Binder and solid-state battery comprising same

By esterification reaction of modified hydroxypropyl cellulose and sulfamic acid, a binder with high mechanical stability and conductivity was prepared, which solved the problem of deterioration of adhesion in sulfide solid electrolyte batteries and improved the Cycling performance and safety of the battery.

CN119081580APending Publication Date: 2024-12-06HUNAN FARNLET NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411212736.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The high reactivity of sulfide solid electrolytes leads to the deterioration of the commonly used binder during charging and discharging of lithium-ion batteries, resulting in collapse of the electrode structure and affecting the cycle stability and safety of the battery.

Method used

Modified hydroxypropyl cellulose is prepared by esterification reaction with fatty acids and sulfamic acid, which enhances the flexibility and ionic conductivity of the molecular chain, and is modified with sulfamic acid groups to form a sulfamic acid group with High mechanical stability and conductive adhesives for the preparation of solid-state batteries.

Benefits of technology

It improves the circulation and conductivity of solid-state batteries, reduces electrode structure collapse and active substance fall off, extends the cycle life of the battery, significantly accelerates the discharge of lithium ions, and enhances the adhesion force.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a binder and a solid-state battery comprising the same, and relates to the technical field of solid-state batteries. The preparation method of the binder comprises the following steps: S1, carrying out first esterification reaction on a first esterifying agent and hydroxyl in hydroxy propyl cellulose to obtain modified hydroxy propyl cellulose; the first esterifying agent comprises fatty acid and / or fatty acid anhydride; s2, carrying out a second esterification reaction on a second esterifying agent and hydroxyl in the modified hydroxy propyl cellulose to obtain the binder, the second esterifying agent comprises sulfamic acid and / or sulfamate. The solid-state battery containing the binder has good conductivity and cycle performance, and has a good application prospect in the solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a binder and a solid-state battery comprising the same. Background Art

[0002] Lithium-ion batteries are widely used in electric vehicles, portable electronic products and other fields due to their high energy density, high operating voltage, no memory effect, and long cycle life. Currently, commercial lithium-ion batteries mostly use liquid electrolytes with organic solvents and lithium salts as the main components. Since liquid electrolytes are easy to leak and burn, there is a problem of insufficient safety when they are used in high energy density batteries. The emergence of solid-state batteries effectively solves the above problems.

[0003] Solid electrolytes are an important component of solid-state batteries and play an important role in the practical application of solid-state batteries. Sulfide solid electrolytes have the advantages of high ionic conductivity and low grain boundary impedance. The electrolyte membrane is usually prepared by mixing sulfide solid electrolytes, binders, and solvents through a wet film formation method. The binder can stabilize the electrode structure and maintain the conduction of ions and electrons during the battery charge and discharge process. However, due to the high reactivity of sulfide solid electrolytes, the commonly used binders tend to deteriorate in adhesion as the battery is charged and discharged, resulting in collapse of the electrode structure and battery failure. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing a binder, which can effectively improve the cycle performance.

[0005] The present invention also provides a binder prepared by the above preparation method.

[0006] The invention also provides a positive electrode plate.

[0007] The invention also provides a solid electrolyte membrane.

[0008] The invention also provides a solid-state battery.

[0009] The present invention also provides the use of the binder, positive electrode sheet or solid electrolyte membrane prepared by the above preparation method in a solid-state battery.

[0010] A method for preparing a binder according to a first aspect of the present invention comprises the following steps: S1, allowing a first esterifying agent to undergo a first esterification reaction with a hydroxyl group in the hydroxypropyl cellulose to obtain modified hydroxypropyl cellulose; the first esterifying agent comprises a fatty acid and / or a fatty acid anhydride; S2. causing a second esterification reaction between a second esterifying agent and the hydroxyl groups in the modified hydroxypropyl cellulose; the second esterifying agent comprises aminosulfonic acid and / or aminosulfonate.

[0011] The preparation method according to the embodiment of the present invention has at least the following beneficial effects: Through this preparation method, grafting fatty acid chains of appropriate length on some hydroxyl groups of hydroxypropyl cellulose can enhance the flexibility of the molecular chain and the room temperature ionic conductivity, making the overall structure more mechanically stable, making it easier to adapt to the deformation and expansion of the material during the battery charging and discharging process, reducing stress concentration, thereby reducing the collapse of the electrode structure caused by volume expansion, and maintaining the electrode structure to prevent the active material from falling off; it can also promote the movement between hydroxypropyl cellulose molecular chains, which is beneficial to the transmission and diffusion of ions in the electrolyte, and improve the charging and discharging speed and efficiency of the battery; and reduce the polarization effect of the hydroxypropyl cellulose molecular chain, reduce the increase in resistance caused by polarization during the cycle of the battery, and improve the cycle stability of the battery. The modification of the aminosulfonic acid group can further widen the conductive ion conductive path, significantly accelerate the discharge of lithium ions, and effectively improve the interaction force with solid electrolytes, active substances, etc., thereby improving the bonding force. In this way, the conductive performance and cycle performance of the solid-state battery are effectively guaranteed, and the prepared Ninajie has a good application prospect in solid-state batteries.

[0012] According to some embodiments of the present invention, the fatty acid includes at least one of C7-C18 fatty acids, wherein C7-C18 can be C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18.

[0013] According to some embodiments of the present invention, the fatty acid includes at least one of caprylic acid, nonanoic acid, decanoic acid, neodecanoic acid, undecanoic acid, lauric acid (dodecanoic acid), tridecanoic acid, tetradecanoic acid (myristic acid palmitic acid), pentadecanoic acid, hexadecanoic acid (palmitic acid), heptadecanoic acid, and octadecanoic acid (stearic acid).

[0014] According to some embodiments of the present invention, the fatty acid anhydride includes at least one of C7-C18 fatty acid anhydrides, wherein C7-C18 may be C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18.

[0015] According to some embodiments of the present invention, the fatty acid anhydride includes at least one of octanoic anhydride, nonanoic anhydride, decanoic anhydride, neodecanoic anhydride, undecanoic anhydride, lauric anhydride (dodecanoic anhydride), tridecanoic anhydride, tetradecanoic anhydride (myristic acid palmitic anhydride), pentadecanoic anhydride, hexadecanoic anhydride (palmitic anhydride), heptadecanoic anhydride, and octadecanoic anhydride (stearic anhydride).

[0016] According to some embodiments of the present invention, the aminosulfonate includes at least one of potassium sulfamate, sodium sulfamate, ammonium sulfamate, and nickel sulfamate.

[0017] According to some embodiments of the present invention, step S1 comprises the following steps: The first esterifying agent, the hydroxypropyl cellulose, the acid-binding agent and the first catalyst are mixed and reacted to obtain modified hydroxypropyl cellulose.

[0018] According to some embodiments of the present invention, in step S1, the acid binding agent includes at least one of pyridine and triethylamine.

[0019] According to some embodiments of the present invention, in step S1, the first catalyst includes toluenesulfonyl chloride.

[0020] According to some embodiments of the present invention, in step S1, the amount of the first esterifying agent is 0.4-0.5 eq / HPC-OH.

[0021] According to some embodiments of the present invention, in step S1, the molar ratio of the acid binding agent to the first catalyst is 1:0.8-1.2.

[0022] According to some embodiments of the present invention, in step S1, the amount of the first catalyst used is 1-1.2 eq / HPC-OH.

[0023] According to some embodiments of the present invention, the reaction temperature of step S1 is 65°C-70°C.

[0024] According to some embodiments of the present invention, the reaction time of step S1 is 12 h to 16 h.

[0025] According to some embodiments of the present invention, the reaction solvent of step S1 includes N,N-dimethylacetamide.

[0026] According to some embodiments of the present invention, step S1 further comprises performing a first post-treatment after the reaction, wherein the first post-treatment comprises at least one of a precipitation product treatment and a solvent removal treatment.

[0027] According to some embodiments of the present invention, the precipitation product treatment includes mixing the reaction product with a 45% (v / v) to 55% (v / v) ether aqueous solution, and performing solid-liquid separation to obtain a solid phase.

[0028] According to some embodiments of the present invention, the solvent removal treatment includes at least one of Soxhlet extraction and rotary evaporation.

[0029] According to some embodiments of the present invention, step S2 comprises the following steps: The modified hydroxypropyl cellulose, the second esterifying agent and the second catalyst are mixed and reacted to obtain the binder.

[0030] According to some embodiments of the present invention, in step S2, the mass ratio of the modified hydroxypropyl cellulose to the second esterifying agent is 1:1.5-2. The modified hydroxypropyl cellulose is hydroxypropyl cellulose grafted with fatty acid chains.

[0031] According to some embodiments of the present invention, in step S2, the mass ratio of the modified hydroxypropyl cellulose to the second catalyst is 1:0.25-0.5.

[0032] According to some embodiments of the present invention, the second catalyst comprises a strongly acidic cation exchange resin, and the strongly acidic cation exchange resin comprises a sulfonic acid type strongly acidic cation exchange resin.

[0033] According to some embodiments of the present invention, the strongly acidic cation exchange resin includes at least one of AMBERLITEIR 120H, AMBERLITE FPC22H, Amberlyst A 15, and Lewatit Monoplus S100.

[0034] According to some embodiments of the present invention, the reaction solvent of step S2 includes N,N-dimethylacetamide.

[0035] According to some embodiments of the present invention, the reaction temperature of step S2 is 90°C-95°C.

[0036] According to some embodiments of the present invention, the reaction time of step S2 is 3 h to 4 h.

[0037] According to some embodiments of the present invention, step S2 further comprises performing a second post-treatment after the reaction, wherein the second post-treatment comprises at least one of a neutralization treatment, a purification treatment, and a solvent removal treatment.

[0038] According to some embodiments of the present invention, the neutralization treatment includes adjusting the pH of the reaction system to 6.8-7.2.

[0039] According to some embodiments of the present invention, the purification treatment comprises dialysis, wherein the molecular weight cut-off of the dialysis is 3.25 kDa to 3.75 kDa, and the dialysis time is 12 h to 16 h.

[0040] The adhesive is prepared by the above preparation method according to the second aspect of the embodiment of the present invention.

[0041] According to a positive electrode sheet of the third embodiment of the present invention, the raw material for preparing the positive electrode sheet includes the binder prepared by the above preparation method. Since the positive electrode sheet adopts all the technical solutions of the binder of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0042] According to some embodiments of the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one or both sides of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, a solid electrolyte, a conductive agent and the binder.

[0043] According to some embodiments of the present invention, in the positive electrode active material layer, the mass percentage of the binder is 0.1 wt % to 10 wt %.

[0044] According to some embodiments of the present invention, in the positive electrode active material layer, the mass percentage of the positive electrode active material is 60wt%~80wt%.

[0045] According to some embodiments of the present invention, in the positive electrode active material layer, the mass percentage of the solid electrolyte is 15wt%~25wt%.

[0046] According to some embodiments of the present invention, in the positive electrode active material layer, the mass percentage of the conductive agent is 0.1 wt % to 10 wt %.

[0047] According to some embodiments of the present invention, the method for preparing the positive electrode sheet comprises the following steps: The positive electrode active material, the solid electrolyte, the conductive agent and the binder are mixed with a solvent to obtain a positive electrode slurry; the positive electrode slurry is loaded on a current collector and dried to obtain a positive electrode sheet.

[0048] A solid electrolyte membrane according to the fourth aspect of the present invention includes the binder prepared by the above preparation method. Since the solid electrolyte membrane adopts all the technical solutions of the binder of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.

[0049] According to some embodiments of the present invention, in the solid electrolyte membrane, the mass percentage of the binder is 0.5wt%~2wt%.

[0050] According to some embodiments of the present invention, the solid electrolyte membrane includes a solid electrolyte and the binder.

[0051] According to some embodiments of the present invention, the method for preparing the solid electrolyte membrane comprises the following steps: The binder and the solid electrolyte are mixed and extruded to obtain the solid electrolyte membrane.

[0052] According to some embodiments of the present invention, the solid electrolyte membrane includes a sulfide solid electrolyte.

[0053] A solid-state battery according to the fifth aspect of the present invention comprises the binder prepared by the above preparation method, the above positive electrode sheet or the above solid electrolyte membrane. Since the solid-state battery adopts all the technical solutions of the binder of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.

[0054] According to the sixth aspect of the present invention, the above-mentioned preparation method, the binder, the positive electrode sheet or the solid electrolyte membrane prepared by the above-mentioned preparation method are used in solid-state batteries.

[0055] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION

[0056] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0057] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0058] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0059] In the description of the present invention, it is necessary to understand that descriptions involving orientation, such as orientation or positional relationship indicated by “up”, “down”, etc., are based on the orientation or positional relationship shown and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0060] In the description of the present invention, it should be noted that, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in the present invention in combination with the specific content of the technical solution.

[0061] In the description of the present invention, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.

[0062] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0063] In the description of the present invention, eq / HPC-OH refers to the molar ratio of a component to the hydroxyl content in hydroxypropyl cellulose. If the amount of component A is 1 eq / HPC-OH, it means that the molar ratio of component A to the hydroxyl content in hydroxypropyl cellulose is 1:1.

[0064] The hydroxypropyl cellulose used in the examples of the present invention was purchased from Shanghai Yuanye Biotechnology Co., Ltd., and the hydroxypropyl content was 50 wt % to 66 wt %.

[0065] Example 1 This example provides a binder, and the preparation method is as follows: S1. Under nitrogen environment, 2 g hydroxypropyl cellulose (HPC) was dissolved in 100 mL N,N-dimethylacetamide, followed by the addition of dodecanoic acid (CAS No.: 93639-08-8, 0.5 eq / HPC-OH), toluenesulfonyl chloride (CAS No.: 1939-99-7, 1 eq / HPC-OH) and pyridine (CAS No.: 110-86-1). After reacting at 65 °C for 16 h, the reactant was poured into 200 mL 50% (v / v) ether aqueous solution, filtered to obtain a precipitate, and the solvent was removed by Soxhlet extraction to obtain modified hydroxypropyl cellulose.

[0066] Wherein, the molar ratio of pyridine to toluenesulfonyl chloride is 1:1.

[0067] S2. Add 2 g of modified hydroxypropyl cellulose and 4 g of aminosulfonic acid (CAS No.: 5329-14-6) to 50 mL of N,N-dimethylacetamide, heat to 90°C, add 1 g of AMBERLITE FPC22H, stir and react for 3 h, terminate the reaction in an ice-water bath, adjust the pH to 7, filter out the solid, dialyze with distilled water (molecular weight cutoff: 3.5 kDa) for 12 h, and remove the solvent by rotary evaporation to obtain the binder.

[0068] Example 2 This example provides a binder, and the preparation method is as follows: S1. Under nitrogen environment, 2 g of hydroxypropyl cellulose was dissolved in 100 mL of N,N-dimethylacetamide, followed by the addition of hexadecanoic acid (CAS No.: 1002-84-2, 0.4 eq / HPC-OH), toluenesulfonyl chloride (1.2 eq / HPC-OH) and pyridine. After reacting at 70 °C for 12 h, the reactant was poured into 200 mL of 50% (v / v) ether aqueous solution, filtered to obtain a precipitate, and the solvent was removed by Soxhlet extraction to obtain modified hydroxypropyl cellulose.

[0069] Wherein, the molar ratio of pyridine to toluenesulfonyl chloride is 1:1.

[0070] S2. Add 2 g of modified hydroxypropyl cellulose and 3 g of aminosulfonic acid to 50 mL of N,N-dimethylacetamide. Heat to 95°C, add 0.5 g of AMBERLITE FPC22H, stir and react for 4 h, terminate the reaction in an ice-water bath, adjust the pH to 7, filter out the solid, dialyze with distilled water (molecular weight cutoff: 3.5 kDa) for 16 h, and remove the solvent by rotary evaporation to obtain the binder.

[0071] Example 3 (Compared to Example 1, dodecanoic acid was replaced with an equal molar amount of octanoic acid) This example provides a binder, and the preparation method is as follows: S1. Under nitrogen environment, 2 g of hydroxypropyl cellulose was dissolved in 100 mL of N,N-dimethylacetamide, and then caprylic acid (CAS No.: 124-07-2, added in an amount of 0.5 eq / HPC-OH), toluenesulfonyl chloride (added in an amount of 1 eq / HPC-OH) and pyridine were added in sequence. After reacting at 65°C for 16 h, the reactant was poured into 200 mL of 50% (v / v) ether aqueous solution, filtered to obtain a precipitate, and the solvent was removed by Soxhlet extraction to obtain modified hydroxypropyl cellulose.

[0072] Wherein, the molar ratio of pyridine to toluenesulfonyl chloride is 1:1.

[0073] S2. Add 2 g of modified hydroxypropyl cellulose and 4 g of aminosulfonic acid to 50 mL of N,N-dimethylacetamide, heat to 90°C, add 1 g of AMBERLITE FPC22H, stir and react for 3 h, terminate the reaction in an ice-water bath, adjust the pH to 7, filter out the solid, dialyze with distilled water (molecular weight cutoff: 3.5 kDa) for 12 h, and remove the solvent by rotary evaporation to obtain the binder.

[0074] Comparative Example 1 (Compared with Example 1, step S1 is omitted) This example provides a binder, and the preparation method is as follows: Add 2 g of hydroxypropyl cellulose and 4 g of aminosulfonic acid to 50 mL of N,N-dimethylacetamide, heat to 90°C, add 1 g of AMBERLITE FPC22H, stir and react for 3 h, terminate the reaction in an ice-water bath, adjust the pH to 7, filter out the solid, dialyze with distilled water (molecular weight cutoff is 3.5 kDa) for 12 h, and remove the solvent by rotary evaporation to obtain the binder.

[0075] Comparative Example 2 (Compared with Example 1, step S2 is omitted) This example provides a binder, and the preparation method is as follows: Under nitrogen environment, 2 g of hydroxypropyl cellulose was dissolved in 100 mL of N,N-dimethylacetamide, followed by the addition of dodecanoic acid (0.5 eq / HPC-OH), toluenesulfonyl chloride (1 eq / HPC-OH) and pyridine. After reacting at 65 °C for 16 h, the reactant was poured into 200 mL of 50% (v / v) ether aqueous solution, filtered to obtain a precipitate, and the solvent was removed by Soxhlet extraction to obtain a binder.

[0076] Wherein, the molar ratio of pyridine to toluenesulfonyl chloride is 1:1.

[0077] Comparative Example 3 (Compared to Example 1, dodecanoic acid was replaced with an equal molar amount of eicosanoic acid) This example provides a binder, and the preparation method is as follows: S1. Under nitrogen environment, 2 g of hydroxypropyl cellulose was dissolved in 100 mL of N,N-dimethylacetamide, and then eicosanoic acid (CAS No.: 506-30-9, added in an amount of 0.5 eq / HPC-OH), toluenesulfonyl chloride (added in an amount of 1 eq / HPC-OH) and pyridine were added in sequence. After reacting at 65°C for 16 h, the reactant was poured into 200 mL of 50% (v / v) ether aqueous solution, filtered to obtain a precipitate, and the solvent was removed by Soxhlet extraction to obtain modified hydroxypropyl cellulose.

[0078] Wherein, the molar ratio of pyridine to toluenesulfonyl chloride is 1:1.

[0079] S2. Add 2 g of modified hydroxypropyl cellulose and 4 g of aminosulfonic acid to 50 mL of N,N-dimethylacetamide, heat to 90°C, add 1 g of AMBERLITE FPC22H, stir and react for 3 h, terminate the reaction in an ice-water bath, adjust the pH to 7, filter out the solid, dialyze with distilled water (molecular weight cutoff: 3.5 kDa) for 12 h, and remove the solvent by rotary evaporation to obtain the binder.

[0080] Test example The binders of Examples 1 to 3 and Comparative Examples 1 to 3 were used to prepare solid-state batteries, and their charge and discharge performance was tested. The preparation method of the solid-state battery is as follows: (1) Positive electrode: After dissolving the binder to be tested in acetone, add active material NCM811 and solid electrolyte Li 6 PS 5 Cl and conductive agent VGCF were fully stirred and mixed to prepare positive electrode slurry. The positive electrode slurry was evenly coated on the surface of aluminum foil, dried at 60°C, cold pressed, and sliced ​​to obtain positive electrode sheets (coating thickness was 50 μm).

[0081] Among them, active material NCM811, solid electrolyte Li 6 PS 5 The mass ratio of Cl, conductive agent VGCF and the binder to be tested is 70:20:5:5.

[0082] (2) Negative electrode: thin lithium sheet (20 μm thick).

[0083] (3) Solid electrolyte membrane: Solid electrolyte Li with a mass ratio of 99:1 3 PS 4 , mix the binder to be tested, add 2 times the mass of deionized water, stir thoroughly and mix evenly, then apply it on the glass surface, dry at 60℃, and slice to obtain an electrolyte membrane with a thickness of 50μm (4) Assembly: The positive electrode sheet, electrolyte membrane sheet, and negative electrode sheet are stacked in order, pressed at 300 MPa, and packaged to obtain a solid-state battery.

[0084] Charge and discharge performance test: Set the operating voltage range to 2.8V~4.2V. Use constant current charge and discharge mode for cycle test, the test current is 1C. The test temperature is 45℃.

[0085] The results are shown in Table 1.

[0086] Table 1 Group <![CDATA[Ionic conductivity of electrolyte membrane mS·cm -1 (at 25 °C)]]> Positive electrode slice Capacity retention after 50 cycles (%) Capacity retention after 200 cycles (%) Example 1 1.75 No powder loss 97.5 95.9 Example 2 1.69 No powder loss 96.4 93.7 Example 3 1.82 No powder loss 97.3 95.0 Comparative Example 1 1.59 No powder loss 92.9 87.4 Comparative Example 2 1.46 Slight powder loss 91.1 84.5 Comparative Example 3 1.65 Slight powder loss 93.9 89.9 The binders of Examples 1 to 3 can all make the electrolyte membrane have high room temperature ionic conductivity, and the edges of the positive electrode sheet remain intact after slicing without powder falling. At the same time, the solid-state battery prepared still has a high capacity retention rate after 200 cycles.

[0087] The room temperature ionic conductivity of the electrolyte membrane prepared by the binder of Comparative Example 1 was significantly reduced, and the cycle performance of the prepared battery was poor. This may be due to the lack of fatty acid chain modification, the poor compatibility between the electrolyte material and the binder, the poor mechanical stability, and thus the poor cycle performance.

[0088] The room temperature ionic conductivity of the electrolyte membrane prepared by the binder of Comparative Example 2 was significantly reduced, and the cycle performance of the prepared battery was poor. This may be due to the lack of aminosulfonic acid group modification, the poor ion diffusion effect, the poor bonding force, and thus the poor conductivity and cycle performance.

[0089] The positive electrode sheet made by the binder of Comparative Example 3 has a slight powdering phenomenon after slicing; and the battery cycle performance is poor. This may be because the grafted fatty acid chain is too long, which hinders the formation of the ion transmission path, resulting in the obstruction of ion movement in the electrolyte, and the too long fatty acid chain may increase the gap and distortion between molecules, affecting the mutual attraction and binding ability between molecules, making the adhesiveness of the binder worse, thereby causing the overall structural stability to deteriorate.

[0090] The embodiments of the present invention are described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A method for preparing a binder, characterized in that: The following steps are involved: S1, allowing a first esterifying agent to undergo a first esterification reaction with a hydroxyl group in hydroxypropyl cellulose to obtain modified hydroxypropyl cellulose; the first esterifying agent comprises a fatty acid and / or a fatty acid anhydride; S2, allowing a second esterifying agent to undergo a second esterification reaction with the hydroxyl groups in the modified hydroxypropyl cellulose to obtain the binder; the second esterifying agent includes aminosulfonic acid and / or aminosulfonate.

2. The preparation method according to claim 1, characterized in that: The fatty acid includes at least one of C7~C18 fatty acids; And / or, the fatty acid anhydride comprises at least one of C7~C18 fatty acid anhydride; And / or, the aminosulfonate includes at least one of potassium aminosulfonate, sodium aminosulfonate, ammonium aminosulfonate, and nickel aminosulfonate.

3. The preparation method according to claim 1, characterized in that: Step S1 includes the following steps: The first esterifying agent, the hydroxypropyl cellulose, the acid-binding agent and the first catalyst are mixed and reacted to obtain modified hydroxypropyl cellulose; And / or, step S2 comprises the following steps: The modified hydroxypropyl cellulose, the second esterifying agent and the second catalyst are mixed and reacted to obtain the binder.

4. The preparation method according to claim 3, characterized in that In step S1, the amount of the first esterifying agent is 0.4-0.5 eq / HPC-OH; And / or, in step S1, the molar ratio of the acid binding agent to the first catalyst is 1:0.8-1.2; And / or, in step S1, the amount of the first catalyst is 1-1.2 eq / HPC-OH; And / or, in step S1, the acid binding agent includes at least one of pyridine and triethylamine; and / or, in step S1, the first catalyst comprises toluenesulfonyl chloride; and / or, the reaction temperature of step S1 is 65°C to 70°C; And / or, the reaction time of step S1 is 12 h to 16 h.

5. The preparation method according to claim 3, characterized in that: In step S2, the mass ratio of the modified hydroxypropyl cellulose, the second esterifying agent, and the second catalyst is 1:1.5-2:0.25-0.5; and / or, in step S2, the second catalyst comprises a strongly acidic cation exchange resin; And / or, the reaction temperature of step S2 is 90°C to 95°C; And / or, the reaction time of step S2 is 3 h to 4 h.

6. A binder, characterized in that: The binder is prepared by the preparation method according to any one of claims 1 to 5.

7. A positive electrode sheet, characterized in that: The raw material for preparing the positive electrode plate comprises a binder prepared by the preparation method according to any one of claims 1 to 5.

8. A solid electrolyte membrane, characterized in that: The solid electrolyte membrane comprises a binder obtained by the preparation method according to any one of claims 1 to 5.

9. A solid-state battery, characterized in that: It comprises a binder obtained by the preparation method according to any one of claims 1 to 5, a positive electrode sheet according to claim 7 or a solid electrolyte membrane according to claim 8.

10. Use of the preparation method according to any one of claims 1 to 5, the binder according to claim 6, the positive electrode sheet according to claim 7 or the solid electrolyte membrane according to claim 8 in a solid-state battery.

Citation Information

Cited By

  • Fine iron powder cold-pressed pellet adhesive and preparation method thereof

    CN120400513A