Catalytic cracking method and cracking catalyst of phosphorus-containing modified ZSM-5 molecular sieve

By using a solid phosphorus-containing compound modified ZSM-5 molecular sieve with a valence of +3 of phosphorus, the problem of self-polymerization of phosphoric acid-modified ZSM-5 molecular sieve under high temperature hydrothermal conditions was solved, and the cracking conversion rate of the catalytic cracking reaction was improved and low carbon olefin yields, the catalyst's high-efficiency hydrothermal stability and activation performance are achieved.

CN119220292AActive Publication Date: 2024-12-31CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310783180.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-29
Publication Date
2024-12-31
Estimated Expiration
2043-06-29

AI Technical Summary

Technical Problem

Existing ZSM-5 molecular sieve modified with phosphoric acid or ammonium phosphate can easily cause the self-agglomeration of phosphorus species under high temperature hydrothermal conditions, blocking pores, reducing pore volume and specific surface area, resulting in low activation efficiency of phosphorus aluminum and unable to effectively improve hydrothermal stability. and low-carbon olefin selectivity.

Method used

The solid phosphorus-containing compound with a valence of +3 valence as a precursor is used to prepare a phosphorus-modified ZSM-5 molecular sieve. Through specific impregnation and hydrothermal aging treatment, the stable efficiency and crystallization retention of phosphorus aluminum are improved, and the crystallization retention of phosphorus aluminum is formed to form excellent water. Catalysts for thermal stability and cleavage activity.

Benefits of technology

The cracking conversion rate and low-carbon olefin yield in the catalytic cracking reaction are improved, the liquefied gas yield is high, and the activation efficiency of phosphorus aluminum is significantly improved, and the catalytic performance is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119220292A_ABST
    Figure CN119220292A_ABST
Patent Text Reader

Abstract

The invention relates to a catalytic cracking catalyst which is characterized by comprising the following components in percentage by weight: 2-20% of a Y-type molecular sieve (calculated as a dry base), 3-80% of a phosphorus modified ZSM-5 molecular sieve (calculated as a dry base), 1-70% of an inorganic binder (calculated as a dry base) and 2-60% of clay (calculated as a dry base) on the basis of the dry base weight of the catalytic cracking catalyst, after the phosphorus-modified ZSM-5 molecular sieve is subjected to hydrothermal aging for 17 hours under the conditions of 800 DEG C and 100% water vapor, the electron binding energy of phosphorus in phosphorus species on the surface of the molecular sieve is 135.2 eV, the crystal retention degree in XRD analysis is 70%-110%, and the inorganic binder comprises a phosphorus-aluminum inorganic binder and / or other inorganic binders.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cracking method and a cracking catalyst, and more particularly to a catalytic cracking method and a cracking catalyst containing a Y-type molecular sieve and a phosphorus-modified ZSM-5 molecular sieve. Background Art

[0002] The cracking reaction of hydrocarbons at high temperature converts long-chain hydrocarbons into high-value-added low-carbon olefins such as ethylene and propylene. ZSM-5 molecular sieve is a medium-pore molecular sieve with high silicon three-dimensional straight channels and MFI structure developed by Mobil Oil Company of the United States (USP3702886). Its unique pore structure gives it good shape-selective catalytic and isomerization performance. It also has high thermal and hydrothermal stability, high specific surface area, wide range of silicon-aluminum ratio, unique surface acidity and low carbon deposition. ZSM-5 molecular sieve is widely used as a catalyst and catalyst carrier, and has been successfully used in production processes such as alkylation, isomerization, disproportionation, catalytic cracking, methanol to gasoline, and methanol to olefins.

[0003] Since 1983, ZSM-5 molecular sieve has been used in catalytic cracking process as a catalytic cracking octane number aid, aiming to improve the octane number of catalytic cracking gasoline and the selectivity of light olefins. US3758403 first reported the use of ZSM-5 as an active component for increasing propylene production, that is, ZSM-5 and REY were used together as active components to prepare FCC catalysts. US5997728 discloses the use of ZSM-5 molecular sieve as an aid for increasing propylene production, and the molecular sieve is not modified in any way. The propylene yield of the above two technologies is not high. Although HZSM-5 molecular sieve has good shape selectivity and isomerization performance, its disadvantage is poor hydrothermal stability and easy deactivation under harsh high-temperature hydrothermal conditions, which reduces the catalytic performance.

[0004] In the 1980s, Mobil Corporation discovered that phosphorus can improve the hydrothermal stability of ZSM-5 zeolite. At the same time, after phosphorus modification of ZSM-5 zeolite, primary cracking products (such as gasoline olefins) can be selectively converted into C3 and C4 olefins, thereby increasing the yield of low-carbon olefins.

[0005] CN 1211469A discloses a five-membered ring molecular sieve composition for producing more propylene and ethylene, which is composed of 85-95% by weight of five-membered ring molecular sieve, 2-10% by weight of phosphorus calculated as oxide, 0.3-5% by weight of alkaline earth metal calculated as oxide, and 0.3-5% by weight of transition metal element calculated as oxide. The composition is used for catalytic thermal cracking reaction to obtain a higher ethylene yield.

[0006] US5171921 discloses a phosphorus-modified ZSM-5 molecular sieve having a silicon-aluminum ratio of 20-60. After being impregnated with a phosphorus-containing compound and treated with steam at 500-700°C, it has higher activity when used for the reaction of converting C3-C20 hydrocarbons into C2-C5 olefins than HZSM-5 that is not treated with phosphorus.

[0007] CN102166533A discloses a method for preparing a phosphorus-modified ZSM-5 molecular sieve, which comprises adding the molecular sieve to a phosphorus-containing aqueous solution, reacting for a period of time at a certain pH value, temperature and pressure, and then filtering, drying and calcining to obtain the phosphorus-modified molecular sieve; then adding the phosphorus-modified molecular sieve to an aqueous solution containing rare earth ions, reacting for a period of time at a certain temperature and pressure, and then filtering, washing, drying and calcining to obtain a composite modified molecular sieve. The composite modified molecular sieve is used to prepare a model catalyst, which has higher hydrothermal stability and micro-activity than the unmodified molecular sieve model catalyst and the molecular sieve model catalyst modified by other methods.

[0008] CN106994364A discloses a method for preparing a phosphorus-modified ZSM-5 molecular sieve, which comprises first mixing one or more phosphorus-containing compounds selected from phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate with a ZSM-5 molecular sieve having a high alkali metal ion content to obtain a mixture having a phosphorus loading of at least 0.1 wt% in terms of P2O5, drying and roasting the mixture, and then performing an ammonium crosslinking step and a water washing step to reduce the alkali metal ion content therein to below 0.10 wt%, and then undergoing drying and hydrothermal aging steps at 400-1000°C and 100% water vapor. The phosphorus-containing ZSM-5 molecular sieve obtained by the preparation method has a high total acid content, excellent cracking conversion rate and propylene selectivity, and also has a high liquefied gas yield.

[0009] Although the modification of ZSM-5 molecular sieves with organic / inorganic phosphorus compounds can inhibit framework dealumination and thus improve hydrothermal stability, the introduction of phosphorus species also has the effect of regulating the properties of the acid center of the ZSM-5 molecular sieve, thereby improving the cracking conversion rate of long-chain alkanes and the selectivity of light olefins, phosphoric acid or ammonium phosphate will self-polymerize due to dehydration to form large molecular phosphorus species such as polyphosphoric acid, which are easily enriched on the outer surface of the molecular sieve, blocking the pores, reducing the pore volume and specific surface area, resulting in a low phosphorus-aluminum activation efficiency. After phosphorus modification, the ideal effect of improving hydrothermal stability cannot be achieved. Summary of the invention

[0010] Based on a large number of experiments, the inventors found that the phosphorus-modified ZSM-5 molecular sieve prepared using a solid phosphorus-containing compound with a phosphorus valence of +3 as a precursor has physicochemical characteristics different from those of the molecular sieve prepared by the conventional +5-valent phosphorus source aqueous solution impregnation method, and can improve the phosphorus-aluminum stabilization efficiency. The hydrothermal stability, cracking activity and low-carbon olefin selectivity of the ZSM-5 molecular sieve modified in this way are improved.

[0011] One of the purposes of the present invention is to provide a catalytic cracking method, in which one of the active components of the catalyst used in the method is a phosphorus-modified ZSM-5 molecular sieve having physicochemical characteristics different from those of conventional phosphorus-containing ZSM-5 molecular sieves and having improved phosphorus-aluminum stabilization efficiency of the molecular sieve, and the method has high cracking conversion rate and low-carbon olefin yield, and high liquefied gas yield in the catalytic cracking reaction of hydrocarbon oil; the second purpose is to provide a cracking catalyst used in the cracking method.

[0012] In order to achieve one of the above-mentioned purposes, a catalytic cracking method is provided in a first aspect of the present invention, wherein hydrocarbon oil is contacted with a cracking catalyst under catalytic cracking reaction conditions, the cracking catalyst containing, based on the dry weight of the cracking catalyst, 2-20% of a Y-type molecular sieve, 3-80% of a phosphorus-modified ZSM-5 molecular sieve, 1-70% of an inorganic binder, and 2-60% of clay on a dry basis, characterized in that the phosphorus-modified ZSM-5 molecular sieve is modified with a phosphorus-containing compound having a phosphorus valence state of +3, and the phosphorus-modified ZSM-5 molecular sieve has an electron binding energy of 135.2 eV in phosphorus species on the surface of the molecular sieve after hydrothermal aging at 800°C and 100% water vapor for 17 hours, and a crystal retention degree of 70% to 110% in XRD analysis.

[0013] In order to achieve the second purpose mentioned above, the second aspect of the present invention provides a cracking catalyst, which contains, based on the dry weight of the cracking catalyst, 2-20% of Y-type molecular sieve, 3-80% of phosphorus-modified ZSM-5 molecular sieve, 1-70% of inorganic binder and 2-60% of clay on a dry basis, characterized in that the phosphorus-modified ZSM-5 molecular sieve is modified with a phosphorus-containing compound with a phosphorus valence state of +3, and the phosphorus-modified ZSM-5 molecular sieve has an electron binding energy of 135.2 eV in phosphorus species on the surface of the molecular sieve after hydrothermal aging at 800°C and 100% water vapor for 17 hours, and a crystal retention degree of 70% to 110% in XRD analysis.

[0014] The catalytic cracking method provided by the present invention comprises a phosphorus-modified ZSM-5 molecular sieve with special physicochemical parameters, wherein the phosphorus-modified ZSM-5 molecular sieve is obtained by selecting a +3-valent phosphorus source for modification; after hydrothermal aging at 800°C and 100% water vapor for 17 hours, the catalyst has a higher crystal retention degree, i.e., has excellent hydrothermal stability; and the method has the characteristics of high cracking conversion rate, low-carbon olefin yield, and high liquefied gas yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is the XPS (P2p Scan) spectrum of the phosphorus-modified ZSM-5 molecular sieve sample in the present invention. DETAILED DESCRIPTION

[0016] The catalytic cracking method provided by the present invention is to contact and react hydrocarbon oil with a cracking catalyst under catalytic cracking reaction conditions, and the cracking catalyst contains 2-20% of Y-type molecular sieve on a dry basis, 3-80% of phosphorus-modified ZSM-5 molecular sieve on a dry basis, 1-70% of inorganic binder on a dry basis and 2-60% of clay on a dry basis based on the dry basis weight of the cracking catalyst. The method is characterized in that the phosphorus-modified ZSM-5 molecular sieve is modified with a phosphorus-containing compound with a phosphorus valence state of +3, and after hydrothermal aging for 17 hours at 800°C and 100% water vapor conditions, the electron binding energy of the phosphorus element in the phosphorus species on the surface of the molecular sieve is 135.2eV, and the crystal retention degree in XRD analysis is 70% to 110%.

[0017] In the method of the present invention, the cracking catalyst is used alone, or the cracking catalyst is used in a mixture with a conventional cracking catalyst, in which the cracking catalyst accounts for no more than 30% by weight of the total amount of the mixture, preferably 1-25% by weight, and more preferably 3-15% by weight. The conventional cracking catalyst is well known to those skilled in the art, and is mainly a cracking catalyst with Y-type molecular sieve as the main active component, which will not be described in detail here.

[0018] In the cracking catalyst used in the method of the present invention, the Y-type molecular sieve is at least one selected from PSRY molecular sieve, PSRY-S molecular sieve, PSRY molecular sieve containing rare earth, PSRY-S molecular sieve containing rare earth, USY molecular sieve, USY molecular sieve containing rare earth, REY molecular sieve, REHY molecular sieve and HY molecular sieve.

[0019] In the cracking catalyst used in the method of the present invention, the phosphorus-modified ZSM-5 molecular sieve has a phosphorus binding energy of 134.5 eV characterized by XPS after drying at 100-120°C in an air atmosphere during the preparation process; after hydrothermal aging at 800°C and 100% water vapor, the phosphorus binding energy is 135.2 eV. The phosphorus-modified molecular sieve in the prior art has almost no valence state transition, so the binding energy after drying and aging is 134.8-134.9 eV. The phosphorus binding energy characterized by XPS represents its chemical environment and valence state, and can explain the degree of polycondensation and valence state transition of phosphorus species during drying and hydrothermal aging.

[0020] Furthermore, in the cracking catalyst used in the method of the present invention, the phosphorus-modified ZSM-5 molecular sieve has a higher crystal retention (70% to 110%) after hydrothermal aging at 800°C and 100% water vapor for 17 hours, which also shows that the phosphorus species has a significant coordination effect with the framework aluminum, so that the framework aluminum is fully protected and the molecular sieve has excellent hydrothermal stability.

[0021] In the cracking catalyst used in the method of the present invention, the phosphorus-modified ZSM-5 molecular sieve has a molar ratio of phosphorus to aluminum of 0.01 to 5, preferably 0.1 to 3.

[0022] In the cracking catalyst used in the method of the present invention, the phosphorus-modified ZSM-5 molecular sieve is obtained by mixing and grinding a solid phosphorus-containing compound precursor with a phosphorus valence state of +3 and a HZSM-5 molecular sieve to obtain a solid phase mixture; the solid phase mixture is subjected to a heating and melting treatment; the heated and melted solid phase mixture is cooled to room temperature, such as 20-25°C, and then subjected to a roasting treatment to obtain the phosphorus-modified ZSM-5 molecular sieve; or the HZSM-5 molecular sieve is contacted and impregnated with an aqueous solution of a phosphorus-containing compound with a phosphorus valence state of +3, and then dried and roasted. The impregnation is carried out at a water-to-sieve weight ratio of 0.5 to 2 at room temperature for 0.5 to 10 hours; the drying is carried out in an atmosphere of air at 100 to 120°C for 2 to 24 hours; the roasting is carried out in an atmosphere of air at 200 to 800°C for 0.5 to 12 hours. The heating and melting treatment has a temperature higher than the melting point of the solid phosphorus-containing compound and lower than the temperature at which the solid phosphorus-containing compound decomposes or dehydrates, and the treatment time is 2 to 72 hours. The solid phosphorus-containing compound precursor with a phosphorus valence of +3 is selected from phosphorous acid and / or ammonium phosphite. The molar ratio of the phosphorus-containing compound precursor with a phosphorus valence of +3 to the HZSM-5 molecular sieve is (0.1 to 5):1, preferably (0.5 to 2.5):1, wherein the HZSM-5 molecular sieve is calculated in terms of aluminum and the phosphorus-containing compound is calculated in terms of phosphorus. The HZSM-5 molecular sieve is obtained by reducing the sodium content of the ZSM-5 molecular sieve to Na2O <0.1wt% through ammonium exchange, and the silicon-aluminum ratio (molar ratio of silicon oxide to aluminum oxide, the same below) ranges ≥10, usually 10 to 200.

[0023] Regarding the phosphorus-modified ZSM-5 molecular sieve in the catalyst of the present application, the present application also introduces the contents of the Chinese invention application with application number 202210899906.6 and application date July 28, 2022 for reference.

[0024] In the cracking catalyst used in the method of the present invention, preferably, the Y-type molecular sieve and the phosphorus-modified ZSM-5 molecular sieve account for 6-85% weight of the catalyst dry basis. Further, the Y-type molecular sieve on a dry basis accounts for 3-15% weight of the catalyst dry basis, and the phosphorus-modified molecular sieve on a dry basis accounts for 5-75% weight of the catalyst dry basis. More preferably, the weight ratio of the Y-type molecular sieve to the phosphorus-modified ZSM-5 molecular sieve is 1:(0.25-40).

[0025] In the cracking catalyst used in the method of the present invention, the inorganic binder includes a phosphorus-aluminum inorganic binder, and the phosphorus-aluminum inorganic binder is 5-40% by weight based on the dry basis of the catalyst. Based on the dry basis weight of the phosphorus-aluminum inorganic binder, the phosphorus-aluminum inorganic binder includes 15-40% by weight of aluminum component based on Al2O3, 45-80% by weight of phosphorus component based on P2O5, and its P / Al weight ratio is 1.0-6.0, the pH value is 1-3.5, and the solid content is 15-60% by weight; for example, it includes 15-40% by weight of aluminum component based on Al2O3 and 45-80% by weight of phosphorus component based on P2O5; preferably, it contains 15-35% by weight of aluminum component based on Al2O3 and 50-75% by weight of phosphorus component based on P2O5, and its P / Al weight ratio is preferably 1.2-6.0, more preferably 2.0-5.0, and the pH value is preferably 1.5-3.0. Preferably, the phosphate-aluminum inorganic binder comprises, based on the dry weight, 20-40 wt% of aluminum component in terms of Al2O3 and 60-80 wt% of phosphorus component in terms of P2O5.

[0026] The phosphate-aluminum inorganic binder can be prepared by the following steps: alumina source, clay (such as rectorite, kaolin) and water are slurried and dispersed into a slurry with a solid content of 5-50% by weight; wherein the alumina source is aluminum hydroxide and / or aluminum oxide (such as pseudo-boehmite, SB powder, γ-alumina) that can be colloided by acid, relative to 15 to 50 parts by weight of the alumina source calculated as Al2O3; concentrated phosphoric acid is added to the slurry at a weight ratio of P / Al=1-6 under stirring, and the resulting mixed slurry is reacted at 50-99°C for 15-90 minutes; wherein P in P / Al is the weight of phosphorus in phosphoric acid as a single substance, and Al is the weight of aluminum in the alumina source as a single substance.

[0027] The inorganic binder may further contain at least one selected from pseudo-boehmite, alumina sol, silica-alumina sol and water glass.

[0028] In the cracking catalyst used in the method of the present invention, the clay is well known to those skilled in the art, and the clay can be at least one selected from kaolin, sepiolite, attapulgite, rectorite, montmorillonite and diatomite, preferably kaolin, metakaolin and rectorite. Based on the dry weight of the catalytic cracking catalyst, it contains 2-60% by weight of clay on a dry basis, preferably 5-55% by weight of clay, and more preferably 15-40% by weight of clay.

[0029] Preparation process of catalyst. In a specific preparation embodiment of the catalyst of the present invention, an inorganic binder (such as pseudo-boehmite, aluminum sol, silica sol, silica-alumina gel or a mixture of two or more thereof) can be mixed with clay (such as kaolin) and water (such as deionized water and / or deionized water) to form a slurry with a solid content of 10 to 50% by weight, stirred evenly, and the slurry pH is adjusted to 1 to 4 with an inorganic acid such as hydrochloric acid, nitric acid, phosphoric acid or sulfuric acid, and the pH value is maintained. After aging at 20 to 80° C. for 0 to 2 hours, such as 0.3 to 2 hours, aluminum sol and / or silica sol are added, stirred for 0.5 to 1.5 hours to form a colloid, and then a molecular sieve is added, the molecular sieve includes the phosphorus-modified ZSM-5 molecular sieve and Y-type molecular sieve, to form a catalyst slurry, the solid content of the catalyst slurry is, for example, 20 to 45 weight%, and the stirring is continued and then spray-dried to form a microsphere catalyst. The microsphere catalyst is then calcined, for example, at 350-650°C or 400-600°C, preferably 450-550°C, for 0.5-6 hours or 0.5-2 hours, and then washed with ammonium sulfate (wherein the washing temperature can be 40-70°C, ammonium sulfate: microsphere catalyst: water = 0.2-0.8:1:5-15 weight ratio) until the sodium oxide content is less than 0.25% by weight, washed with water and filtered, and then dried.

[0030] In another specific preparation embodiment of the catalyst of the present invention, the Y-type molecular sieve and the phosphorus-modified ZSM-5 molecular sieve, the phosphorus-aluminum inorganic binder and other inorganic binders can be mixed, clay is added, slurried, and spray-dried.

[0031] The present invention also provides a cracking catalyst used in the above-mentioned catalytic cracking of hydrocarbon oil. Based on the dry weight of the cracking catalyst, the cracking catalyst contains 2-20% of Y-type molecular sieve on a dry basis, 3-80% of phosphorus-modified ZSM-5 molecular sieve on a dry basis, 1-70% of inorganic binder on a dry basis and 2-60% of clay on a dry basis. The invention is characterized in that the phosphorus-modified ZSM-5 molecular sieve is modified with a phosphorus-containing compound with a phosphorus valence state of +3. After hydrothermal aging of the phosphorus-modified ZSM-5 molecular sieve at 800°C and 100% water vapor for 17 hours, the electron binding energy of the phosphorus element in the phosphorus species on the surface of the molecular sieve is 135.2 eV, and the crystal retention in XRD analysis is 70% to 110%.

[0032] When the cracking catalyst is used in the catalytic cracking process, the catalyst can be added to the catalytic cracking reactor alone, for example, under catalytic cracking conditions, hydrocarbon oil is contacted with the catalytic cracking catalyst of the present invention for reaction; or, the cracking catalyst can be used in a mixture with other cracking catalysts, and the catalytic cracking catalyst of the present invention can account for no more than 30% by weight of the total amount of the above mixture, preferably 1-25% by weight, and more preferably 3-15% by weight. In the cracking method provided by the present invention, the raw material can be various hydrocarbon oils. The hydrocarbon oil can be selected from various petroleum fractions, such as crude oil, naphtha, catalytic gasoline, atmospheric residue, vacuum residue, atmospheric wax oil, vacuum wax oil, straight run wax oil, propane light / heavy deoiling, coking wax oil and coal liquefaction products. The hydrocarbon oil can contain heavy metal impurities such as nickel and vanadium and sulfur and nitrogen impurities, such as the sulfur content in the hydrocarbon oil can be as high as 3.0% by weight, the nitrogen content can be as high as 2.0% by weight, and the content of metal impurities such as vanadium and nickel can be as high as 3000ppm.

[0033] In the hydrocarbon oil catalytic cracking method of the present invention, the catalytic cracking conditions may be conventional in the art, preferably including: a reaction temperature of 500 to 800°C, such as 550 to 680°C.

[0034] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] X-ray diffraction (XRD) spectra were measured on a Rigaku TTR-3 powder X-ray diffractometer. Instrument parameters: copper target (tube voltage 40 kV, tube current 250 mA), scintillation counter, step width 0.02°, scanning rate 0.4 (°) / min. The ZSM-5 molecular sieve synthesized by the method of Example 1 in CN1056818C was used as a standard sample, and its crystallinity was set to 100%. The relative crystallinity is expressed as a percentage of the sum of the peak areas of the five characteristic diffraction peaks at 2θ between 22.5 and 25.0° of the X-ray diffraction spectra of the obtained product and the standard sample.

[0036] X-ray photoelectron spectroscopy (XPS) was used to analyze the molecular sieve surface and examine the migration of phosphorus compounds using the ESCALAB 250 X-ray photoelectron spectrometer from Thermo Fisher-VG. Instrument parameters: The excitation source was monochromatic AlKα X-ray with a power of 150 W, and the charge shift was corrected using the C1s peak (284.8 eV) from contaminated carbon.

[0037] Unless otherwise specified, the instruments and reagents used in the embodiments of the present invention are commonly used by those skilled in the art.

[0038] The properties of some of the raw materials used in the examples are as follows:

[0039] Pseudo-boehmite is an industrial product produced by Shandong Aluminum Company, with a solid content of 60% by weight.

[0040] Alumina sol is an industrial product produced by Sinopec Catalyst Qilu Branch, with an Al2O3 content of 21.5% by weight.

[0041] Silica sol is an industrial product produced by Sinopec Catalyst Qilu Branch, with a SiO2 content of 28.9% by weight and a Na2O content of 8.9%.

[0042] The kaolin was kaolin for catalytic cracking catalyst produced by Suzhou Kaolin Company, with a solid content of 78% by weight. The rectorite was produced by Hubei Zhongxiang Mingliu Rectorite Development Co., Ltd., with a quartz sand content of <3.5% by weight, an Al2O3 content of 39.0% by weight, a Na2O content of 0.03% by weight, and a solid content of 77% by weight.

[0043] SB aluminum hydroxide powder, produced by Condex, Germany, has an Al2O3 content of 75% by weight.

[0044] HRY molecular sieve is an industrial product produced by Sinopec Catalyst Changling Branch, with a rare earth content of 10% by weight.

[0045] PSRY molecular sieve is an industrial product produced by Sinopec Catalyst Changling Branch, with a Na2O content of <1.5% by weight, a P2O5 content of 0.8-1.2% by weight, a unit cell constant of <2.456nm, and a crystallinity of ≥64%.

[0046] Unless otherwise specified, the instruments and reagents used in the embodiments of the present invention are commonly used by those skilled in the art.

[0047] Examples 1-6 illustrate the phosphorus-modified ZSM-5 molecular sieve used in the catalyst of the present invention and its preparation.

[0048] Example 1

[0049] Take 10.8g of solid phosphorous acid and add it to 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30). After grinding and mixing for 0.5h, transfer it to a Teflon-lined stainless steel high-pressure reactor for a melting process with a heating temperature of 100°C and a time of 10h. After the melting process, wait for the sample to naturally cool to room temperature and then take it out; the above sample is calcined at 550°C for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve sample, recorded as RYB-1.

[0050] Example 1-1

[0051] Take 10.8g of solid phosphorous acid and dissolve it in 145g of deionized water at 25°C, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25°C for 0.5h, move it to an oven and dry it at 120°C for 12h, and calcine it at 550°C in an air atmosphere in a muffle furnace for 2h. The obtained phosphorus-modified ZSM-5 molecular sieve comparison sample is recorded as RYB-1s.

[0052] Example 2

[0053] 15.4 g of solid diammonium hydrogen phosphite was added to 100 g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), which was ground and mixed for 0.5 h and then transferred to a Teflon-lined stainless steel high-pressure reactor for a melting process at a heating temperature of 100°C for 10 h. After the melting process, the sample was taken out after naturally cooling to room temperature. The above sample was calcined at 550°C for 2 h to obtain a phosphorus-modified ZSM-5 molecular sieve sample, recorded as RYB-2.

[0054] Comparative Example 1

[0055] Take 17.4g of diammonium hydrogen phosphate and dissolve it in 145g of deionized water at 25°C, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25°C for 0.5h, move it to an oven and dry it at 120°C for 12h, and calcine it at 550°C in an air atmosphere in a muffle furnace for 2h. The obtained phosphorus-modified ZSM-5 molecular sieve comparison sample is recorded as D-1.

[0056] Comparative Example 2

[0057] Take 15.1g of phosphoric acid solution (mass fraction 85wt%) and dissolve it in 145g of deionized water at 25℃, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25℃ for 0.5h, move it to an oven and dry it at 120℃ for 12h, and calcine it at 550℃ in an air atmosphere in a muffle furnace for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve comparison sample, recorded as D-2.

[0058] In Examples 1, 1-1, 2 and Comparative Examples 1 and 2, the phosphorus-aluminum ratio of the phosphorus-containing compound to the molecular sieve was 1.25.

[0059] The XPS (P2p Scan) spectrum of sample RYB-1 is shown in Figure 1 . Figure 1The peaks 134.5eV and 135.2eV represent the electron binding energy of phosphorus in the surface phosphorus species of sample RYB-1 after drying and calcination, respectively. The XPS (P2pScan) spectra of RYB-1s and RYB-2 have Figure 1 characteristics.

[0060] The XRD relative crystallinity and crystal retention of RYB-1, RYB-1s, RYB-2, D-1 and D-2 before and after hydrothermal aging at 800℃, 100% water vapor and 17h are shown in Table 1.

[0061] Table 1

[0062]

[0063] Example 3

[0064] Take 6.5g of solid phosphorous acid and add it to 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30). After grinding and mixing for 0.5h, transfer it to a Teflon-lined stainless steel high-pressure reactor for a melting process with a heating temperature of 100°C and a time of 10h. After the melting process, wait for the sample to naturally cool to room temperature and then take it out; the above sample is calcined at 550°C for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve sample, recorded as RYB-3.

[0065] Example 3-1

[0066] Take 6.5g of solid phosphorous acid and dissolve it in 145g of deionized water at 25°C, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25°C for 0.5h, move it to an oven and dry it at 120°C for 12h, and calcine it at 550°C in an air atmosphere in a muffle furnace for 2h. The obtained phosphorus-modified ZSM-5 molecular sieve comparison sample is recorded as RYB-3s.

[0067] Example 4

[0068] 9.3 g of solid diammonium hydrogen phosphite was added to 100 g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), which was ground and mixed for 0.5 h and then transferred to a Teflon-lined stainless steel autoclave for a melting process at a heating temperature of 100°C for 10 h. After the melting process, the sample was taken out after naturally cooling to room temperature. The above sample was calcined at 550°C for 2 h to obtain a phosphorus-modified ZSM-5 molecular sieve sample, recorded as RYB-4.

[0069] Comparative Example 3

[0070] Take 10.5g of diammonium hydrogen phosphate and dissolve it in 145g of deionized water at 25°C, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25°C for 0.5h, move it to an oven and dry it at 120°C for 12h, and calcine it at 550°C in an air atmosphere in a muffle furnace for 2h. The obtained phosphorus-modified ZSM-5 molecular sieve comparison sample is recorded as D-3.

[0071] Comparative Example 4

[0072] 9.2 g of phosphoric acid solution (mass fraction 85 wt%) was dissolved in 145 g of deionized water at 25 ° C, stirred for 0.5 h to obtain a phosphorus-containing aqueous solution, 100 g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30) was added, and modified by impregnation method. After impregnation at 25 ° C for 0.5 h, it was moved to an oven for drying at 120 ° C for 12 h, and calcined at 550 ° C in an air atmosphere in a muffle furnace for 2 h. The obtained phosphorus-modified ZSM-5 molecular sieve comparison sample was recorded as D-4.

[0073] In Examples 3, 3-1, 4 and Comparative Examples 3 and 4, the phosphorus-aluminum ratio of the phosphorus-containing compound to the molecular sieve was 0.75.

[0074] The XPS (P2p Scan) spectra of samples RYB-3, RYB-3s, and RYB-4 all have Figure 1 characteristics.

[0075] The XRD relative crystallinity and crystal retention of RYB-3, RYB-3s, RYB-4, D-3 and D-4 before and after hydrothermal aging at 800℃, 100% water vapor and 17h are shown in Table 3.

[0076] Table 3

[0077]

[0078] Example 5

[0079] Take 15.0g of solid phosphorous acid and add it to 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30). After grinding and mixing for 0.5h, transfer it to a Teflon-lined stainless steel high-pressure reactor for a melting process with a heating temperature of 100°C and a time of 10h. After the melting process, wait for the sample to naturally cool to room temperature and then take it out; the above sample is calcined at 550°C for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve sample, recorded as RYB-5.

[0080] Example 5-1

[0081] Take 15.0g of solid phosphorous acid and dissolve it in 145g of deionized water at 25°C, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25°C for 0.5h, move it to an oven and dry it at 120°C for 12h, and calcine it at 550°C in an air atmosphere in a muffle furnace for 2h. The obtained phosphorus-modified ZSM-5 molecular sieve comparison sample is recorded as RYB-5s.

[0082] Example 6

[0083] Take 21.7g of solid diammonium hydrogen phosphite and add it to 100g HZSM-5 molecular sieve (nSiO2 / nAl2O3=30). After grinding and mixing for 0.5h, transfer it to a Teflon-lined stainless steel high-pressure reactor for a melting process with a heating temperature of 100°C and a time of 10h. After the melting process, wait for the sample to naturally cool to room temperature and then take it out; the above sample is calcined at 550°C for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve sample, recorded as RYB-6.

[0084] Comparative Example 5

[0085] Take 24.5g of diammonium hydrogen phosphate and dissolve it in 145g of deionized water at 25°C. Stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25°C for 0.5h, move it to an oven and dry it at 120°C for 12h. Calcinate it at 550°C in an air atmosphere in a muffle furnace for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve comparison sample, recorded as D-5.

[0086] Comparative Example 6

[0087] Take 21.4g of phosphoric acid solution (mass fraction 85wt%) and dissolve it in 145g of deionized water at 25℃, stir for 0.5h to obtain a phosphorus-containing aqueous solution, add 100g of HZSM-5 molecular sieve (nSiO2 / nAl2O3=30), and modify it by impregnation method. After impregnation at 25℃ for 0.5h, move it to an oven and dry it at 120℃ for 12h, and calcine it at 550℃ in an air atmosphere in a muffle furnace for 2h to obtain a phosphorus-modified ZSM-5 molecular sieve comparison sample, recorded as D-6.

[0088] In Examples 5, 5-1, 6 and Comparative Examples 5 and 6, the phosphorus-aluminum ratio of the phosphorus-containing compound to the molecular sieve was 1.75.

[0089] The XPS (P2p Scan) spectra of samples RYB-5, RYB-5s, and RYB-6 all have Figure 1 characteristics.

[0090] The XRD relative crystallinity and crystal retention of RYB-5, RYB-5s, RYB-6, D-5 and D-6 before and after hydrothermal aging at 800℃, 100% water vapor and 17h are shown in Table 5.

[0091] Table 5

[0092]

[0093]

[0094] Examples 7-26 illustrate the cracking catalysts provided by the present invention.

[0095] The phosphorus-aluminum inorganic binder used in the embodiment is prepared by the following process:

[0096] 1. NJ1: 1.91 kg of pseudo-boehmite (containing 1.19 kg of Al2O3), 0.56 kg of kaolin (0.5 kg on a dry basis) and 3.27 kg of decationized water were slurried for 30 minutes, and 5.37 kg of concentrated phosphoric acid (mass concentration 85%) was added to the slurry under stirring, with the phosphoric acid addition rate being 0.04 kg of phosphoric acid / min / kg of alumina source, and the temperature was raised to 70°C, and then reacted at this temperature for 45 minutes to obtain a phosphorus-aluminum inorganic binder. The material ratio is shown in Table 6, and the sample number is NJ1.

[0097] 2. NJ2: According to the preparation process of NJ1, the material ratio is shown in Table 9, and the sample number is NJ2.

[0098] Table 6

[0099]

[0100]

[0101] Embodiment 7-9

[0102] Take the phosphorus-modified molecular sieve RYB-1, Y-type molecular sieve (PSRY molecular sieve), kaolin and pseudo-boehmite of Example 1, add decationized water and beat for 120 minutes to obtain a slurry with a solid content of 30 weight%, add hydrochloric acid to adjust the pH value of the slurry to 3.0, and then continue to beat for 45 minutes, and then add the phosphorus-aluminum inorganic binder NJ1. After stirring for 30 minutes, the obtained slurry is spray-dried to obtain microspheres, and the microspheres are calcined at 500°C for 1 hour to obtain a catalyst, numbered Cat1.

[0103] The samples RYB-1s and RYB-2 of Example 1-1 and Example 2 were used to replace the molecular sieve RYB-1, respectively, and the catalysts numbered Cat2 and Cat3 were prepared according to the above preparation process.

[0104] In the material proportions of Cat1, Cat2 and Cat3, based on dry weight, phosphorus-modified molecular sieve accounts for 60%, PSRY accounts for 5%, kaolin accounts for 20%, phosphorus-aluminum binder NJ1 accounts for 10%, and pseudo-boehmite accounts for 5%.

[0105] Comparative Examples 7 and 8

[0106] The preparation process and material ratio are the same as those of Example 7, except that the phosphorus-modified molecular sieves D-1 and D-2 of Comparative Examples 1 and 2 are used to replace the molecular sieve RYB-1, to prepare comparative catalysts, numbered DCat1 and DCat2, respectively.

[0107] Examples 10-12

[0108] Take the phosphorus-modified molecular sieve RYB-3, Y-type molecular sieve (HRY molecular sieve), and kaolin of Example 3, add decationized water and aluminum sol, and beat for 120 minutes to obtain a slurry with a solid content of 30 wt%, add hydrochloric acid to adjust the pH value of the slurry to 3.0, and then continue to beat for 45 minutes, and then add the phosphorus-aluminum inorganic binder NJ2. After stirring for 30 minutes, the obtained slurry is spray-dried to obtain microspheres, and the microspheres are calcined at 500°C for 1 hour to obtain a catalyst, numbered Cat4.

[0109] The molecular sieve RYB-3 was replaced by the phosphorus-modified molecular sieves RYB-3s and RYB-4 of Example 3-1 and Example 4, respectively, and catalysts numbered Cat5 and Cat6 were prepared according to the above preparation process.

[0110] In the material ratio of Cat4, Cat5 and Cat6, based on dry weight, phosphorus-modified ZSM-5 molecular sieve accounts for 60%, HRY accounts for 5%, kaolin accounts for 20%, phosphorus-aluminum binder NJ2 accounts for 10%, and aluminum sol accounts for 5%.

[0111] Comparative Examples 9 and 10

[0112] The preparation process and material ratio are the same as those of Example 10, except that the phosphorus-modified molecular sieves D-3 and D-4 of Comparative Examples 3 and 4 are used to replace the molecular sieve RYB-3, to prepare comparative catalysts, numbered DCat3 and DCat4, respectively.

[0113] Examples 13-15

[0114] Take the phosphorus-modified molecular sieve RYB-5, Y-type molecular sieve (PSRY molecular sieve), and kaolin of Example 5, add decationized water and aluminum sol and beat for 120 minutes to obtain a slurry with a solid content of 30 wt%, add hydrochloric acid to adjust the pH value of the slurry to 3.0, and then continue to beat for 45 minutes, and then add the phosphorus-aluminum inorganic binder NJ1. After stirring for 30 minutes, the obtained slurry is spray-dried to obtain microspheres, and the microspheres are calcined at 500°C for 1 hour to obtain a catalyst, numbered Cat7.

[0115] The molecular sieve RYB-5 was replaced by the phosphorus-modified molecular sieves RYB-5s and RYB-6 of Example 5-1 and Example 6, respectively, and catalysts numbered Cat8 and Cat9 were prepared according to the above preparation process.

[0116] In the material proportions of Cat7, Cat8 and Cat9, based on dry weight, phosphorus-modified ZSM-5 molecular sieve accounts for 50%, PSRY accounts for 20%, kaolin accounts for 15%, phosphorus-aluminum binder NJ1 accounts for 10%, and aluminum sol accounts for 5%.

[0117] Comparative Examples 11 and 12

[0118] The preparation process and material ratio are the same as those of Example 13, except that the phosphorus-modified molecular sieves D-5 and D-6 of Comparative Examples 5 and 6 are used to replace the molecular sieve RYB-5, to prepare comparative catalysts, numbered DCat5 and DCat6, respectively.

[0119] The following examples illustrate the catalytic cracking method provided by the present invention.

[0120] Examples 16-18

[0121] Catalysts Cat1-Cat3 were aged for 17 hours at 800°C in a 100% steam atmosphere. The aged catalysts were loaded into a fixed bed microreactor to evaluate the catalytic cracking ability of the catalysts for light hydrocarbons. The evaluation conditions were a reaction temperature of 650°C, a regeneration temperature of 620°C, and a catalyst-oil ratio of 3.2.

[0122] The properties of the feedstock oil are shown in Table 7. The reaction results are shown in Table 8.

[0123] Table 7

[0124] project Light hydrocarbons <![CDATA[Density (20 °C) / (kg·m -3 )]]> 670.7 Element mass composition / % C 83.81 H 16.19 <![CDATA[S / mg.L -1 ]]> 2.6 <![CDATA[N / mg.L -1 ]]> <0.3 Distillation range / ℃ Initial distillation point 33.7 10% 56.3 30% 69.1 50% 86.6 70% 107.2 90% 130.5 95% 137.5 Final distillation point 155.7 Hydrocarbon mass composition / % Normal alkanes 72.69 Isoalkanes 25.48 Olefins 0.13 Cycloalkanes 1.56 Aromatics 0.17 total 100.03

[0125] Comparative Examples 13 and 14

[0126] Same as Example 16, except that comparative catalysts DCat1 and DCat2 are used to replace Cat1.

[0127] The reaction results are shown in Table 8.

[0128] Table 8

[0129]

[0130]

[0131] Examples 19-21

[0132] Catalyst C at 4-C at 6. The catalyst was aged for 17 hours at 800°C in a 100% steam atmosphere. The aged catalyst was loaded into a fixed bed microreactor to evaluate the catalytic cracking ability of the catalyst for light hydrocarbons. The evaluation conditions were reaction temperature of 650°C, regeneration temperature of 620°C, and catalyst-oil ratio of 3.2.

[0133] The reaction results are shown in Table 9.

[0134] Comparative Examples 15 and 16

[0135] Same as Example 19, except that comparative catalysts DCat3 and DCat4 are used to replace Cat4.

[0136] The reaction results are shown in Table 9.

[0137] Table 9

[0138] project Embodiment 19 Embodiment 20 Embodiment 21 Comparative Example 15 Comparative Example 16 Catalyst name Cat4 Cat5 Cat6 DCat3 DCat4 Conversion rate 69.63 67.01 68.76 62.80 61.49 Coke quantity 10.44 11.02 10.89 12.71 12.97 Liquid product yield / wt% 28.12 30.53 29.31 31.25 31.29 Gas product yield / wt% 61.44 58.45 59.80 56.04 55.74 Cracked gas product yield wt% C2= 16.13 15.23 15.81 11.27 11.01 C3= 21.17 18.01 19.37 16.03 15.73

[0139] Examples 22-24

[0140] Catalysts Cat7-Cat9 were aged for 17 hours at 800°C in a 100% steam atmosphere. The aged catalysts were loaded into a fixed bed microreactor to evaluate the catalytic cracking ability of the catalysts for light hydrocarbons. The evaluation conditions were a reaction temperature of 650°C, a regeneration temperature of 620°C, and a catalyst-oil ratio of 3.2.

[0141] The reaction results are shown in Table 10.

[0142] Comparative Examples 17 and 18

[0143] Same as Example 22, except that comparative catalysts DCat5 and DCat6 are used to replace Cat7.

[0144] The reaction results are shown in Table 10.

[0145] Table 10

[0146] project Embodiment 22 Embodiment 23 Embodiment 24 Comparative Example 17 Comparative Example 18 Catalyst name Cat7 Cat8 Cat9 DCat5 DCat6 Conversion rate 54.15 51.81 54.03 45.72 43.84 Coke quantity 4.29 4.47 4.16 4.71 4.53 Liquid product yield / wt% 50.05 53.11 51.16 57.56 59.09 Gas product yield / wt% 45.66 42.42 44.68 37.73 36.38 Cracked gas product yield wt% C2= 7.44 6.99 7.29 4.58 4.18 C3= 12.32 11.61 11.90 8.77 8.01

[0147] Examples 25-27

[0148] Catalysts Cat1-Cat3 were aged for 17 hours at 800°C in a 100% steam atmosphere. The aged catalysts were loaded into a fixed bed microreactor to evaluate the catalytic cracking ability of the catalysts for light hydrocarbons. The evaluation conditions were reaction temperature 660°C, regeneration temperature 600°C, catalyst-oil ratio 15.

[0149] The reaction results are shown in Table 11.

[0150] Comparative Examples 19 and 20

[0151] Same as Example 25, except that comparative catalysts DCat1 and DCat2 are used to replace Cat1.

[0152] The reaction results are shown in Table 11.

[0153] Table 11

[0154] project Embodiment 25 Embodiment 26 Embodiment 27 Comparative Example 19 Comparative Example 20 Catalyst name Cat1 Cat2 Cat3 DCat1 DCat2 Conversion rate 78.42 75.81 77.67 72.18 71.00 Coke quantity 10.55 11.23 10.79 12.47 12.15 Liquid product yield / wt% 22.69 24.11 23.52 26.76 27.42 Gas product yield / wt% 66.76 64.66 65.69 60.77 60.43 Cracked gas product yield wt% C2= 18.07 17.48 17.93 16.71 16.07 C3= 23.80 21.92 23.27 19.83 19.26

[0155] It can be seen from Tables 8, 9, 10 and 11 that the catalytic cracking catalysts prepared by modifying ZSM-5 molecular sieves with phosphorus-containing compounds having a phosphorus valence state of +3 have increased hydrocarbon conversion rates, reduced coke, and improved ethylene and propylene yields compared to the catalytic cracking catalysts prepared by modifying ZSM-5 molecular sieves with phosphorus-containing compounds having a phosphorus valence state of +5.

Claims

1. A catalytic cracking method, comprising contacting a hydrocarbon oil with a cracking catalyst under catalytic cracking reaction conditions, wherein the cracking catalyst contains, based on the dry weight of the cracking catalyst, 2-20% of a Y-type molecular sieve, 3-80% of a phosphorus-modified ZSM-5 molecular sieve, 1-70% of an inorganic binder, and 2-60% of clay, based on the dry weight of the cracking catalyst, characterized in that: The phosphorus-modified ZSM-5 molecular sieve is modified with a phosphorus-containing compound having a phosphorus valence state of +3. After hydrothermal aging of the phosphorus-modified ZSM-5 molecular sieve at 800°C and 100% water vapor for 17 hours, the electron binding energy of the phosphorus element in the phosphorus species on the molecular sieve surface is 135.2 eV, and the crystal retention in XRD analysis is 70% to 110%.

2. The method according to claim 1, characterized in that The cracking catalyst is used alone, or in a mixture with a conventional cracking catalyst. In the mixture, the cracking catalyst accounts for no more than 30% by weight of the total amount of the mixture, preferably 1-25% by weight, and more preferably 3-15% by weight.

3. The method according to claim 1, wherein: The catalytic cracking reaction conditions include: a reaction temperature of 500-800°C.

4. The method according to claim 1, wherein: The hydrocarbon oil is selected from one or more of crude oil, naphtha, gasoline, atmospheric residue, vacuum residue, atmospheric wax oil, vacuum wax oil, straight-run wax oil, propane light / heavy deoiling, coker wax oil and coal liquefaction products.

5. The method according to claim 1, wherein: The Y-type molecular sieve is at least one selected from PSRY molecular sieve, PSRY-S molecular sieve, PSRY molecular sieve containing rare earth, PSRY-S molecular sieve containing rare earth, USY molecular sieve, USY molecular sieve containing rare earth, REY molecular sieve, REHY molecular sieve and HY molecular sieve.

6. The method according to claim 1, wherein: After the phosphorus-modified ZSM-5 molecular sieve is hydrothermally aged for 17 hours under the conditions of 800° C. and 100% water vapor, the crystal retention rate in XRD analysis is 95% to 110%.

7. The method according to claim 1, characterized in that The phosphorus-modified ZSM-5 molecular sieve has a molar ratio of phosphorus to aluminum of 0.01 to 5, preferably 0.1 to 3.

8. The method according to claim 1, characterized in that The phosphorus-modified ZSM-5 molecular sieve is obtained by mixing and grinding a solid phosphorus-containing compound precursor with a phosphorus valence state of +3 and a HZSM-5 molecular sieve to obtain a solid phase mixture; heating and melting the solid phase mixture; cooling the heated and melted solid phase mixture to room temperature and then calcining the mixture; Alternatively, the HZSM-5 molecular sieve is contacted and impregnated with an aqueous solution of a phosphorus-containing compound having a phosphorus valence state of +3, followed by drying and calcining to obtain the obtained product.

9. The method according to claim 8, characterized in that The heating and melting treatment has a temperature higher than the melting point of the solid phosphorus-containing compound precursor and lower than the temperature at which the solid phosphorus-containing compound precursor decomposes or dehydrates, and the treatment time is 2 to 72 hours.

10. The method according to claim 1 or 8, characterized in that: The solid phosphorus-containing compound precursor with a phosphorus valence state of +3 is selected from phosphorous acid and / or ammonium phosphite.

11. The method according to claim 8, characterized in that The solid phosphorus-containing compound precursor with a phosphorus valence state of +3 is calculated as phosphorus and the HZSM-5 molecular sieve is calculated as aluminum, and the molar ratio of the two is 0.1-5, preferably 0.5-2.

5.

12. The method according to claim 1, wherein: The inorganic binder comprises a phosphorus-aluminum inorganic binder, and the phosphorus-aluminum inorganic binder accounts for 5-40% by weight based on the dry basis of the catalyst.

13. The method according to claim 1 or 12, wherein: The inorganic binder also contains at least one selected from pseudo-boehmite, aluminum sol, silica-alumina sol and water glass.

14. The method according to claim 1, wherein: The clay is selected from at least one of kaolin, sepiolite, attapulgite, rectorite, montmorillonite and diatomaceous earth.

15. A cracking catalyst, comprising, based on the dry weight of the cracking catalyst, 2-20% of a Y-type molecular sieve, 3-80% of a phosphorus-modified ZSM-5 molecular sieve, 1-70% of an inorganic binder, and 2-60% of clay, based on the dry weight of the cracking catalyst, characterized in that: The phosphorus-modified ZSM-5 molecular sieve is modified with a phosphorus-containing compound having a phosphorus valence state of +3. After hydrothermal aging of the phosphorus-modified ZSM-5 molecular sieve at 800°C and 100% water vapor for 17 hours, the electron binding energy of the phosphorus element in the phosphorus species on the molecular sieve surface is 135.2 eV, and the crystal retention in XRD analysis is 70% to 110%.

Citation Information

Patent Citations

  • Hydrocarbon cracking catalyst containing phosphorus

    CN1060304A

  • Catalytic cracking aid, preparation method thereof and hydrocarbon oil catalytic cracking method

    CN112138711A

  • Cracking catalyst, preparation method and application

    CN114425432A

Cited By

  • Recovery process of p-tert-butylphenol waste liquid

    CN121044969A