Preparation method of elastic polyurethane material

By introducing modified copolymers in the polyurethane synthesis process, optimizing molecular structure and interactions, forming a uniform microscopic phase separation structure, the problem of insufficient mechanical properties of existing elastic polyurethane materials is solved, the rebound performance and durability are improved, and Improved processing performance.

CN119060295APending Publication Date: 2024-12-03ZHEJIANG HENGTAIYUAN PU CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411292030.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The mechanical properties of existing elastic polyurethane materials need to be further improved, and in order to broaden their application areas, their performance needs to be improved.

Method used

Using a preparation method, including preparing polyurethane prepolymers and polyurethane elastomers, by introducing modified copolymers during polyurethane synthesis, optimizing molecular structure and interaction modes, and adjusting the soft and hard segment ratio and distribution through modified copolymers , form a uniform microscopic phase separation structure, improve rebound performance and durability, and improve processing performance.

Benefits of technology

The prepared elastic polyurethane material has excellent softness and elastic properties, improves resilience and durability, and the introduction of modified copolymers reduces viscosity, improves fluidity, makes the material easier to process, and improves production efficiency. Reduced defects and waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060295A_ABST
    Figure CN119060295A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an elastic polyurethane material, and relates to the technical field of polyurethane materials, and the preparation method comprises the following steps: S1, preparing a polyurethane prepolymer; s2, preparing a polyurethane elastomer; the prepared elastic polyurethane material has excellent flexibility and elastic performance, the elastic polyurethane material has a special soft and hard segment structure, and due to the soft and hard segment coexisting structure, when polyurethane is subjected to external force, the soft segment can deform to absorb energy, the hard segment is kept relatively stable, and the elastic polyurethane material has the advantages that the elastic polyurethane material has the excellent flexibility and elastic performance, and the service life of the elastic polyurethane material is prolonged. And a supporting point is provided for the recovery of the soft section, so that excellent rebound resilience is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane materials, in particular to a method for preparing an elastic polyurethane material. Background Art

[0002] Elastic polyurethane, as a polyurethane material with rubber properties, has attracted much attention for its excellent performance and wide application fields. Elastic polyurethane materials are a type of polymer generated by the reaction of isocyanate functional group molecules and polyols. This unique chemical reaction not only gives polyurethane materials high elasticity, but also makes them have a variety of excellent properties such as wear resistance, tear resistance, chemical resistance and wide temperature compatibility.

[0003] Polyurethane elastomers have many excellent characteristics: Polyurethane elastomers have a wide hardness range, which can be adjusted from below Shore A0 to above Shore D90. They can still maintain good rubber elasticity and elongation at break at high hardness, and have good mechanical properties at low hardness. In addition, the tensile strength and tear strength of polyurethane elastomers are better than general rubbers, and the impact strength and bending strength are higher than ordinary plastics. Polyurethane elastomers have good resistance to a variety of oils and chemical solvents, and can maintain stable performance in harsh environments. This material has good bonding effects with metals, wood, ceramics and polar polymer materials, and is easy to process and apply.

[0004] Since elastic polyurethane materials have so many excellent properties, they are widely used in various fields, including machinery, transportation, health care, sports goods, and architectural decoration.

[0005] However, the mechanical properties of the elastic polyurethane materials prepared by the existing methods need to be further improved. In order to further expand its application field, further improvements need to be made to its performance.

[0006] Based on this, a method for preparing an elastic polyurethane material is provided to solve the existing technical problems. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing an elastic polyurethane material to solve the deficiencies in the prior art.

[0008] The technical solution adopted by the present invention is as follows:

[0009] A method for preparing an elastic polyurethane material comprises the following steps:

[0010] S1: Preparation of polyurethane prepolymer:

[0011] Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 105-108° C., perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 62-64° C.;

[0012] Add isocyanate to the reactor, raise the temperature to 78-80°C, stir and react for 4 hours, then vacuum degas for 20 minutes, discharge and set aside;

[0013] The polyurethane prepolymer is stored under a nitrogen atmosphere;

[0014] S2 Preparation of polyurethane elastomer:

[0015] The polyurethane prepolymer prepared above is added to a reaction kettle, and then heated to 81-84°C, vacuum dehydrated for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into a mold, vulcanized for 30-40 minutes on a flat vulcanizer, demolded, aged for 12-15 hours, and cooled to room temperature to obtain the product;

[0016] Before injecting into the mold, the mold is preheated;

[0017] The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm.

[0018] As a further technical solution: the molecular weight of the glycerol polyether polyol in S1 is 5000;

[0019] The molecular weight of polytetramethylene ether glycol is 2000.

[0020] As a further technical solution: the mixed molar ratio of polytetrahydrofuran ether diol and glycerol polyether polyol in S1 is 1:3-5;

[0021] The mass ratio of the glycerol polyether polyol to the isocyanate is 1:2.

[0022] As a further technical solution: The preparation method of the modified copolymer described in S2 is:

[0023] First, styrene is added into the reactor, and then an inert gas is introduced into the reactor to exhaust the air in the reactor;

[0024] Adding sodium maleate, itaconic anhydride and an initiator into a solvent, stirring and mixing evenly to obtain a composite liquid;

[0025] The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid;

[0026] The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer;

[0027] The amount of methanol added was twice the volume of the reaction solution.

[0028] As a further technical solution, the inert gas is nitrogen or neon.

[0029] As a further technical solution: the mixing ratio of the sodium maleate, itaconic anhydride, initiator and solvent is 3-4g:1-1.5g:0.2-0.3g:350mL.

[0030] As a further technical solution, the solvent is dimethyl malonate;

[0031] The initiator is dicumyl peroxide.

[0032] As a further technical solution, the chain extender is any one of 1,6-hexanediol, 1,3-propylene glycol, 1,8-octanediol, and 1,4-butanediol.

[0033] As a further technical solution: the mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 10-12:3-3.5:1-1.2.

[0034] As a further technical solution, the vulcanization temperature is 110°C and the pressure is 15MPa;

[0035] The aging temperature of the aging treatment is 100°C.

[0036] Beneficial effects:

[0037] The elastic polyurethane material prepared by the present invention has excellent softness and elasticity. The elastic polyurethane material of the present invention has a special soft and hard segment structure. This structure of coexistence of soft and hard segments enables the soft segment of the polyurethane to deform to absorb energy when subjected to external force, while the hard segment remains relatively stable, providing a support point for the recovery of the soft segment, thereby achieving excellent rebound performance.

[0038] The elastic polyurethane material prepared by the present invention contains a variety of groups, including carbamate groups, ether groups, ester groups and urea groups, etc. These groups can form relatively stable hydrogen bonds, and the formation of a large number of hydrogen bonds greatly enhances the interaction between the molecules in the elastic polyurethane material. At the same time, it can further promote the microscopic phase separation between the polyurethane soft segment and the hard segment, thereby forming a relatively unique microstructure and further enhancing the elastic properties of the polyurethane elastomer.

[0039] The present invention can further optimize the molecular structure and interaction mode of polyurethane by introducing a modified copolymer with special properties during the polyurethane synthesis process, further enhance the attraction between polyurethane molecules, make the prepared polyurethane material more closely combined together, thereby improving the resilience performance; in addition, the introduction of the modified copolymer can also adjust the ratio and distribution of soft and hard segments in the polyurethane; by adjusting the ratio and distribution of the soft and hard segments, it can help to form a more uniform microscopic phase separation structure, so that the soft segment can better disperse and absorb energy during the stretching process, and the hard segment can also more effectively provide support for the recovery of the soft segment; this optimized structure helps to improve the resilience performance and durability of the polyurethane.

[0040] At the same time, the introduction of modified copolymers can also improve the processing performance of the prepared elastic polyurethane material. Mainly, the introduction of modified copolymers can reduce the viscosity of the elastic polyurethane and improve the fluidity, making the elastic polyurethane material easier to process into the desired shape and size, which not only improves production efficiency, but also helps to reduce defects and waste in the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a bar graph of the resilience of the samples of the embodiment and the comparative example. DETAILED DESCRIPTION

[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Example 1

[0044] A method for preparing an elastic polyurethane material comprises the following steps:

[0045] S1: Preparation of polyurethane prepolymer:

[0046] Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 105°C, perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 62°C;

[0047] Add isocyanate to the reactor, raise the temperature to 78°C, keep stirring and react for 4 hours, then perform vacuum degassing for 20 minutes, discharge the material and set aside;

[0048] The polyurethane prepolymer is stored under nitrogen atmosphere; the molecular weight of glycerol polyether polyol is 5000;

[0049] The molecular weight of polytetramethylene ether glycol is 2000.

[0050] The mixed molar ratio of polytetramethylene ether diol and glycerol polyether polyol is 1:3;

[0051] The mass ratio of the glycerol polyether polyol to the isocyanate is 1:2.

[0052] S2 Preparation of polyurethane elastomer:

[0053] The polyurethane prepolymer prepared above is added to the reactor, and then heated to 81°C, vacuum dewatered for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into the mold, vulcanized for 30 minutes on a flat vulcanizer, demolded, aged for 12 hours, and cooled to room temperature to obtain the product; the vulcanization temperature is 110°C and the pressure is 15MPa;

[0054] The chain extender is 1,6-hexanediol.

[0055] The mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 10:3:1.

[0056] The aging temperature of the aging treatment is 100°C.

[0057] Before injecting into the mold, the mold is preheated;

[0058] The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm.

[0059] The preparation method of the modified copolymer is:

[0060] First, styrene is added into the reactor, and then nitrogen is introduced into the reactor to exhaust the air in the reactor;

[0061] Adding sodium maleate, itaconic anhydride and dicumyl peroxide to dimethyl malonate, stirring and mixing evenly to obtain a composite liquid;

[0062] The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid;

[0063] The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer;

[0064] The amount of methanol added was twice the volume of the reaction solution.

[0065] The mixing ratio of sodium maleate, itaconic anhydride, dicumyl peroxide, and dimethyl malonate is 3g:1g:0.2g:350mL.

[0066] Example 2

[0067] A method for preparing an elastic polyurethane material comprises the following steps:

[0068] S1: Preparation of polyurethane prepolymer:

[0069] Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 106°C, perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 63°C;

[0070] Add isocyanate to the reactor, raise the temperature to 79°C, keep the temperature and stir for 4 hours, then perform vacuum degassing for 20 minutes, discharge the material and set aside;

[0071] The polyurethane prepolymer is stored under nitrogen atmosphere; the molecular weight of glycerol polyether polyol is 5000;

[0072] The molecular weight of polytetramethylene ether glycol is 2000.

[0073] The mixed molar ratio of polytetramethylene glycol and glycerol polyether polyol is 1:3.5;

[0074] The mass ratio of the glycerol polyether polyol to the isocyanate is 1:2.

[0075] S2 Preparation of polyurethane elastomer:

[0076] The polyurethane prepolymer prepared above is added to the reactor, and then heated to 82°C, vacuum dehydrated for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into the mold, vulcanized for 35 minutes on a flat vulcanizer, demolded, aged for 14 hours, and cooled to room temperature to obtain the product; the vulcanization temperature is 110°C and the pressure is 15MPa;

[0077] The chain extender is 1,6-hexanediol.

[0078] The mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 11:3.2:1.1.

[0079] The aging temperature of the aging treatment is 100°C.

[0080] Before injecting into the mold, the mold is preheated;

[0081] The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm;

[0082] The preparation method of the modified copolymer is:

[0083] First, styrene is added into the reactor, and then nitrogen is introduced into the reactor to exhaust the air in the reactor;

[0084] Adding sodium maleate, itaconic anhydride and dicumyl peroxide to dimethyl malonate, stirring and mixing evenly to obtain a composite liquid;

[0085] The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid;

[0086] The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer;

[0087] The amount of methanol added was twice the volume of the reaction solution.

[0088] The mixing ratio of sodium maleate, itaconic anhydride, dicumyl peroxide, and dimethyl malonate is 3.5g:1.2g:0.22g:350mL.

[0089] Example 3

[0090] A method for preparing an elastic polyurethane material comprises the following steps:

[0091] S1: Preparation of polyurethane prepolymer:

[0092] Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 106°C, perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 63°C;

[0093] Add isocyanate to the reactor, raise the temperature to 78°C, keep stirring and react for 4 hours, then perform vacuum degassing for 20 minutes, discharge the material and set aside;

[0094] The polyurethane prepolymer is stored under nitrogen atmosphere; the molecular weight of glycerol polyether polyol is 5000;

[0095] The molecular weight of polytetramethylene ether glycol is 2000.

[0096] The mixed molar ratio of polytetramethylene ether diol and glycerol polyether polyol is 1:4;

[0097] The mass ratio of the glycerol polyether polyol to the isocyanate is 1:2.

[0098] S2 Preparation of polyurethane elastomer:

[0099] The polyurethane prepolymer prepared above is added to the reactor, and then heated to 83°C, vacuum dewatered for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into the mold, vulcanized for 35 minutes on a flat vulcanizer, demolded, aged for 13 hours, and cooled to room temperature to obtain the product; the vulcanization temperature is 110°C and the pressure is 15MPa;

[0100] The chain extender is 1,6-hexanediol.

[0101] The mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 11:3.3:1.

[0102] The aging temperature of the aging treatment is 100°C.

[0103] Before injecting into the mold, the mold is preheated;

[0104] The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm;

[0105] The preparation method of the modified copolymer is:

[0106] First, styrene is added into the reactor, and then nitrogen is introduced into the reactor to exhaust the air in the reactor;

[0107] Adding sodium maleate, itaconic anhydride and dicumyl peroxide to dimethyl malonate, stirring and mixing evenly to obtain a composite liquid;

[0108] The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid;

[0109] The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer;

[0110] The amount of methanol added was twice the volume of the reaction solution.

[0111] The mixing ratio of sodium maleate, itaconic anhydride, diisopropylbenzene peroxide and dimethyl malonate is 3.5g:1.2g:0.25g:350mL.

[0112] Example 4

[0113] A method for preparing an elastic polyurethane material comprises the following steps:

[0114] S1: Preparation of polyurethane prepolymer:

[0115] Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 107°C, perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 63°C;

[0116] Add isocyanate to the reactor, raise the temperature to 79°C, keep the temperature and stir for 4 hours, then perform vacuum degassing for 20 minutes, discharge the material and set aside;

[0117] The polyurethane prepolymer is stored under nitrogen atmosphere; the molecular weight of glycerol polyether polyol is 5000;

[0118] The molecular weight of polytetramethylene ether glycol is 2000.

[0119] The mixed molar ratio of polytetramethylene ether diol and glycerol polyether polyol is 1:4;

[0120] The mass ratio of the glycerol polyether polyol to the isocyanate is 1:2.

[0121] S2 Preparation of polyurethane elastomer:

[0122] The polyurethane prepolymer prepared above is added to the reactor, and then heated to 83°C, vacuum dehydrated for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into the mold, vulcanized for 38 minutes on a flat vulcanizer, demolded, aged for 14 hours, and cooled to room temperature to obtain the product; the vulcanization temperature is 110°C and the pressure is 15MPa;

[0123] The chain extender is 1,6-hexanediol.

[0124] The mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 10:3.5:1.2.

[0125] The aging temperature of the aging treatment is 100°C.

[0126] Before injecting into the mold, the mold is preheated;

[0127] The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm;

[0128] The preparation method of the modified copolymer is:

[0129] First, styrene is added into the reactor, and then nitrogen is introduced into the reactor to exhaust the air in the reactor;

[0130] Adding sodium maleate, itaconic anhydride and dicumyl peroxide to dimethyl malonate, stirring and mixing evenly to obtain a composite liquid;

[0131] The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid;

[0132] The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer;

[0133] The amount of methanol added was twice the volume of the reaction solution.

[0134] The mixing ratio of sodium maleate, itaconic anhydride, diisopropylbenzene peroxide, and dimethyl malonate is 3.8g:1.2g:0.28g:350mL.

[0135] Example 5

[0136] A method for preparing an elastic polyurethane material comprises the following steps:

[0137] S1: Preparation of polyurethane prepolymer:

[0138] Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 108°C, perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 64°C;

[0139] Add isocyanate to the reactor, raise the temperature to 80°C, keep the temperature and stir for 4 hours, then perform vacuum degassing for 20 minutes, discharge the material and set aside;

[0140] The polyurethane prepolymer is stored under nitrogen atmosphere; the molecular weight of glycerol polyether polyol is 5000;

[0141] The molecular weight of polytetramethylene ether glycol is 2000.

[0142] The mixed molar ratio of polytetramethylene ether diol and glycerol polyether polyol is 1:5;

[0143] The mass ratio of the glycerol polyether polyol to the isocyanate is 1:2.

[0144] S2 Preparation of polyurethane elastomer:

[0145] The polyurethane prepolymer prepared above is added to the reactor, and then heated to 84°C, vacuum dewatered for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into the mold, vulcanized for 40 minutes on a flat vulcanizer, demolded, aged for 15 hours, and cooled to room temperature to obtain the product; the vulcanization temperature is 110°C and the pressure is 15MPa;

[0146] The chain extender is 1,6-hexanediol.

[0147] The mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 12:3.5:1.2.

[0148] The aging temperature of the aging treatment is 100°C.

[0149] Before injecting into the mold, the mold is preheated;

[0150] The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm;

[0151] The preparation method of the modified copolymer is:

[0152] First, styrene is added into the reactor, and then nitrogen is introduced into the reactor to exhaust the air in the reactor;

[0153] Adding sodium maleate, itaconic anhydride and dicumyl peroxide to dimethyl malonate, stirring and mixing evenly to obtain a composite liquid;

[0154] The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid;

[0155] The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer;

[0156] The amount of methanol added was twice the volume of the reaction solution.

[0157] The mixing ratio of sodium maleate, itaconic anhydride, diisopropylbenzene peroxide and dimethyl malonate is 4g:1.5g:0.3g:350mL.

[0158] Comparative Example 1:

[0159] Based on Example 1, no modified copolymer is added and the rest of the technical scheme remains unchanged.

[0160] test:

[0161] The properties of the polyurethane materials prepared in the examples and comparative examples were tested, and the tensile strength and elongation at break were tested according to GB / T1040.1-2018. The results are shown in Table 1:

[0162] Table 1

[0163] Tensile strength MPa Elongation at break % Example 1 51.3 1305 Example 2 52.0 1318 Example 3 52.8 1326 Example 4 51.5 1315 Example 5 51.0 1298 Comparative Example 1 43.6 1002

[0164] It can be seen from Table 1 that the elastic polyurethane material prepared by the present invention has higher tensile strength.

[0165] For the ball rebound rate test of the embodiment, refer to GB / T6670-2008:

[0166] Table 2

[0167]

[0168]

[0169] It can be seen from Table 2 that the elastic polyurethane material prepared by the present invention has excellent resilience, and the introduction of the modified copolymer can significantly improve the resilience of the elastic polyurethane material.

[0170] Based on the sample in Example 1, the effects of different chain extenders on the resilience of the elastic polyurethane material were compared:

[0171] Example 1 uses 1,6-hexanediol, Group 1 uses 1,3-propylene glycol, Group 2 uses 1,8-octanediol, and Group 3 uses 1,4-butanediol;

[0172] Among them, groups 1-3 and Example 1 only use different chain extenders;

[0173] Table 3

[0174] Rebound rate % Example 1 87.3 Group 1 85.2 Group 2 86.8 Group 3 86.0

[0175] It can be seen from Table 3 that the elastic polyurethane materials prepared by different chain extenders have different resilience. Using 1,6-hexanediol as a chain extender can prepare an elastic polyurethane material with higher resilience.

[0176] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. A method for preparing an elastic polyurethane material, characterized in that: The following steps are involved: S1: Preparation of polyurethane prepolymer: Add polytetrahydrofuran ether diol and glycerol polyether polyol into the reaction kettle, then heat it to 105-108° C., perform vacuum dehydration treatment for 2 hours under a negative pressure of 0.05 MPa, and then adjust the temperature to 62-64° C.; Add isocyanate to the reactor, raise the temperature to 78-80°C, stir and react for 4 hours, then vacuum degas for 20 minutes, discharge and set aside; The polyurethane prepolymer is stored under a nitrogen atmosphere; S2 Preparation of polyurethane elastomer: The polyurethane prepolymer prepared above is added to a reaction kettle, and then heated to 81-84°C, vacuum dehydrated for 2 hours, and then the modified copolymer and chain extender are added, stirred for 10 minutes, vacuum degassed for 10 minutes, and then injected into a mold, vulcanized for 30-40 minutes on a flat vulcanizer, demolded, aged for 12-15 hours, and cooled to room temperature to obtain the product; Before injecting into the mold, the mold is preheated; The preheating treatment is to preheat the slurry mold to 80° C. and keep it warm.

2. The method for preparing an elastic polyurethane material according to claim 1, characterized in that: The molecular weight of the glycerol polyether polyol in S1 is 5000; The molecular weight of polytetramethylene ether glycol is 2000.

3. The method for preparing an elastic polyurethane material according to claim 1, characterized in that: The mixed molar ratio of polytetramethylene ether diol and glycerol polyether polyol in S1 is 1:3-5; The mass ratio of the glycerol polyether polyol to the isocyanate is 1:

2.

4. The method for preparing an elastic polyurethane material according to claim 1, characterized in that: The preparation method of the modified copolymer described in S2 is: First, styrene is added into the reactor, and then an inert gas is introduced into the reactor to exhaust the air in the reactor; Adding sodium maleate, itaconic anhydride and an initiator into a solvent, stirring and mixing evenly to obtain a composite liquid; The composite liquid was added dropwise to the reaction kettle, the temperature was adjusted to 70°C, and the reaction was stirred for 2 hours, and the material was discharged to obtain a reaction liquid; The reaction solution was precipitated with methanol, filtered, washed with deionized water for 10 minutes, and dried at 60° C. for 12 hours to obtain a modified copolymer; The amount of methanol added was twice the volume of the reaction solution.

5. The method for preparing an elastic polyurethane material according to claim 4, characterized in that: The inert gas is nitrogen or neon.

6. The method for preparing an elastic polyurethane material according to claim 4, characterized in that The mixing ratio of the sodium maleate, itaconic anhydride, initiator and solvent is 3-4g:1-1.5g:0.2-0.3g:350mL.

7. The method for preparing an elastic polyurethane material according to claim 4, characterized in that: The solvent is dimethyl malonate; The initiator is dicumyl peroxide.

8. The method for preparing an elastic polyurethane material according to claim 1, characterized in that: The chain extender is any one of 1,6-hexanediol, 1,3-propylene glycol, 1,8-octanediol and 1,4-butanediol.

9. The method for preparing an elastic polyurethane material according to claim 1, characterized in that The mixing mass ratio of the polyurethane prepolymer, the modified copolymer and the chain extender is 10-12:3-3.5:1-1.

2.

10. The method for preparing an elastic polyurethane material according to claim 1, characterized in that: The vulcanization temperature is 110°C and the pressure is 15MPa; The aging temperature of the aging treatment is 100°C.

Citation Information

Cited By

  • Polyurethane and preparation method thereof

    CN119552338A