottom protective layer, 40-50 parts of polyurethane, 20-30 parts of fluorinated polymer, 5-10 parts of aramid fiber and 5-10 parts of plasticizer; The self-healing material comprises microcapsules, wherein the microcapsules are filled with 3-5% by mass of trimethylolpropane trithiol, 3-5% by mass of diallyl ether and 1-2% by mass of isocyanate.
[0005] Optionally, the antioxidant comprises 15-20% by volume of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 25-30% of dilauryl thiodipropionate, 10-15% of tris[2,4-di-tert-butylphenyl]phosphite, and the remainder of toluene and impurities; The ultraviolet absorber is 0.3-0.5 parts by weight of UV-531 and 0.2-0.4 parts by weight of UV-327; The nano material is 5-10 parts by weight of nano titanium dioxide and 2-5 parts by weight of nano zinc oxide; The CAS number of the organotin catalyst is 77-58-7.
[0006] Optionally, the molecular weight of the low molecular weight polyethylene is 3000-10000; the toughening agent is SEBS; and the plasticizer is diisooctyl phthalate.
[0007] Optionally, the compression strength of the foamed polypropylene is 0.2-0.4 MPa; the Shore A hardness of the polyurethane is 40-55, and the tensile strength is 15-30 MPa; the particle size of the ceramic microbeads is 30-100 μm, and the aramid fiber is poly(p-phenylene terephthalamide) fiber.
[0008] Optionally, the ethylene content in the ethylene-propylene rubber is 45-70%; and the added amounts of propylene and ethylene in the polypropylene random copolymer are (7-9) g: (1-3) g.
[0009] On the other hand, the present invention also provides a method for preparing a multi-layer TPO waterproof membrane, the method comprising the following steps: The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively for preparation; The upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the ground protection layer are heated and then composited, and after the composite is completed, they are cooled and solidified for 30 minutes.
[0010] Optionally, the preparation of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer is specifically carried out by mixing the raw materials respectively: Upper surface protective layer material: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 40-45:15-20, and antioxidants, ultraviolet absorbers, nanomaterials, organic tin catalysts and self-healing materials are added for mixing, the mixing temperature is controlled to be 180° C., the mixing time is controlled to be 30 minutes, the mixing pressure is controlled to be 10 MPa, stirring is performed during the mixing process, and extrusion molding is performed after the raw materials are evenly mixed; Enhanced functional layer materials: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 25:25, and polyester fiber, low molecular weight polyethylene, toughening agent and plasticizer are added for mixing; the mixing temperature is controlled to be 190°C, the mixing time is controlled to be 45 minutes, the mixing pressure is controlled to be 8MPa, stirring is performed during the mixing process, and extrusion molding is performed after the raw materials are evenly mixed; Thermal insulation layer materials: Mix the foamed polypropylene and polyurethane in a weight ratio of 35-45:20-25, and add aluminum silicate fiber, barium carbonate and ceramic microbeads for mixing; during the mixing process, use a foaming machine for mixing, control the mixing temperature to 130°C, and the mixing time to 60 minutes. Control the mixing pressure to 5MPa, use a foaming machine for mixing, and control the foaming temperature to 120°C and the foaming pressure to 2MPa; Bottom protective layer material: The polyurethane and fluorinated polymer are mixed in a weight ratio of 40-50:20-30, and aramid fiber and plasticizer are added for mixing. The mixing temperature is controlled to be 165°C, the mixing time is 40 minutes, and the mixing pressure is controlled to be 6MPa. After the raw materials are evenly mixed, calendering is performed, and the calendering temperature is 160°C and the calendering pressure is 4MPa.
[0011] Optionally, pretreatment is required before the compounding, and the pretreatment includes drying at 80° C.-100° C. for more than 10 minutes.
[0012] Optionally, the composite process includes bonding at 120° C.-150° C. and 2-5 MPa for 5-10 minutes.
[0013] Optionally, during the mixing process of the upper surface protective layer, the antioxidant and the ultraviolet absorber need to be premixed at a temperature of 130° C.-150° C.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: the multilayer TPO waterproofing coiled material provided by the present invention effectively improves the comprehensive performance of the waterproofing coiled material by rationally configuring the components of each layer of materials. The upper surface protective layer adopts a self-healing material, so that the coiled material can repair itself when damaged, thereby extending the service life. The addition of antioxidants and ultraviolet absorbers improves the weather resistance of the upper surface protective layer, so that the coiled material can still maintain stable performance under harsh environments. The setting of the enhanced functional layer improves the mechanical properties of the waterproofing coiled material, making it more adaptable to various construction environments. The optimized design of the thermal insulation layer enables the coiled material to have good thermal insulation performance and reduce building energy consumption. The addition of the bottom protective layer effectively improves the wear resistance and puncture resistance of the waterproofing coiled material. The present invention also provides a preparation method of a multilayer TPO waterproofing coiled material, which ensures the quality and performance of the coiled material by strictly controlling the preparation process of each layer of materials. The optimization of the pretreatment and composite process makes the adhesion between the layers of the coiled material stronger and improves the overall performance. The present invention has the advantages of simple preparation process, high production efficiency, superior product performance, etc., and has good market application prospects. DETAILED DESCRIPTION
[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] This embodiment provides a multi-layer TPO waterproof membrane, which includes the following layers from top to bottom: The upper surface protective layer comprises the following components in parts by weight: 40-45 parts of ethylene-propylene rubber, 15-20 parts of polypropylene random copolymer, 0.8-1.5 parts of antioxidant, 0.5-0.9 parts of ultraviolet absorber, 7-15 parts of nanomaterial, 0.5-1 parts of organic tin catalyst and 0.5-1 parts of self-healing material; The reinforcing functional layer comprises the following components in parts by weight: 25 parts of ethylene-propylene rubber, 25 parts of polypropylene random copolymer, 5-10 parts of polyester fiber, 1-2 parts of low molecular weight polyethylene, 1-2 parts of toughening agent and 1-2 parts of plasticizer; The thermal insulation layer comprises the following components in parts by weight: 35-45 parts of foamed polypropylene, 20-25 parts of polyurethane, 10-15 parts of aluminum silicate fiber, 0.5-1 parts of barium carbonate and 5-10 parts of ceramic microbeads; The bottom protective layer comprises the following components in parts by weight: 40-50 parts of polyurethane, 20-30 parts of fluorinated polymer, 5-10 parts of aramid fiber and 5-10 parts of plasticizer; The self-healing material comprises microcapsules containing 3-5% by mass of trimethylolpropane trithiol, 3-5% by mass of diallyl ether and 1-2% by mass of isocyanate.
[0017] Optionally, the antioxidant comprises 15-20% by volume of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 25-30% of dilauryl thiodipropionate, 10-15% of tris[2,4-di-tert-butylphenyl]phosphite, and the remainder of toluene and impurities; The ultraviolet absorber is 0.3-0.5 parts by weight of UV-531 and 0.2-0.4 parts by weight of UV-327; The nano material is 5-10 parts by weight of nano titanium dioxide and 2-5 parts by weight of nano zinc oxide; The CAS number of the organotin catalyst is 77-58-7.
[0018] Optionally, the molecular weight of the low molecular weight polyethylene is 3000-10000; the toughening agent is SEBS; and the plasticizer is diisooctyl phthalate.
[0019] Optionally, the compression strength of the foamed polypropylene is 0.2-0.4 MPa; the Shore A hardness of the polyurethane is 40-55, and the tensile strength is 15-30 MPa; the particle size of the ceramic microbeads is 30-100 μm, and the aramid fiber is poly(p-phenylene terephthalamide) fiber.
[0020] Optionally, the ethylene content in the ethylene-propylene rubber is 45-70%; and the added amounts of propylene and ethylene in the polypropylene random copolymer are (7-9) g: (1-3) g.
[0021] The present invention also provides a method for preparing a multi-layer TPO waterproof membrane, comprising the following steps: The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively to prepare; The upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the ground protection layer are composited after being heated, and after the composite is completed, they are cooled and solidified for 30 minutes.
[0022] Optionally, the raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed separately for preparation, specifically including: Upper surface protective layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of (40-45): (15-20), and an antioxidant, an ultraviolet absorber, a nanomaterial, an organic tin catalyst and a self-healing material are added and mixed again; during the mixing again, the mixing temperature is controlled to be 180° C., the mixing time is 30 min, and the mixing pressure is 10 MPa. After the mixing again is completed, extrusion molding is performed; Enhanced feature layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 25:25, and polyester fiber, low molecular weight polyethylene, toughening agent and plasticizer are added for secondary mixing; the mixing temperature in the secondary mixing is controlled to be 190° C., the mixing time is controlled to be 45 min, the mixing pressure is controlled to be 8 MPa, and the secondary mixing is followed by extrusion molding; Thermal insulation layer: The foamed polypropylene and polyurethane are mixed in a weight ratio of 35-45:20-25, and aluminum silicate fiber, barium carbonate and ceramic microbeads are added for mixing; during the mixing process of the thermal insulation layer, a foaming machine is used for mixing, and the mixing temperature is controlled to be 130° C., the mixing time is 60 minutes, and the mixing pressure is 5 MPa; Bottom protective layer: The polyurethane and the fluorinated polymer are mixed in a weight ratio of 40-50:20-30, and aramid fiber and a plasticizer are added and mixed; during the mixing process of the bottom protective layer, the mixing temperature is controlled to be 165°C, the mixing time is 40 minutes, and the mixing pressure is controlled to be 6MPa. After the mixing is completed, the calendering is performed, and the calendering temperature is 160°C and the calendering pressure is 4MPa.
[0023] Optionally, also include: The pretreatment is performed before the compounding, and the pretreatment includes drying at 80° C.-100° C. for 10 minutes.
[0024] Optionally, the composite process is to perform bonding for 5-10 minutes at 120-150° C. and 2-5 MPa.
[0025] Optionally, before the mixing process of the upper surface protective layer, the antioxidant and the ultraviolet absorber are pre-mixed at a temperature of 130-150°C.
[0026] The performance of the waterproof membrane of the present invention is tested by the following examples: Example 1
[0027] The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively to prepare; Upper surface protective layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 40:15, and 0.8 parts of antioxidant, 0.5 parts of ultraviolet absorber, 7 parts of nanomaterial, 0.5 parts of organic tin catalyst and 0.5 parts of self-healing material are added and mixed again; during the mixing again, the mixing temperature is controlled to be 180° C., the mixing time is 30 minutes, and the mixing pressure is 10 MPa. After the mixing again is completed, extrusion molding is performed; Enhanced feature layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 25:25, and 5 parts of polyester fiber, 1 part of low molecular weight polyethylene, 1 part of toughening agent and 1 part of plasticizer are added for secondary mixing; the mixing temperature in the secondary mixing is controlled to be 190° C., the mixing time is 45 min, the mixing pressure is controlled to be 8 MPa, and the secondary mixing is followed by extrusion molding; Thermal insulation layer: The foamed polypropylene and polyurethane are mixed in a weight ratio of 35:20, and 10 parts of aluminum silicate fiber, 0.5 parts of barium carbonate and 5 parts of ceramic microbeads are added and mixed; during the mixing process of the thermal insulation layer, a foaming machine is used for mixing, and the mixing temperature is controlled to be 130° C., the mixing time is 60 minutes, and the mixing pressure is 5 MPa; Bottom protective layer: Polyurethane and fluorinated polymer are mixed in a weight ratio of 40:20, and 5 parts of aramid fiber and 5 parts of plasticizer are added and mixed; during the mixing process of the bottom protective layer, the mixing temperature is controlled to be 165°C, the mixing time is 40 minutes, and the mixing pressure is controlled to be 6MPa. After the mixing is completed, calendering is performed, and the calendering temperature is 160°C and the calendering pressure is 4MPa.
[0028] The upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the ground protection layer are heated and bonded at 150° C. and 5 MPa for compounding. A pretreatment is performed before the compounding is completed. The pretreatment includes drying at 80° C. for 10 minutes, and then cooling and curing for 30 minutes to obtain a waterproof membrane. Example 2
[0029] The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively to prepare; Upper surface protective layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 45:20, and 1.5 parts of antioxidant, 0.9 parts of ultraviolet absorber, 15 parts of nanomaterial, 1 part of organic tin catalyst and 1 part of self-healing material are added and mixed again; during the mixing again, the mixing temperature is controlled to be 180° C., the mixing time is 30 minutes, and the mixing pressure is 10 MPa. After the mixing again is completed, extrusion molding is performed; Enhanced feature layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 25:25, and 10 parts of polyester fiber, 2 parts of low molecular weight polyethylene, 2 parts of toughening agent and 2 parts of plasticizer are added for secondary mixing; the mixing temperature in the secondary mixing is controlled to be 190° C., the mixing time is 45 min, the mixing pressure is controlled to be 8 MPa, and the secondary mixing is followed by extrusion molding; Thermal insulation layer: The foamed polypropylene and polyurethane are mixed in a weight ratio of 45:25, and 15 parts of aluminum silicate fiber, 1 part of barium carbonate and 10 parts of ceramic microbeads are added and mixed; during the mixing process of the thermal insulation layer, a foaming machine is used for mixing, and the mixing temperature is controlled to be 130° C., the mixing time is 60 minutes, and the mixing pressure is 5 MPa; Bottom protective layer: The polyurethane and the fluorinated polymer are mixed in a weight ratio of 50:30, and 10 parts of aramid fiber and 10 parts of plasticizer are added and mixed; during the mixing process of the bottom protective layer, the mixing temperature is controlled to be 165°C, the mixing time is 40 minutes, and the mixing pressure is controlled to be 6MPa. After the mixing is completed, calendering is performed, and the calendering temperature is 160°C and the calendering pressure is 4MPa.
[0030] The upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the ground protection layer are heated and bonded at 150° C. and 5 MPa for compounding. A pretreatment is performed before the compounding is completed. The pretreatment includes drying at 80° C. for 10 minutes, and then cooling and curing for 30 minutes to obtain a waterproof membrane. Example 3
[0031] The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively to prepare; Upper surface protective layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 40:20, and 0.9 parts of antioxidant, 0.7 parts of ultraviolet absorber, 9 parts of nanomaterial, 0.8 parts of organic tin catalyst and 0.8 parts of self-healing material are added and mixed again; during the mixing again, the mixing temperature is controlled to be 180° C., the mixing time is 30 min, and the mixing pressure is 10 MPa. After the mixing again, extrusion molding is performed; Enhanced feature layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 25:25, and 7 parts of polyester fiber, 1.5 parts of low molecular weight polyethylene, 1.5 parts of toughening agent and 1.5 parts of plasticizer are added for secondary mixing; the mixing temperature is controlled to be 190° C., the mixing time is 45 minutes, and the mixing pressure is controlled to be 8 MPa during the secondary mixing, and extrusion molding is performed after the secondary mixing; Thermal insulation layer: The foamed polypropylene and polyurethane are mixed in a weight ratio of 45:20, and 13 parts of aluminum silicate fiber, 0.7 parts of barium carbonate and 8 parts of ceramic microbeads are added for mixing; during the mixing process of the thermal insulation layer, a foaming machine is used for mixing, and the mixing temperature is controlled to be 130° C., the mixing time is 60 minutes, and the mixing pressure is 5 MPa; Bottom protective layer: The polyurethane and the fluorinated polymer are mixed in a weight ratio of 40:30, and 7 parts of aramid fiber and 8 parts of plasticizer are added and mixed; during the mixing process of the bottom protective layer, the mixing temperature is controlled to be 165°C, the mixing time is 40 minutes, and the mixing pressure is controlled to be 6MPa. After the mixing is completed, calendering is performed, and the calendering temperature is 160°C and the calendering pressure is 4MPa.
[0032] The upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the ground protection layer are heated and bonded at 150° C. and 5 MPa for compounding. A pretreatment is performed before the compounding is completed. The pretreatment includes drying at 80° C. for 10 minutes, and then cooling and curing for 30 minutes to obtain a waterproof membrane.
[0033] Comparative Example 1 No self-healing material is added to the upper surface protective layer, and the remaining steps are the same as those in the embodiment.
[0034] Comparative Example 2 No ultraviolet absorber and antioxidant are added to the upper surface protective layer, and the remaining steps are the same as those in the embodiment.
[0035] The waterproof membranes obtained in Examples 1-3 and Comparative Examples 1-2 were subjected to performance testing, and the test data are shown in Table 1.
[0036] Table 1 Test data table
[0037] The water impermeability is measured at 0.1MPa. It can be seen from the above data that the self-healing material greatly improves the tensile strength recovery rate of the waterproof coiled material by comparing the data of the embodiment of the present application with that of comparative example 1. It can be seen from the comparison of the data of the embodiment of the present application with that of comparative example 2 that the antioxidant and ultraviolet absorber greatly enhance the tensile strength retention rate of the waterproof coiled material after ultraviolet irradiation. It can be seen that the upper surface protective layer adopts the self-healing material, so that the coiled material can repair itself when damaged and extend its service life. The addition of antioxidants and ultraviolet absorbers improves the weather resistance of the upper surface protective layer, so that the coiled material can still maintain stable performance in harsh environments.
[0038] In summary, the multilayer TPO waterproofing membrane provided by the present invention effectively improves the comprehensive performance of the waterproofing membrane by rationally configuring the components of each layer of materials. The upper surface protective layer adopts self-healing material, so that the membrane can repair itself when damaged, thereby extending the service life. The addition of antioxidants and ultraviolet absorbers improves the weather resistance of the upper surface protective layer, so that the membrane can still maintain stable performance under harsh environments. The setting of the enhanced functional layer improves the mechanical properties of the waterproofing membrane, making it more adaptable to various construction environments. The optimized design of the thermal insulation layer enables the membrane to have good thermal insulation performance and reduce building energy consumption. The addition of the bottom protective layer effectively improves the wear resistance and puncture resistance of the waterproofing membrane. The present invention also provides a preparation method for a multilayer TPO waterproofing membrane, which ensures the quality and performance of the membrane by strictly controlling the preparation process of each layer of materials. The optimization of the pretreatment and composite process makes the adhesion between the layers of the membrane stronger and improves the overall performance. The present invention has the advantages of simple preparation process, high production efficiency, superior product performance, etc., and has good market application prospects.
[0039] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A multi-layer TPO waterproof membrane, It is characterized in that The multi-layer TPO waterproof membrane includes the following layers from top to bottom: The upper surface protective layer comprises the following components in parts by weight: 40-45 parts of ethylene-propylene rubber, 15-20 parts of polypropylene random copolymer, 0.8-1.5 parts of antioxidant, 0.5-0.9 parts of ultraviolet absorber, 7-15 parts of nanomaterial, 0.5-1 parts of organic tin catalyst and 0.5-1 parts of self-healing material; The reinforcing functional layer comprises the following components in parts by weight: 25 parts of ethylene-propylene rubber, 25 parts of polypropylene random copolymer, 5-10 parts of polyester fiber, 1-2 parts of low molecular weight polyethylene, 1-2 parts of toughening agent and 1-2 parts of plasticizer; The thermal insulation layer comprises the following components in parts by weight: 35-45 parts of foamed polypropylene, 20-25 parts of polyurethane, 10-15 parts of aluminum silicate fiber, 0.5-1 parts of barium carbonate and 5-10 parts of ceramic microbeads; The bottom protective layer comprises the following components in parts by weight: 40-50 parts of polyurethane, 20-30 parts of fluorinated polymer, 5-10 parts of aramid fiber and 5-10 parts of plasticizer; The self-healing material comprises microcapsules, wherein the microcapsules are filled with 3-5% by mass of trimethylolpropane trithiol, 3-5% by mass of diallyl ether and 1-2% by mass of isocyanate.
2. The multi-layer TPO waterproof membrane according to claim 1, It is characterized in that The antioxidant comprises 15-20% by volume of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 25-30% of dilauryl thiodipropionate, 10-15% of tris[2,4-di-tert-butylphenyl]phosphite, and the remainder of toluene and impurities; The ultraviolet absorber is 0.3-0.5 parts by weight of UV-531 and 0.2-0.4 parts by weight of UV-327; The nano material is 5-10 parts by weight of nano titanium dioxide and 2-5 parts by weight of nano zinc oxide; The CAS number of the organotin catalyst is 77-58-7.
3. The multi-layer TPO waterproof membrane according to claim 1, It is characterized in that The molecular weight of the low molecular weight polyethylene is 3000-10000; the toughening agent is SEBS; and the plasticizer is diisooctyl phthalate.
4. The multi-layer TPO waterproof membrane according to claim 1, It is characterized in that The compression strength of the foamed polypropylene is 0.2-0.4 MPa; the Shore A hardness of the polyurethane is 40-55, and the tensile strength is 15-30 MPa; the particle size of the ceramic microbeads is 30-100 μm, and the aramid fiber is poly(p-phenylene terephthalamide) fiber.
5. The multi-layer TPO waterproof membrane according to claim 1, It is characterized in that The ethylene content of the ethylene-propylene rubber is 45-70%; the added amount of propylene:ethylene in the polypropylene random copolymer is (7-9) g: (1-3) g.
6. A method for preparing the multilayer TPO waterproof membrane according to any one of claims 1 to 5, It is characterized in that The following steps are involved: The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively to prepare; The upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the ground protection layer are composited after being heated, and after the composite is completed, they are cooled and solidified for 30 minutes.
7. The method for preparing the multi-layer TPO waterproof membrane according to claim 6, It is characterized in that The raw materials of the upper surface protection layer, the enhanced functional layer, the thermal insulation layer and the bottom surface protection layer are mixed respectively and prepared, specifically including: Upper surface protective layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of (40-45): (15-20), and an antioxidant, an ultraviolet absorber, a nanomaterial, an organic tin catalyst and a self-healing material are added and mixed again; during the mixing again, the mixing temperature is controlled to be 180° C., the mixing time is 30 min, and the mixing pressure is 10 MPa. After the mixing again is completed, extrusion molding is performed; Enhanced feature layer: Ethylene-propylene rubber and polypropylene random copolymer are mixed in a weight ratio of 25:25, and polyester fiber, low molecular weight polyethylene, toughening agent and plasticizer are added for secondary mixing; the mixing temperature in the secondary mixing is controlled to be 190° C., the mixing time is controlled to be 45 min, the mixing pressure is controlled to be 8 MPa, and the secondary mixing is followed by extrusion molding; Thermal insulation layer: The foamed polypropylene and polyurethane are mixed in a weight ratio of 35-45:20-25, and aluminum silicate fiber, barium carbonate and ceramic microbeads are added for mixing; during the mixing process of the thermal insulation layer, a foaming machine is used for mixing, and the mixing temperature is controlled to be 130° C., the mixing time is 60 minutes, and the mixing pressure is 5 MPa; Bottom protective layer: The polyurethane and the fluorinated polymer are mixed in a weight ratio of 40-50:20-30, and aramid fiber and a plasticizer are added and mixed; during the mixing process of the bottom protective layer, the mixing temperature is controlled to be 165°C, the mixing time is 40 minutes, and the mixing pressure is controlled to be 6MPa. After the mixing is completed, the calendering is performed, and the calendering temperature is 160°C and the calendering pressure is 4MPa.
8. The method for preparing the multi-layer TPO waterproof membrane according to claim 6, It is characterized in that Also includes: The pretreatment is performed before the compounding, and the pretreatment includes drying at 80° C.-100° C. for 10 minutes.
9. The method for preparing the multi-layer TPO waterproof membrane according to claim 6, It is characterized in that The composite process is to bond for 5-10 minutes at 120-150° C. and 2-5 MPa.
10. The method for preparing the multi-layer TPO waterproof membrane according to claim 6, It is characterized in that Before the mixing process of the upper surface protective layer, the antioxidant and the ultraviolet absorber are pre-mixed at a temperature of 130-150°C.
Citation Information
Patent Citations
Self-repairing polymer waterproof coiled material and preparation method thereof
CN111546732A
Environment-friendly heat-preservation waterproof roll for roof and preparation method thereof
CN111718669A
Multilayer composite waterproof coiled material and preparation method thereof
CN112900651A
High-strength and deformation-resistant TPO waterproof coiled material and preparation method thereof
CN114274620A
Pre-paved TPO self-adhesive waterproof coiled material and preparation method thereof
CN116218395A
Cited By
A high-reflectivity tpo waterproofing membrane for photovoltaics and method of making the same