Stone plastic floor and preparation method thereof

By using a hot press composite process of PBAT substrate layer, TPU color film layer and TPU wear-resistant layer in stone plastic flooring, combined with degradable materials and natural stone powder, the poor performance and insufficient environmental protection performance in the preparation process of stone plastic flooring are solved. Problem, improves service life and environmental protection, and effectively kills bacteria.

CN119058211AInactive Publication Date: 2024-12-03JIANGSU KA LAI NEW DECORATIVE MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411336112.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The lack of precise control during the preparation of existing stone plastic floors, resulting in poor performance, short service life, poor environmental protection performance and inability to kill bacteria.

Method used

The PBAT substrate layer, TPU color film layer and TPU wear-resistant layer are combined through a hot press composite process to accurately control the temperature, pressure, time and speed, and use degradable materials and natural stone powder to add antibacterial agents to improve performance and environmental protection. sex.

Benefits of technology

It improves the performance and service life of stone plastic floors, enhances overall stability and anti-permeability, and effectively kills bacteria through antibacterial agents, providing a healthier use environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119058211A_ABST
    Figure CN119058211A_ABST
Patent Text Reader

Abstract

The invention discloses a stone-plastic floor and a preparation method thereof, and relates to the technical field of stone-plastic floor preparation, the stone-plastic floor comprises a PBAT base material layer, a TPU color film layer and a TPU wear-resistant layer, and the PBAT base material layer, the TPU color film layer and the TPU wear-resistant layer are compounded through a hot-pressing compounding process to form the complete stone-plastic floor. Through the arrangement of the PBAT base material layer, the TPU color film layer and the TPU wear-resistant layer, the temperature, the pressure, the rotating speed and the time in the preparation process are accurately controlled, the performance of the prepared stone-plastic floor is improved, the situation that the temperature, the pressure, the rotating speed and the time do not reach the standard or exceed the threshold value, and consequently raw materials are not fully mixed or react excessively is avoided, and the service life of the stone-plastic floor is prolonged. Therefore, the performance of the prepared stone-plastic floor is relatively poor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stone plastic floor preparation, in particular to a stone plastic floor and a preparation method thereof. Background Art

[0002] Stone plastic flooring is also called stone plastic floor tiles. Its formal name should be "PVC sheet flooring". It is a new type of floor decoration material developed through high-quality and high-tech research. It uses stone powder to form a solid base layer with high density and high fiber mesh structure. The surface is covered with a super wear-resistant polymer PVC wear-resistant layer. It is processed through hundreds of processes. Stone plastic flooring is widely used in homes, shopping malls, offices, schools, hospitals and other places.

[0003] The existing defects are:

[0004] 1. Patent document US09186869B2 discloses composite floor support and thermoplastic coating, but the temperature, pressure, speed and time in the preparation process are not accurately controlled in the above document. In the preparation process, insufficient mixing or over-reaction of raw materials is likely to occur, resulting in technical problems such as poor performance of stone plastic floor;

[0005] 2. Patent document US20160229161A1 discloses wood plastic PVC flooring, but the above document uses glue to stick the various layers of the floor, which easily causes the technical problem of a low service life of the stone plastic flooring;

[0006] 3. Patent document KR101583521B1 discloses a PVC floor coating method, but the raw materials used in the above document are not degradable, and the raw materials used contain heavy metal materials and formaldehyde, which has a technical problem of poor environmental performance;

[0007] 4. Patent document CN106587720B discloses a stone plastic floor and a preparation method thereof. However, the stone plastic floor prepared in the above document cannot achieve the technical problem of killing bacteria and inhibiting bacterial reproduction. Summary of the invention

[0008] The object of the present invention is to provide a stone plastic floor and a preparation method thereof to solve the technical problems raised in the above background technology.

[0009] To achieve the above object, the present invention provides the following technical solutions: a method for preparing a stone plastic floor, comprising a PBAT substrate layer, a TPU color film layer and a TPU wear-resistant layer, wherein the PBAT substrate layer, the TPU color film layer and the TPU wear-resistant layer are compounded by a hot pressing compounding process to form a complete stone plastic floor;

[0010] The composition and weight of the raw materials of the PBAT substrate layer of the stone plastic floor are: 130-150 parts of PBAT resin, 240-280 parts of calcium filler, 3-8 parts of stabilizer, 2-5 parts of antibacterial agent, 1-3 parts of plasticizer, 10-15 parts of polylactic acid fiber and 5-8 parts of dispersant;

[0011] The preparation steps of the PBAT substrate layer of the stone plastic floor are as follows:

[0012] Step S1, placing the required raw materials; PBAT resin, calcium filler, stabilizer, antibacterial agent, plasticizer, polylactic acid fiber and dispersant into a mixing tank in sequence, and mixing and stirring under precisely controlled temperature, pressure, time and speed;

[0013] Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the PBAT substrate layer of the stone plastic floor.

[0014] Preferably, the composition and weight of the raw materials of the TPU color film layer of the stone plastic floor are: 80-120 parts of TPU granules, 1-5 parts of colorant and 5-8 parts of dispersant;

[0015] The steps for preparing the TPU color film layer of the stone plastic floor are as follows:

[0016] Step S1, placing TPU pellets, colorant and dispersant into a mixing tank in sequence, and mixing and stirring under precisely controlled temperature, pressure, time and speed;

[0017] Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the TPU color film layer of the stone plastic floor.

[0018] Preferably, the TPU wear-resistant layer of the stone plastic floor has the following raw material composition and weight parts: 80-120 parts of TPU granules and 20-35 parts of ABS granules;

[0019] The steps for preparing the TPU wear-resistant layer of the stone plastic floor are as follows:

[0020] Step S1, placing TPU pellets and ABS pellets into a mixing tank in sequence, and mixing and stirring them under precisely controlled temperature, pressure, time and speed;

[0021] Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the TPU wear-resistant layer of the stone plastic floor.

[0022] Preferably, the hot pressing temperature of the hot pressing composite process is 130° C.-180° C., the hot pressing pressure is 10 MPa-20 MPa, and the hot pressing time is 1 h-2 h.

[0023] Preferably, the calcium filler is pebble powder, the pebble powder is 300-800 mesh, the stabilizer is one of carbodiimide type anti-hydrolysis stabilizer, isocyanate and epoxy, the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent, the plasticizer regulator is one of tributyl citrate or trioctyl citrate, and the dispersant is one of starch or cellulose.

[0024] Preferably, in step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 800 r / min-1100 r / min, the mixing temperature is 110° C.-140° C., and the mixing time is 2 h-4 h;

[0025] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 140° C.-170° C., the mold temperature is 180° C.-220° C., the main engine speed is 10 r / min-20 r / min, and the feed speed is 15 r / min-25 r / min.

[0026] Preferably, the colorant is a natural pigment or a bio-based pigment, and the dispersant is a starch or a cellulose.

[0027] Preferably, in step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 800r / min-1100r / min, the mixing temperature is 80°C-95°C, and the mixing time is 40min-80min;

[0028] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 120°C-135°C, the mold temperature is 150°C-170°C, the main machine speed is 10r / min-20r / min, and the feeding speed is 15r / min-25r / min.

[0029] Preferably, in step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 800 r / min-1100 r / min, the mixing temperature is 90° C.-115° C., and the mixing time is 20 min-60 min;

[0030] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 140°C-175°C, the mold temperature is 150°C-180°C, the main engine speed is 10r / min-20r / min, and the feeding speed is 15r / min-25r / min.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention accurately controls the temperature, pressure, rotation speed and time in the preparation process by setting the PBAT substrate layer, the TPU color film layer and the TPU wear-resistant layer, which is beneficial to improving the performance of the prepared stone plastic floor, and avoiding the situation where the temperature, pressure, rotation speed and time do not meet the standards or exceed the threshold, resulting in insufficient mixing or over-reaction of the raw materials, thereby causing the prepared stone plastic floor to have poor performance;

[0033] 2. The present invention adopts a hot-pressing composite process to form a stone-plastic floor, which can make each layer closely combined, thereby improving the overall stability and anti-permeability effect of the floor, thereby increasing the service life of the stone-plastic floor;

[0034] 3. The PBAT resin, stabilizer, antibacterial agent, plasticizer and dispersant used in the present invention are all biodegradable materials, and the pebble powder in the natural stone powder used as the calcium filler is reused, so the required materials do not contain heavy metal materials and formaldehyde, thereby improving the environmental friendliness of the preparation of the stone plastic floor;

[0035] 4. The present invention can effectively kill bacteria and inhibit bacterial reproduction by adding antibacterial agents, thereby providing a healthier use environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the workflow of the present invention;

[0037] Figure 2 It is a schematic diagram of the structure of the stone plastic floor of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1: Please refer to Figure 1 , an embodiment of the present invention: a method for preparing a stone plastic floor, comprising a PBAT substrate layer, a TPU color film layer and a TPU wear-resistant layer, the PBAT substrate layer, the TPU color film layer and the TPU wear-resistant layer are compounded by a hot pressing compounding process to form a complete stone plastic floor;

[0040] The composition and weight of the raw materials of the PBAT substrate layer of the stone plastic floor are: 140 parts of PBAT resin, 260 parts of calcium filler, 5 parts of stabilizer, 3 parts of antibacterial agent, 2 parts of plasticizer, 12 parts of polylactic acid fiber and 6.5 parts of dispersant;

[0041] The preparation steps of the PBAT substrate layer of the stone plastic floor are as follows:

[0042] Step S1, placing the required raw materials; PBAT resin, calcium filler, stabilizer, antibacterial agent, plasticizer, polylactic acid fiber and dispersant into a mixing tank in sequence, and mixing and stirring under precisely controlled temperature, pressure, time and speed;

[0043] Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the PBAT substrate layer of the stone plastic floor;

[0044] The composition and weight of the raw materials of the TPU color film layer of the stone plastic floor are: 100 parts of TPU granules, 3 parts of colorant and 6.5 parts of dispersant;

[0045] The preparation steps of the TPU color film layer of the stone plastic floor are as follows:

[0046] Step S1, placing TPU pellets, colorant and dispersant into a mixing tank in sequence, and mixing and stirring under precisely controlled temperature, pressure, time and speed;

[0047] Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the TPU color film layer of the stone plastic floor;

[0048] The TPU wear-resistant layer of the stone plastic floor has the following raw materials in terms of composition and weight: 100 parts of TPU granules and 30 parts of ABS granules;

[0049] The preparation steps of the TPU wear-resistant layer of the stone plastic floor are as follows:

[0050] Step S1, placing TPU pellets and ABS pellets into a mixing tank in sequence, and mixing and stirring them under precisely controlled temperature, pressure, time and speed;

[0051] Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the TPU wear-resistant layer of the stone plastic floor;

[0052] The hot pressing temperature of the hot pressing composite process is 160°C, the hot pressing pressure is 15MPa, and the hot pressing time is 1.5h;

[0053] The calcium filler is pebble powder with a mesh size of 500; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0054] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 950 r / min, the mixing temperature is 125° C., and the mixing time is 3 h;

[0055] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 155° C., the die temperature is 200° C., the main engine speed is 15 r / min, and the feed speed is 20 r / min;

[0056] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0057] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 950 r / min, the mixing temperature is 90° C., and the mixing time is 60 min;

[0058] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 130° C., the mold temperature is 160° C., the main machine speed is 15 r / min, and the feed speed is 20 r / min;

[0059] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 950 r / min, the mixing temperature is 100° C., and the mixing time is 40 min;

[0060] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 155° C., the mold temperature is 165° C., the main engine speed is 15 r / min, and the feed speed is 20 r / min.

[0061] Example 2: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as that of embodiment 1, except that: the hot pressing temperature of the hot pressing composite process is 130°C, the hot pressing pressure is 10MPaMPa, and the hot pressing time is 1h;

[0062] The calcium filler is pebble powder with a mesh size of 300; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0063] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 110° C., and the mixing time is 2 h;

[0064] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 140° C., the die temperature is 180° C., the main engine speed is 10 r / min, and the feed speed is 15 r / min;

[0065] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0066] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 80° C., and the mixing time is 40 min;

[0067] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 120°C, the mold temperature is 150°C, the main machine speed is 10r / min, and the feeding speed is 15r / min;

[0068] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 90° C., and the mixing time is 20 min;

[0069] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 140° C., the mold temperature is 150° C., the main machine speed is 10 r / min, and the feed speed is 15 r / min.

[0070] Example 3: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as that of embodiment 1, except that: the hot pressing temperature of the hot pressing composite process is 180°C, the hot pressing pressure is 20MPa, and the hot pressing time is 2h;

[0071] The calcium filler is pebble powder with a mesh size of 800; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0072] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 140° C., and the mixing time is 4 h;

[0073] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 170° C., the die temperature is 220° C., the main engine speed is 20 r / min, and the feed speed is 25 r / min;

[0074] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0075] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 95° C., and the mixing time is 80 min;

[0076] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 135°C, the mold temperature is 170°C, the main machine speed is 20r / min, and the feed speed is 25r / min;

[0077] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 115° C., and the mixing time is 60 min;

[0078] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 175° C., the mold temperature is 180° C., the main engine speed is 20 r / min, and the feed speed is 25 r / min.

[0079] Example 4: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation is the same as that of embodiment 1, except that: the hot pressing temperature of the hot pressing composite process is 130°C, the hot pressing pressure is 20MPa, and the hot pressing time is 2h;

[0080] The calcium filler is pebble powder with a mesh size of 300; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0081] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 140° C., and the mixing time is 4 h;

[0082] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 140° C., the die temperature is 180° C., the main engine speed is 20 r / min, and the feed speed is 25 r / min;

[0083] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0084] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 80° C., and the mixing time is 80 min;

[0085] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 120°C, the mold temperature is 150°C, the main machine speed is 20r / min, and the feed speed is 25r / min;

[0086] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 90° C., and the mixing time is 60 min;

[0087] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 140° C., the mold temperature is 150° C., the main machine speed is 20 r / min, and the feed speed is 25 r / min.

[0088] Example 5: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as that of embodiment 1, except that: the hot pressing temperature of the hot pressing composite process is 180°C, the hot pressing pressure is 10MPa, and the hot pressing time is 1h;

[0089] The calcium filler is pebble powder with a mesh size of 500; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0090] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 140° C., and the mixing time is 2 h;

[0091] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 170° C., the die temperature is 220° C., the main engine speed is 10 r / min, and the feed speed is 15 r / min;

[0092] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0093] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 95° C., and the mixing time is 40 min;

[0094] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 135°C, the mold temperature is 170°C, the main machine speed is 10r / min, and the feeding speed is 15r / min;

[0095] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 800 r / min, the mixing temperature is 115° C., and the mixing time is 20 min;

[0096] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 175° C., the mold temperature is 180° C., the main machine speed is 10 r / min, and the feed speed is 15 r / min.

[0097] Example 6: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation is the same as that of embodiment 1, except that: the hot pressing temperature of the hot pressing composite process is 150°C, the hot pressing pressure is 20MPa, and the hot pressing time is 1.5h;

[0098] The calcium filler is pebble powder with a mesh size of 300; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0099] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 130° C., and the mixing time is 3 h;

[0100] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 165° C., the die temperature is 220° C., the main engine speed is 20 r / min, and the feed speed is 19 r / min;

[0101] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0102] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 1100 r / min, the mixing temperature is 85° C., and the mixing time is 70 min;

[0103] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 120°C, the mold temperature is 170°C, the main machine speed is 15r / min, and the feeding speed is 25r / min;

[0104] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 1000 r / min, the mixing temperature is 110° C., and the mixing time is 60 min;

[0105] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 165° C., the mold temperature is 160° C., the main machine speed is 10 r / min, and the feed speed is 25 r / min.

[0106] Comparative Example 1: An embodiment is provided: The specific implementation method is the same as Example 1, except that: the composition and weight proportions of the raw materials of the stone plastic floor substrate layer are: 140 parts of PVC resin, 260 parts of calcium filler, 5 parts of stabilizer, 3 parts of antibacterial agent, 2 parts of plasticizer regulator and 6.5 parts of dispersant.

[0107] Comparative Example 2: An embodiment is provided: The specific implementation method is the same as Example 1, except that: the composition and weight of the raw materials of the stone plastic floor substrate layer are: 140 parts of PVC resin, 260 parts of calcium filler, 5 parts of stabilizer, 3 parts of antibacterial agent, 2 parts of plasticizer regulator, 12 parts of glass fiber and 6.5 parts of dispersant.

[0108] Comparative Example 3: An embodiment is provided: The specific implementation method is the same as Example 1, except that: the composition and weight of the raw materials of the stone plastic floor substrate layer are: 140 parts of PVC resin, 260 parts of calcium filler, 5 parts of stabilizer, 2 parts of plasticizer regulator, 12 parts of glass fiber and 6.5 parts of dispersant.

[0109] Comparative Example 4: An embodiment is provided: The specific implementation method is the same as that of Example 1, except that: the hot pressing temperature of the hot pressing composite process is 120°C, the hot pressing pressure is 8MPa, and the hot pressing time is 0.9h;

[0110] The calcium filler is pebble powder with a mesh size of 200; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0111] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 700 r / min, the mixing temperature is 100° C., and the mixing time is 1.5 h;

[0112] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 130° C., the die temperature is 170° C., the main engine speed is 8 r / min, and the feed speed is 12 r / min;

[0113] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0114] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 700 r / min, the mixing temperature is 70° C., and the mixing time is 30 min;

[0115] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 110° C., the mold temperature is 140° C., the main machine speed is 8 r / min, and the feed speed is 15 r / min;

[0116] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 700 r / min, the mixing temperature is 80° C., and the mixing time is 15 min;

[0117] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 130° C., the mold temperature is 140° C., the main machine speed is 8 r / min, and the feed speed is 14 r / min.

[0118] Comparative Example 5: An embodiment is provided: The specific implementation is the same as that of Example 1, except that: the hot pressing temperature of the hot pressing composite process is 200°C, the hot pressing pressure is 22MPa, and the hot pressing time is 2.5h;

[0119] The calcium filler is pebble powder with a mesh size of 900; the stabilizer is one of carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of silver ion antibacterial agent, quaternary ammonium salt antibacterial agent or nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose;

[0120] In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 1200 r / min, the mixing temperature is 1500° C., and the mixing time is 4.5 h;

[0121] In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 180° C., the die temperature is 230° C., the main engine speed is 24 r / min, and the feed speed is 26 r / min;

[0122] The colorant is one of natural pigment or bio-based pigment, and the dispersant is one of starch or cellulose;

[0123] In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 1200 r / min, the mixing temperature is 100° C., and the mixing time is 90 min;

[0124] In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 140°C, the mold temperature is 180°C, the main machine speed is 22r / min, and the feed speed is 28r / min;

[0125] In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 1200 r / min, the mixing temperature is 120° C., and the mixing time is 70 min;

[0126] In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 180° C., the mold temperature is 200° C., the main machine speed is 22 r / min, and the feed speed is 28 r / min.

[0127] Comparative Example 6: An embodiment is provided: The specific implementation method is the same as that of Example 1, except that the PBAT substrate layer, the TPU color film layer and the TPU wear-resistant layer are bonded together by an adhesive.

[0128] Test result 1: The stone plastic floor prepared in Examples 1-6 and Comparative Examples 1-6 was used for performance testing:

[0129]

[0130] Furthermore, by setting the PBAT substrate layer, the TPU color film layer and the TPU wear-resistant layer, the temperature, pressure, rotation speed and time in the preparation process are precisely controlled, which is beneficial to improving the performance of the prepared stone plastic floor, and avoiding the situation where the temperature, pressure, rotation speed and time do not meet the standards or exceed the threshold, resulting in insufficient mixing or over-reaction of the raw materials, thereby causing the prepared stone plastic floor to have poor performance;

[0131] The stone plastic floor formed by the hot pressing composite process can make each layer closely combined, thereby improving the overall stability and anti-permeability effect of the floor, thereby increasing the service life of the stone plastic floor;

[0132] The PBAT resin, stabilizer, antibacterial agent, plasticizer and dispersant used are all biodegradable materials, and the calcium filler uses the pebble powder in the natural stone powder, which is reused. Therefore, the required materials do not contain heavy metal materials and formaldehyde, thereby improving the environmental friendliness of the preparation of the stone plastic floor;

[0133] By adding antibacterial agents, bacteria can be effectively killed, bacterial reproduction can be inhibited, and a healthier use environment can be provided.

[0134] Working principle: through the setting of PBAT substrate layer, TPU color film layer and TPU wear-resistant layer, the temperature, pressure, speed and time in the preparation process are precisely controlled, which is beneficial to improve the performance of the prepared stone plastic floor, avoid the situation that the temperature, pressure, speed and time are not up to standard or exceed the threshold, resulting in insufficient mixing or over-reaction of raw materials, and then resulting in poor performance of the prepared stone plastic floor. The stone plastic floor formed by the hot pressing composite process can make each layer closely combined, thereby improving the overall stability and anti-penetration effect of the floor, and thus can increase the service life of the obtained stone plastic floor. The PBAT resin, stabilizer, antibacterial agent, plasticizer regulator and dispersant used are all biodegradable materials, and the pebble powder in the natural stone powder used by the calcium filler is reused, so the required materials do not contain heavy metal materials and formaldehyde, thereby improving the environmental protection of the prepared stone plastic floor. By adding antibacterial agents, bacteria can be effectively killed and bacterial reproduction can be inhibited, providing a healthier use environment.

[0135] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a stone plastic floor, comprising a PBAT substrate layer, a TPU color film layer and a TPU wear-resistant layer, characterized in that: Compounding the PBAT substrate layer, the TPU color film layer and the TPU wear-resistant layer through a hot pressing compounding process to form a complete stone plastic floor; The composition and weight of the raw materials of the PBAT substrate layer of the stone plastic floor are: 130-150 parts of PBAT resin, 240-280 parts of calcium filler, 3-8 parts of stabilizer, 2-5 parts of antibacterial agent, 1-3 parts of plasticizer, 10-15 parts of polylactic acid fiber and 5-8 parts of dispersant; The preparation steps of the PBAT substrate layer of the stone plastic floor are as follows: Step S1, placing the required raw materials; PBAT resin, calcium filler, stabilizer, antibacterial agent, plasticizer, polylactic acid fiber and dispersant into a mixing tank in sequence, and mixing and stirring under precisely controlled temperature, pressure, time and speed; Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the PBAT substrate layer of the stone plastic floor.

2. The method for preparing a stone plastic floor according to claim 1, characterized in that: The TPU color film layer of the stone plastic floor has the following raw materials in terms of composition and weight: 80-120 parts of TPU granules, 1-5 parts of colorant and 5-8 parts of dispersant; The steps for preparing the TPU color film layer of the stone plastic floor are as follows: Step S1, placing TPU pellets, colorant and dispersant into a mixing tank in sequence, and mixing and stirring under precisely controlled temperature, pressure, time and speed; Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the TPU color film layer of the stone plastic floor.

3. The method for preparing a stone plastic floor according to claim 1, characterized in that: The TPU wear-resistant layer of the stone plastic floor has the following raw materials in terms of composition and weight: 80-120 parts of TPU granules and 20-35 parts of ABS granules; The steps for preparing the TPU wear-resistant layer of the stone plastic floor are as follows: Step S1, placing TPU pellets and ABS pellets into a mixing tank in sequence, and mixing and stirring them under precisely controlled temperature, pressure, time and rotation speed; Step S2, obtaining the raw materials mixed and stirred in step S1, filling them into an extruder, and performing extrusion molding under precisely controlled temperature, pressure, time and speed to obtain the TPU wear-resistant layer of the stone plastic floor.

4. The method for preparing a stone plastic floor according to claim 1, characterized in that: The hot pressing temperature of the hot pressing composite process is 130° C.-180° C., the hot pressing pressure is 10 MPa-20 MPa, and the hot pressing time is 1 h-2 h.

5. The method for preparing a stone plastic floor according to claim 1, characterized in that: The calcium filler is pebble powder with a mesh size of 300-800; the stabilizer is one of a carbodiimide anti-hydrolysis stabilizer, isocyanate and epoxy; the antibacterial agent is one of a silver ion antibacterial agent, a quaternary ammonium salt antibacterial agent or a nano antibacterial agent; the plasticizer is one of tributyl citrate or trioctyl citrate; and the dispersant is one of starch or cellulose.

6. The method for preparing a stone plastic floor according to claim 1, characterized in that: In step S1 of preparing the PBAT substrate layer, the rotation speed of the mixing tank is 800 r / min-1100 r / min, the mixing temperature is 110° C.-140° C., and the mixing time is 2 h-4 h; In step S2 of preparing the PBAT substrate layer, the extrusion temperature of the extruder is 140° C.-170° C., the mold temperature is 180° C.-220° C., the main engine speed is 10 r / min-20 r / min, and the feed speed is 15 r / min-25 r / min.

7. The method for preparing a stone plastic floor according to claim 2, characterized in that: The colorant is one of natural pigments or bio-based pigments, and the dispersant is one of starch or cellulose.

8. The method for preparing a stone plastic floor according to claim 1, characterized in that: In step S1 of preparing the TPU color film layer, the rotation speed of the mixing tank is 800 r / min-1100 r / min, the mixing temperature is 80° C.-95° C., and the mixing time is 40 min-80 min; In step S2 of preparing the TPU color film layer, the extrusion temperature of the extruder is 120°C-135°C, the mold temperature is 150°C-170°C, the main machine speed is 10r / min-20r / min, and the feeding speed is 15r / min-25r / min.

9. The method for preparing a stone plastic floor according to claim 1, characterized in that: In step S1 of preparing the TPU wear-resistant layer, the rotation speed of the mixing tank is 800 r / min-1100 r / min, the mixing temperature is 90° C.-115° C., and the mixing time is 20 min-60 min; In step S2 of preparing the TPU wear-resistant layer, the extrusion temperature of the extruder is 140°C-175°C, the mold temperature is 150°C-180°C, the main engine speed is 10r / min-20r / min, and the feeding speed is 15r / min-25r / min.

Citation Information

Patent Citations

  • A stone-plastic flooring and its preparation method

    CN106587720B

  • The method of coating for PVC flooring tile

    KR101583521B1

  • Wood-plastic PVC floorboard

    US20160229161A1

  • Composite floor underlayment with thermoplastic coatings

    US9186869B2