Preparation and application of catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide

By using CuMnO2-Vo catalyst composed of Mn and Cu, the problem of low activity of manganese-based catalysts is solved through ultrasonic and radio frequency plasma treatment, and efficient carbon dioxide electrocatalytic reduction of ethylene is achieved, suitable for industrial applications and shown good stability and selective.

CN119082784APending Publication Date: 2024-12-06CHONGQING UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411204358.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Manganese-based catalysts have low catalytic activity during the electrocatalytic reduction of carbon dioxide to make ethylene, resulting in difficulty in C-C coupling and low product selectivity, making it difficult to achieve industrial application.

Method used

Using Mn and Cu as active components, the thick layer of nanosheets were peeled off by physical ultrasound, and radio frequency plasma treatment was performed under room temperature to regulate the oxygen vacancies of the nanosheets and the d-band center of the active components, and prepare the CuMnO2-Vo catalyst. , improve the stability of the catalyst and selectivity of specific products.

Benefits of technology

It significantly improves the catalytic activity of the catalyst and the selectivity of ethylene, reduces production costs, is suitable for industrial applications, and shows high stability and Faraday efficiency at room temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082784A_ABST
    Figure CN119082784A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of a catalyst for preparing ethylene through electrocatalytic reduction of carbon dioxide, and the preparation method of the catalyst comprises the following steps: (1) adding water-soluble copper salt and manganese salt into deionized water to obtain a solution A; polyvinylpyrrolidone K30 is dissolved in deionized water, and a solution B is obtained; (2) adding a NaOH solution into the solution A to adjust the pH value of the solution to 7-9, and then dropwise adding the solution B into the solution A to obtain mixed slurry; (3) carrying out a hydrothermal reaction on the mixed slurry at a hydrothermal reaction temperature of 50-120 DEG C for 12-36 h to obtain a black precipitate and a supernatant; performing ultrasonic treatment on the black precipitate and the supernate to obtain a black solution; centrifuging, washing and drying to obtain black powder; and (4) the black powder is subjected to radio frequency plasma treatment for 10 min under the treatment atmosphere of O2 and the power of 250 W, and the CuMnO2-Vo catalyst is obtained. The catalyst is used as a catalyst for preparing ethylene through carbon dioxide electrocatalytic reduction, the electrocatalytic activity of CO2RR is high, the Faraday efficiency of a specific product ethylene is high, and the catalyst is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of low-carbon processing, in particular to the preparation and application of a catalyst for producing ethylene through electrocatalytic reduction of carbon dioxide. Background Art

[0002] Capturing and storing CO2 to produce fuels or chemicals is an important strategy to achieve CO2 emission reductions and also facilitate the transition to alternative energy sources.

[0003] Electrocatalytic reduction of carbon dioxide is one of the most promising CO2 utilization technologies. Its core lies in the catalyst. Under normal temperature conditions and the action of the catalyst, greenhouse gas CO2 is converted into ethylene, which has the dual advantages of implementing the strategy of mitigating global warming and providing valuable chemicals and fuels. Therefore, the development of catalysts for electrocatalytic reduction of carbon dioxide to ethylene is imperative.

[0004] Electrocatalytic CO2 RR technology involves multiple proton-electron transfer steps to generate multiple products. Therefore, it is necessary to regulate proton-electron transfer through catalysts to improve the selectivity of directional products. The precious metal catalysts Pd, Pt, Rh, Ru and Ir that have been studied have good catalytic activity and stability, but the cost of using precious metals as catalysts is very high and it is difficult to apply them to industrialization. As a non-precious metal with abundant reserves, high activity and low price, manganese-based catalysts have received extensive attention and are expected to become catalysts for the electrocatalytic reduction of carbon dioxide to ethylene. However, when using manganese-based catalysts, the adsorption bonding of the key intermediates *COOH and *CO is weak, making CC coupling difficult, resulting in low selectivity of C2 products and low catalytic activity. Therefore, adjusting the binding strength of the key intermediates on the two-dimensional material is a key issue in improving the catalytic activity. Therefore, developing a catalyst that saves time, energy and improves the catalytic performance of electrocatalytic reduction of carbon dioxide has become the focus of realizing the industrialization of electrocatalytic reduction of carbon dioxide. Summary of the invention

[0005] In view of the above-mentioned problem of low catalytic activity when current manganese-based catalysts are used as catalysts for electrocatalytic reduction of carbon dioxide to produce ethylene, the present invention provides a method for preparing a catalyst for electrocatalytic reduction of carbon dioxide to produce ethylene.

[0006] This preparation method uses Mn and Cu as active components, peels off thick nanosheets through physical ultrasonic methods, and modulates the power of radio frequency plasma treatment at room temperature to regulate the oxygen vacancies of the nanosheets and the d-band center of the active components, so as to improve the stability of the catalyst and the selectivity of specific products.

[0007] The preparation method of the catalyst for producing ethylene by electrocatalytic reduction of carbon dioxide provided by the present invention comprises the following steps:

[0008] (1) Weigh equimolar amounts of water-soluble copper salt and manganese salt, add deionized water, and stir until completely dissolved to obtain a light blue solution A; dissolve polyvinylpyrrolidone K30 (PVP) in deionized water to obtain a colorless and transparent solution B.

[0009] (2) NaOH solution was added to solution A to adjust the pH of the solution to 7-9, and then solution B was added dropwise to solution A, stirred for 30 min to obtain a mixed slurry, and stirring was continued for 30 min.

[0010] (3) subjecting the mixed slurry obtained in step (2) to a hydrothermal reaction at a temperature of 50 to 120°C for 12 to 36 hours until a black precipitate and a supernatant are obtained; subjecting the black precipitate and the supernatant to an ultrasonic treatment to obtain a black solution; and centrifuging the black solution, washing, and drying to obtain a black powder.

[0011] (4) The black powder was placed in a radio frequency plasma device for treatment. Specifically, the black powder was treated at room temperature and an O2 atmosphere at a power of 250 W for 10 min to obtain CuMnO2-V o Catalyst. That is, as a catalyst for the electrocatalytic reduction of carbon dioxide to produce ethylene.

[0012] Preferably, in step (1), the copper salt is Cu(NO3)2·3H2O, the manganese salt is MnCl2·4H2O, and the concentrations of Cu(NO3)2·3H2O and MnCl2·4H2O in deionized water are both 0.3 mol / L.

[0013] Preferably, in step (2), the concentration of the NaOH solution used is 5 mol / L.

[0014] Preferably, in step (3), the hydrothermal reaction temperature is 80° C. and the reaction time is 24 h.

[0015] It is further preferred that in step (3), the drying condition is drying at 60° C. for 11-13 h.

[0016] It is further preferred that in step (3), the frequency of ultrasonic treatment is 40 kHz and the treatment time is 12 h.

[0017] The CuMnO2-V prepared by the above method o The catalyst is used as a catalyst for the electrocatalytic reduction of carbon dioxide to produce ethylene, and can be used as a catalyst for the direct and efficient conversion of flue gas CO2 into ethylene.

[0018] Compared with the prior art, the present invention is beneficial in that:

[0019] (1) Studies have shown that the composition and properties of defective two-dimensional manganese-based nanomaterials are crucial to controlling the catalytic active centers of CO2 RR; the existing structural defects can improve the catalytic activity by increasing the number of active sites. The CuMnO2 material prepared by the present invention, as a two-dimensional manganese-based nanomaterial, presents a layered structure composed of edge-sharing twisted [MnO6] octahedral clusters and linear binary [CuO2], and the surface oxygen vacancy concentration of the CuMnO2 nanosheet catalyst is modified based on the room temperature modulated radio frequency plasma method to form a high concentration of oxygen vacancies. The presence of oxygen vacancies can destroy its stable structure and improve the catalytic activity.

[0020] (2) Another effect of using the room temperature modulated RF plasma method is to use the oxygen vacancy concentration on the CuMnO2 surface to regulate the d-band center of the metal at the active site of the catalyst, thereby strengthening the adsorption and CC coupling reaction of the intermediate state *CO in the carbon dioxide electroreduction to ethylene, thereby improving the selectivity of carbon dioxide electroreduction to ethylene and further enhancing the catalytic activity.

[0021] (3) Since layered CuMnO2 two-dimensional nanosheets are prone to curling and stacking, the present invention uses a template to open holes in the vertically erected two-dimensional nanosheets, thereby inhibiting the curling and stacking of the layered CuMnO2 two-dimensional nanosheets and enhancing the structural stability of the two-dimensional material.

[0022] (4) Oxygen-rich CuMnO2-V was prepared by hydrothermal + plasma treatment. o The catalyst has a simple preparation process, low cost, high activity for electrocatalytic CO2 RR, high Faraday efficiency of the specific product ethylene, and is suitable for industrial production.

[0023] (5) The two-dimensional manganese-based nanosheets prepared by the present invention are used for the electrocatalytic reduction of CO2 reaction. The catalytic activity of the catalyst is significantly improved compared with that of the unactivated catalyst. At room temperature, the starting potential is -0.5 V vs. RHE and the current density is -14.57 mA cm 2 The ethylene Faraday efficiency was 93.4% (at -1.0 V vs. RHE), which was significantly improved compared with the conventional CuMnO2 catalyst. The 192h stability evaluation showed that after 192h of reaction, the ethylene Faraday efficiency of the catalyst only decreased by 7.8% (from 93.4% to 85.6%).

[0024] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1The Faraday efficiency of the catalyst prepared in Example 1 in electrocatalyzing methane production at different potentials.

[0026] Figure 2 The Faraday efficiency of the catalyst prepared in Example 2 in electrocatalyzing methane production at different potentials.

[0027] Figure 3 This is a stability test chart of CuMnO2-Vo catalyzing carbon dioxide to ethylene.

[0028] Figure 4 The XRD spectra of the catalysts prepared in Example 1 and Example 2. DETAILED DESCRIPTION

[0029] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0030] Example 1

[0031] A catalyst is prepared by the following steps:

[0032] 3.6g of Cu(NO3)2·3H2O and 3.0g of MnCl2·3H2O were dissolved in 50ml of deionized water and stirred magnetically for 30 minutes to obtain solution A; 1.727g of polyvinylpyrrolidone K30 (PVP) was dissolved in 50ml of deionized water to obtain solution B; 20ml of 5mol / L NaOH solution was added to solution A, and then solution B was slowly added dropwise to solution A and stirred at room temperature for 30 minutes to obtain a mixed slurry. The mixed slurry was transferred to a polytetrafluoroethylene (PTFE) container and heated at 80℃ for 24 hours to obtain a supernatant and a precipitate. The supernatant and the precipitate were ultrasonicated at 40kHz for 12 hours to obtain a black solution; the black solution was centrifuged, the solid was washed, and the solid was dried at 60℃ overnight; the dried solid was placed in a muffle furnace, calcined at 600℃ for 3 hours, and naturally cooled to room temperature to obtain a black powder, namely CuMnO2.

[0033] Example 2

[0034] A preparation method for a catalyst for electrocatalytic reduction of carbon dioxide to produce ethylene, comprising the following steps:

[0035] The black powder CuMnO2 prepared in Example 1 was placed in a radio frequency plasma device for treatment at a power of 250 W in an oxygen atmosphere at room temperature cold plasma for 10 minutes to obtain a two-dimensional nanosheet CuMnO2-V o catalyst.

[0036] Example 3 and Example 4

[0037] Compared with Example 2, the difference is that the plasma treatment power is changed, and other conditions remain unchanged. The plasma treatment power of Example 3 is adjusted to 50W to obtain the catalyst CuMnO2-V o The plasma treatment power of Example 4 was adjusted to 150W to obtain the catalyst CuMnO2-V o .

[0038] Research has found that when the power is greater than 250W, the structure of the catalyst will be severely damaged and the performance will be reduced. Therefore, the power cannot exceed 250W.

[0039] Example 5 and Example 6

[0040] Compared with Example 2, the difference is that the plasma treatment time is different, and other conditions remain unchanged. The plasma treatment time of Example 5 is 5 minutes. The plasma treatment time of Example 6 is 15 minutes.

[0041] Example 7

[0042] A catalyst is prepared by the following steps:

[0043] 3.6g of Cu(NO3)2·3H2O and 3.0g of MnCl2·3H2O were dissolved in 50ml of deionized water and stirred magnetically for 30 minutes to obtain solution A; 20ml of 5mol / L NaOH solution was added to solution A; solution A was transferred to a polytetrafluoroethylene (PTFE) container and heated at 80℃ for 24 hours to obtain a supernatant and a precipitate, and the supernatant and the precipitate were ultrasonicated at 40kHz for 12 hours to obtain a black solution; the black solution was centrifuged, the solid was washed, and the solid was dried at 60℃ overnight; the dried solid was placed in a muffle furnace, calcined at 600℃ for 3 hours, and naturally cooled to room temperature to obtain a black powder. The black powder was placed in a radio frequency plasma device for treatment, and treated at a power of 250W for 10 minutes in an oxygen atmosphere room temperature cold plasma to obtain a catalyst.

[0044] The performance tests of the catalysts prepared in each example are as follows:

[0045] (1) Evaluation of catalytic activity of catalysts

[0046] The electrochemical measurements of the catalysts were performed in a standard three-electrode system using a 0.1 M KHCO3 CO2 saturated solution electrolyte (298 K, pH = 6.8) in a sealed two-chamber electrochemical cell (Nafion-212 membrane). A platinum foil was used as the counter electrode with an area of ​​0.07 cm -2The glassy carbon electrode was used as the working electrode and the calomel electrode was used as the reference electrode. The electrochemical workstation was CHI-660E. The catalyst activity was evaluated by cyclic voltammetry (CV) and linear sweep voltammetry (LSV). The electrochemical impedance spectroscopy was performed in the frequency range of 1-105 Hz, with a potential of -1.0 V vs. RHE and an amplitude of 5 mV.

[0047] Catalyst product evaluation was performed by using a chromatograph (SC-3000B) equipped with a TDX01 molecular sieve column to detect gaseous products. Liquid products were analyzed using a mixture of 0.1 mL of D2O and 0.05 mL of dimethyl sulfoxide as an internal standard solution. This solution was then mixed with 0.1 mL of electrolyte for nuclear magnetic resonance detection after the electrolysis reaction.

[0048] The processing parameters and catalytic activity evaluation of the catalysts prepared in each embodiment are shown in Table 1. It can be seen from Table 1 that the starting potential of the catalyst prepared in Example 2 is the smallest. The smaller the starting potential, the better the catalytic activity of the catalyst. Therefore, it is determined that the catalyst prepared in Example 2 has the best catalytic activity. Furthermore, the greater the current density, the better the catalytic activity. The current density of the catalyst in Example 2 is the largest, which also proves that the catalyst activity in Example 2 is the best. Therefore, the double-layer capacitance, overpotential and stability of the catalyst in Example 2 were further tested. Because the catalytic activity of the catalysts in other embodiments is lower than that in Example 2, there is no need to further test the double-layer capacitance, overpotential and stability. "—" in Table 1 indicates data that has not been tested.

[0049] The Faraday efficiencies of the catalysts prepared in Example 1 and Example 2 for electrocatalytic methane production at different potentials are as follows: Figure 1 and Figure 2 At -1.0 V vs. RHE, after 192 h of continuous electrocatalytic reaction of carbon dioxide to ethylene using the catalyst of Example 2, the Faraday efficiency of the ethylene product remained at 85.6%, which was only 7.8% lower than the initial value. Figure 3 shown.

[0050] The evaluation results of the catalyst products of Example 1 and Example 2 (at -1.0 V vs. RHE) are shown in Table 2.

[0051] Table 1. Processing parameters and catalytic activity evaluation of catalysts prepared in various examples

[0052]

[0053] Table 2. Evaluation results of catalyst products of Example 1 and Example 2

[0054] Example Catalyst name <![CDATA[FE(H2)]]> FE(CO) FE(HCOOH) <![CDATA[FE(CH3OH)]]> <![CDATA[FE(CH3CH2OH)]]> <![CDATA[FE(C2H4)]]> 1 <![CDATA[CuMnO2]]> 18.8 1.9 35.8 30.6 0.3 12.3 2 <![CDATA[CuMnO2-V o ]]> 1.1 0.3 1.5 2.1 1.5 93.4

[0055] (2) XRD characterization

[0056] The XRD spectra of the catalysts prepared in Example 1 and Example 2 are as follows: Figure 4 As shown in the figure, it can be seen that the activation with O2 cold plasma produces abundant oxygen vacancy defects in the crystal structure, CuMnO2-V o The XRD characteristic diffraction peak pattern of CuMnO2 is consistent with the diffraction peak pattern of CuMnO2 (PDF#50-0860), indicating that the lattice structure has not been significantly damaged after O2 plasma treatment. o The diffraction peak intensity of the catalyst decreased significantly, indicating that the potential had changed. Further study of the crystal structure found that CuMnO2 and CuMnO2-V o The Rietveld refinement results are in good agreement with the monoclinic C2 / m space group symmetry of CuMnO2. o The lattice parameters a, b, c (5.579, 2.865, ) is smaller than the lattice parameters of CuMnO2 (5.585, 2.884, ), indicating that CuMnO2-V o The atomic arrangement and lattice space have changed.

[0057] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a catalyst for electrocatalytic reduction of carbon dioxide to ethylene, It is characterized in that The following steps are involved: (1) Weigh equimolar amounts of water-soluble copper salt and manganese salt, add deionized water, and stir until completely dissolved to obtain a light blue solution A; dissolve polyvinyl pyrrolidone K30 in deionized water to obtain a colorless and transparent solution B; (2) Adding NaOH solution to solution A to adjust the pH of the solution to 7-9, then adding solution B dropwise to solution A, stirring for 30 min to obtain a mixed slurry, and continuing to stir for 30 min; (3) subjecting the mixed slurry obtained in step (2) to a hydrothermal reaction at a temperature of 50 to 120°C for 12 to 36 hours until a black precipitate and a supernatant are obtained; subjecting the black precipitate and the supernatant to an ultrasonic treatment to obtain a black solution; The black solution is centrifuged, washed, and dried to obtain a black powder; (4) The black powder is placed in a radio frequency plasma device for treatment, and the plasma treatment atmosphere is O 2 , treated with 250W power for 10min, and CuMnO 2 -V o The catalyst is a catalyst for the electrocatalytic reduction of carbon dioxide to produce ethylene.

2. The method for preparing the catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that In step (3), the frequency of ultrasonic treatment is 40 kHz and the treatment time is 12 h.

3. The method for preparing the catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that In step (3), the hydrothermal reaction temperature is 80° C. and the reaction time is 24 h.

4. The method for preparing the catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that In step (3), the drying condition is drying at 60° C. for 11-13 h.

5. The method for preparing the catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide according to claim 1, It is characterized in that In step (1), the copper salt is Cu(NO 3 ) 2 ·3H 2 O, manganese salt is MnCl 2 ·4H 2 O, Cu(NO 3 ) 2 ·3H 2 O and MnCl 2 ·4H 2 The concentration of O in deionized water was 0.3 mol / L.

6. The method for preparing the catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide according to claim 4, It is characterized in that In step (2), the concentration of the NaOH solution used is 5 mol / L.

7. A catalyst for electrocatalytic reduction of carbon dioxide to produce ethylene, It is characterized in that The method is prepared by any one of claims 1 to 6.

8. Use of the catalyst for preparing ethylene by electrocatalytic reduction of carbon dioxide as claimed in claim 7, It is characterized in that The catalyst is used as a catalyst for electrocatalytic reduction of carbon dioxide to produce ethylene.

Citation Information

Cited By

  • Ultrasonic synthesis non-noble metal-based MOF (Metal Organic Framework) catalyst as well as preparation method and application thereof

    CN120424355A