Novel silica powder surface modification method and application of composite material thereof

The novel silicon micro-powder surface modification method with MXene nanosheets addresses oxidation and interface issues, achieving high conductivity and shielding efficiency, with improved stability and multifunctionality for diverse applications.

CN120308963APending Publication Date: 2025-07-15JIANGXI GUANGYUAN CHEM
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510439491.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-09
Publication Date
2025-07-15

AI Technical Summary

Technical Problem

MXene is easy to oxidize and stack, poor bonding of silicon powder and MXene interfaces, and insufficient versatility of existing composite materials, resulting in poor conductivity, mechanical properties and stability.

Method used

Silicon powder was surface modified by titanate coupling agent, and a core-shell structure of silicon powder/MXene composite material was formed by hydrothermal in situ growth method, and a borate protective layer was applied to the surface to improve interface bonding and antioxidant properties.

Benefits of technology

It achieves high conductivity, excellent electromagnetic shielding efficiency and high specific capacity, improves the stability of the material in high temperature/humid environments, and expands application scenarios to electromagnetic shielding, energy storage and flexible electronics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005350618550000061
    Figure BDA0005350618550000061
Patent Text Reader

Abstract

The invention relates to the technical field of silica powder surface modification, in particular to a novel silica powder surface modification method and application of a composite material of the novel silica powder surface modification method. Silica powder surface modification comprises the steps that silica powder is subjected to surface chemical modification through a titanate coupling agent, active functional groups are introduced, and the interface bonding force between the silica powder and MXene is enhanced; high-quality preparation of MXene: etching an MAX phase by adopting hydrofluoric acid (HF) or lithium fluoride / hydrochloric acid (LiF / HCl), and obtaining few layers of MXene nanosheets through ultrasonic stripping to ensure high conductivity and large specific surface area; the modified silica powder and MXene dispersion liquid are uniformly mixed, MXene stacking is inhibited, the specific surface area is increased, and the ion transmission efficiency is improved; mXene nanosheets grow on the surface of the silica powder in situ to form a core-shell structure, so that the interface bonding strength and the mechanical property are enhanced; the composite material is applied to the fields of electromagnetic shielding, energy storage, flexible electronics and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This solution relates to the technical field of surface modification of silica powder, specifically referring to a new surface modification method of silica powder and the application of its composite materials. Background Art

[0002] MXene (Ti3C2T x ) is widely used in the fields of electromagnetic shielding and energy storage due to its high conductivity (>6000 S / cm), large specific surface area, and adjustable surface functional groups. In the prior art, MXene is often compounded with polymers (such as PVDF, PVA) or ceramic materials (such as Al2O3, SiO2) to form films, coatings, or porous structures. The shielding effectiveness (SE) is achieved by reflecting and absorbing electromagnetic waves, usually in the range of 30 - 60 dB. As an electrode material, MXene achieves a high specific capacity (such as >300 mAh / g in lithium-ion batteries) through surface redox reactions and ion intercalation mechanisms. Silica powder (SiO2) is commonly used to reinforce polymer or ceramic matrices due to its low cost, high heat resistance, and good mechanical properties. In the prior art, silica powder is mostly used as a filler or reinforcing phase to improve the mechanical strength or thermal stability of materials.

[0003] Prior art and methods: physical mixing method, chemical modification method, template method.

[0004] Problems and disadvantages of the prior art:

[0005] 1. MXene is prone to oxidation and stacking: Since the surface functional groups of MXene (such as -OH, -F) are unstable in the environment and van der Waals forces cause the sheets to aggregate, MXene is prone to oxidation in humid or high-temperature environments, resulting in a decrease in conductivity and shielding effectiveness; MXene nanosheets are prone to stacking, reducing the specific surface area and ion transport efficiency (such as battery performance degradation);

[0006] 2. Poor interfacial bonding between silica powder and MXene: The existing physical mixing method is difficult to achieve uniform dispersion and strong interfacial bonding, resulting in unsatisfactory mechanical properties and conductivity of the composite material. The reason is that the surface of silica powder is inert and lacks chemical bonding with MXene;

[0007] 3. Lack of versatility: The existing composite materials mostly focus on a single property (such as electromagnetic shielding or energy storage), and it is difficult to balance mechanical properties, thermal stability, and versatility. The reason is the limitations of material design and processes, and the synergistic effect of silica powder and MXene has not been fully utilized. Summary of the Invention

[0008] Aiming at the problems of easy oxidation and stacking of MXene, poor interfacial bonding, and lack of versatility in the prior art, this solution provides a new surface modification method of silica powder and the application of its composite materials.

[0009] The technical solution adopted in this solution is as follows: A new method for surface modification of silica powder, including the following steps:

[0010] Step 1, pretreatment of silica powder:

[0011] The surface of the silica powder is modified with a titanate coupling agent;

[0012] Step 2, preparation of MXene:

[0013] Etch the MAX phase (such as Ti3AlC2) with hydrofluoric acid (HF) or a mixed solution of lithium fluoride / hydrochloric acid (LiF / HCl) to prepare multi-layer MXene (Ti3C2T x ), and obtain few-layer MXene nanosheets by ultrasonic exfoliation;

[0014] Step 3, preparation of composite material:

[0015] The MXene nanosheets are coated on the silica powder by hydrothermal in-situ growth method to form a core-shell structure, with the pretreated silica powder as the core and MXene as the shell, to obtain a silica powder / MXene composite material;

[0016] Step 4, post-treatment and forming:

[0017] (1) Heat treatment: Heat-treat the composite material in an inert atmosphere (such as Ar) at (300 - 500 °C) to remove residual solvents and enhance interfacial bonding, aiming to improve the crystallinity and thermal stability of the composite material, enhance the chemical bonding between the silica powder and MXene, and improve the mechanical properties;

[0018] (2) Compression molding: Coat the heat-treated composite material on a substrate (such as a polyimide film) or form it through a tablet press to prepare film, coating or bulk materials, to obtain a high-density and uniform composite material, suitable for different application scenarios; The film material can be used for flexible electronic devices, and the bulk material can be used for electromagnetic shielding or energy storage devices;

[0019] Step 5, antioxidant treatment:

[0020] Coat a borate ester protective layer on the surface of the composite material to improve the antioxidant performance of the composite material in high-temperature / humid environments, extend the service life of the material, and be suitable for harsh environments.

[0021] Furthermore, the specific process of the pretreatment of the silica powder is:

[0022] Disperse the silica powder in ethanol (ethanol concentration is 10 wt%), and add tetra-neoalkoxy bis(didecylphosphite) titanate coupling agent (dosage is 1 - 2% of the mass of the silica powder);

[0023] Magnetically stir at 60 °C for 6 hours to introduce active functional groups onto the surface of silica powder;

[0024] Centrifuge and wash (centrifugation speed is 3500 rpm, time is 5 minutes) to remove the unreacted coupling agent, and dry it under vacuum for standby.

[0025] Furthermore, the specific process for preparing MXene is as follows:

[0026] Add 2.4 g of LiF and 1.5 g of Ti3AlC2 to 30 mL of HCl (concentration is 9 M) in sequence, and then use magnetic stirring at 40 °C for at least 30 min to etch off the Al layer in Ti3AlC2;

[0027] Reaction equation:

[0028] Ti3AlC2 + 3LiF + 3HCl → Ti3C2Tx + 3LiCl + AlF3 + 1.5H2Ti3AlC2 + 3LiF + 3HCl → Ti3C2Tx + 3LiCl + AlF3 + 1.5H2

[0029] When the Al layer is completely etched and the Ti3AlC2 nanosheets are converted into Ti3C2T x nanosheets, centrifuge and wash at 3500 rpm at room temperature (25 °C) for 5 minutes until pH≈6, until the upper layer of the liquid turns dark green, and remove LiCl and AlF3;

[0030] Ultrasonically treat the above liquid in an ultrasonic treatment device at 40 °C for 15 minutes under the conditions of a power of 500 W and a frequency of 40 kHz;

[0031] Alternately centrifuge and ultrasonically treat a total of 8 times to increase the yield of MXene and obtain a few-layer MXene nanosheet dispersion.

[0032] Furthermore, the specific process for preparing the composite material is as follows:

[0033] Adopt hydrothermal in-situ growth, mix the modified silica powder and the MXene nanosheet dispersion at a mass ratio of 1:4, and ultrasonically disperse for 30 minutes to ensure uniform mixing;

[0034] Transfer the mixed solution to a hydrothermal reaction kettle, control the filling degree at 70%-80%, and carry out a hydrothermal reaction at 180 °C for 12 hours to enable the in-situ growth of MXene nanosheets on the surface of silica powder to form a core-shell structure;

[0035] Wash the reaction product 3 times with deionized water, centrifuge (3500 rpm, 5 minutes) to remove the unreacted MXene, and freeze-dry or vacuum-dry to obtain the silica powder / MXene composite material.

[0036] Further, in Step 1, the coupling agent is tetra-neoalkoxy bis(didecylphosphite) titanate.

[0037] Further, in Step 2, the particle size of the silica powder is 1 - 10 μm.

[0038] Further, in Step 2, the Ti3AlC2 is in powder form and the particle size is < 38 μm.

[0039] Further, in Step 5, the borate ester is trimethyl borate.

[0040] The coating process is as follows:

[0041] Disperse the silica powder / MXene composite material

[0042] Disperse the silica powder / MXene composite material in absolute ethanol (concentration 10 mg / mL), and perform ultrasonic treatment for 30 minutes (power 100 W, frequency 40 kHz);

[0043] Add the borate ester: Add the borate ester at 1 - 2% of the mass of the composite material (for example, add 10 - 20 mg of TMB to 1 g of the composite material); under nitrogen protection, stir magnetically for 6 hours (at room temperature) to make the borate ester uniformly adsorbed on the surface of the composite material;

[0044] Heat treatment: Vacuum dry the coated composite material at 80 °C for 12 hours to form stable chemical bonds between the borate ester and the surface of the composite material;

[0045] Washing and drying: Wash 3 times with absolute ethanol to remove the unreacted borate ester; vacuum dry to obtain the composite material with antioxidant treatment.

[0046] This solution also discloses the applications of the silica powder / MXene composite material in electromagnetic shielding, energy storage, and flexible electronics, such as aerospace, lithium-ion batteries, and sensors.

[0047] The beneficial effects achieved by this solution with the above structure are as follows:

[0048] 1. Through innovative composite processes and structural designs, high conductivity (> 1000 S / m), excellent electromagnetic shielding effectiveness (> 50 dB), and high specific capacity (> 800 mAh / g) are achieved;

[0049] 2. Improve the material stability: Through antioxidant treatment and interface optimization, extend the service life of the composite material in high-temperature / humid environments;

[0050] 3. Expand the application scenarios: Develop multifunctional materials suitable for electromagnetic shielding (such as aerospace), energy storage (such as lithium-ion batteries), and flexible electronics (such as sensors). Specific embodiments

[0051] The technical solutions in the embodiments of this solution will be described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of this solution, rather than all of the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments in this solution without making creative efforts belong to the scope of protection of this solution.

[0052] Embodiment

[0053] A new method for surface modification of silica powder includes the following steps:

[0054] Step 1, pretreatment of silica powder:

[0055] The silica powder is subjected to surface modification treatment and chemically modified with tetra-neoalkoxy bis(didecylphosphite acyloxy) titanate coupling agent. The purpose is to introduce active functional groups on the surface of the silica powder, enhance its interfacial binding force with MXene, improve the dispersibility of the silica powder in the MXene dispersion, and avoid agglomeration.

[0056] The specific process of one embodiment is as follows:

[0057] Disperse the silica powder (particle size 1 - 10 μm) in an ethanol aqueous solution (ethanol concentration 10 wt%), and add tetra-neoalkoxy bis(didecylphosphite acyloxy) titanate coupling agent (dosage is 1 - 2% of the mass of the silica powder);

[0058] Magnetically stir at 60 °C for 6 hours to introduce active functional groups on the surface of the silica powder;

[0059] Centrifuge and wash (centrifugation speed 3500 rpm, time 5 minutes) to remove the unreacted coupling agent, and dry in vacuum for standby;

[0060] Step 2, preparation of MXene:

[0061] To obtain MXene nanosheets with high conductivity (>6000 S / cm) and large specific surface area, and provide high-quality MXene materials for subsequent composites, etch the MAX phase (such as Ti3AlC2, powder particle size <38 μm) with hydrofluoric acid (HF) or a mixed solution of lithium fluoride / hydrochloric acid (LiF / HCl) to prepare multilayer MXene (Ti3C2T x )), and obtain few-layer MXene nanosheets by ultrasonic exfoliation;

[0062] The specific process of one embodiment is as follows:

[0063] 2.4 g of LiF and 1.5 g of Ti3AlC2 were added to 30 mL of HCl (concentration 9 M) in sequence, and then magnetically stirred at 40 °C for at least 30 min to etch away the Al layer in Ti3AlC2;

[0064] Reaction equation:

[0065] Ti3AlC2 + 3LiF + 3HCl → Ti3C2Tx + 3LiCl + AlF3 + 1.5H2Ti3AlC2 + 3LiF + 3HCl → Ti3C2Tx + 3LiCl + AlF3 + 1.5H2

[0066] When the Al layer was completely etched and the Ti3AlC2 nanosheets were converted into Ti3C2T x nanosheets, centrifugal washing was carried out at 3500 rpm at room temperature of 25 °C for 5 minutes until pH≈6, until the upper layer of the liquid became dark green, and LiCl and AlF3 were removed;

[0067] The above liquid was ultrasonically treated in an ultrasonic treatment device at 40 °C for 15 minutes under the conditions of a power of 500 W and a frequency of 40 kHz;

[0068] Centrifugation and ultrasonic treatment were alternated 8 times in total to increase the MXene yield and obtain a few-layer MXene nanosheet dispersion;

[0069] Step three, composite material preparation:

[0070] In-situ growth method, MXene nanosheets were hydrothermally grown in-situ to form a core-shell structure, with the pretreated silicon micropowder as the core and MXene as the shell, aiming to enhance the interfacial bonding strength, improve the mechanical properties and electrical conductivity of the composite material, and obtain a silicon micropowder / MXene composite material;

[0071] The specific process of one embodiment is as follows:

[0072] Hydrothermal in-situ growth was adopted, and the modified silicon micropowder and the MXene nanosheet dispersion were mixed at a mass ratio of 1:4 and ultrasonically dispersed for 30 minutes to ensure uniform mixing;

[0073] The mixed solution was transferred to a hydrothermal reaction kettle, and the filling degree was controlled at 70%-80%. Hydrothermal reaction was carried out at 180 °C for 12 hours to enable MXene nanosheets to grow in-situ on the surface of silicon micropowder and form a core-shell structure;

[0074] The reaction product was washed 3 times with deionized water, centrifuged (3500 rpm, 5 minutes) to remove the unreacted MXene, and freeze-dried or vacuum-dried to obtain a silicon micropowder / MXene composite material;

[0075] Step four, post-treatment and forming:

[0076] (1) Heat treatment: Heat-treat the composite material in an inert atmosphere (such as Ar) at 300 - 500 °C to remove residual solvents and enhance interfacial bonding. The purpose is to improve the crystallinity and thermal stability of the composite material, strengthen the chemical bonding between silica powder and MXene, and enhance mechanical properties;

[0077] (2) Compression molding: Coat the heat-treated composite material on a substrate (such as a polyimide film) or form it through a tablet press to prepare thin films, coatings or bulk materials, obtaining high-density and uniform composite materials suitable for different application scenarios; The thin film material can be used for flexible electronic devices, and the bulk material can be used for electromagnetic shielding or energy storage devices;

[0078] Step Five, antioxidant treatment:

[0079] Coat a borate ester protective layer on the surface of the composite material. The borate ester is trimethyl borate to improve the antioxidant performance of the composite material in high-temperature / humid environments, extend the service life of the material, and is suitable for harsh environments;

[0080] A specific coating process for one embodiment is as follows:

[0081] Disperse the composite material: Disperse the silica powder / MXene composite material in absolute ethanol to a concentration of 10 mg / mL, and ultrasonically treat it for 30 minutes (power 100 W, frequency 40 kHz);

[0082] Add borate ester: Add borate ester according to 1 - 2% of the mass of the composite material (such as adding 10 - 20 mg TMB to 1 g of composite material); Under nitrogen protection, magnetically stir for 6 hours (room temperature) to make the borate ester evenly adsorbed on the surface of the composite material;

[0083] Heat treatment: Vacuum dry the coated composite material at 80 °C for 12 hours to form a stable chemical bond between the borate ester and the surface of the composite material;

[0084] Washing and drying: Wash 3 times with absolute ethanol to remove unreacted borate ester; Vacuum dry to obtain the antioxidant-treated composite material.

[0085] This solution also discloses the application of a surface-modified silica powder composite material in electromagnetic shielding, energy storage and flexible electronics, such as aerospace, lithium-ion batteries, sensors, as shown in the following table.

[0086] Table 1 Composite Material Performance Table

[0087]

[0088] I. Material Performance Optimization

[0089] Balance of High Conductivity and Mechanical Properties

[0090] Prior art: MXene is prone to stacking, resulting in a decrease in conductivity; the interfacial bonding between silica powder and MXene is poor, and the mechanical properties are insufficient.

[0091] This solution: Through surface modification of silica powder and in-situ growth method, enhance interfacial bonding, inhibit MXene stacking, and achieve high conductivity (>1000 S / m) and high mechanical properties (compressive strength >200 MPa).

[0092] Improved antioxidant performance

[0093] Prior art: MXene is prone to oxidation in humid or high-temperature environments, resulting in performance degradation.

[0094] This solution: Through antioxidant treatment (such as borate ester coating) and silica powder coating, significantly improve the environmental stability of the composite material and extend its service life.

[0095] Multi-functional synergistic optimization

[0096] Prior art: Existing composite materials mostly focus on single performance (such as electromagnetic shielding or energy storage), and it is difficult to balance mechanical properties, thermal stability, and multi-functionality.

[0097] This solution: Through gradient structure design and porous network construction, achieve the synergistic optimization of electromagnetic shielding, energy storage, and mechanical properties, and meet the application requirements in multiple fields.

[0098] II. Process innovation and cost reduction

[0099] Enhanced interfacial bonding

[0100] Prior art: The physical mixing method is difficult to achieve uniform dispersion and strong interfacial bonding.

[0101] This solution: Adopt chemical modification (such as silane coupling agent treatment) and in-situ growth method to significantly enhance the interfacial bonding between silica powder and MXene, and improve the overall performance of the composite material.

[0102] Low cost and environmental protection

[0103] Prior art: The preparation cost of MXene is high, which limits its large-scale application.

[0104] This solution: Partially replace MXene with low-cost silica powder to reduce the material cost. At the same time, utilize the thermal stability and mechanical properties of silica powder to improve the cost performance of the composite material.

[0105] Simple and controllable process

[0106] Prior art: Existing composite processes are complex and difficult to achieve large-scale production.

[0107] This solution: Using the solution mixing method and the template method, the process is simple and highly controllable, suitable for industrial production.

[0108] III. Improvement of application performance

[0109] Excellent electromagnetic shielding effectiveness

[0110] Existing technology: The electromagnetic shielding effectiveness (SE) of MXene-based composites is usually 30 - 60 dB, and the performance deteriorates under high-temperature environments;

[0111] Outstanding energy storage performance

[0112] Existing technology: The specific capacity of MXene-based electrode materials is usually 300 - 500 mAh / g, and the cycling stability is insufficient;

[0113] This solution: As the anode of a lithium-ion battery, the composite material has a specific capacity > 800 mAh / g, and the capacity retention rate after 500 cycles > 90%, significantly improving the energy storage performance;

[0114] Enhanced mechanical properties

[0115] Existing technology: The mechanical properties of MXene-based composites are poor, making it difficult to meet the requirements of structure-function integration;

[0116] This solution: Through the strengthening effect of silica powder, the compressive strength of the composite material > 200 MPa, and the Young's modulus > 10 GPa, suitable for high-strength application scenarios.

[0117] IV. Expansion of multifunctional applications

[0118] High-temperature electromagnetic shielding

[0119] Existing technology: Most existing electromagnetic shielding materials are suitable for normal-temperature environments, with insufficient high-temperature performance;

[0120] This solution: The composite material still maintains excellent shielding effectiveness under high-temperature environments, suitable for fields such as aerospace;

[0121] Flexible electronic devices

[0122] Existing technology: Most existing flexible materials rely on polymer matrices, making it difficult to balance mechanical properties and conductivity;

[0123] This solution: The composite material combines high conductivity and flexibility, suitable for flexible pressure sensors (sensitivity ≥ 5 kPa-1, response time < 50 ms);

[0124] Structure-function integration

[0125] Existing technology: Existing materials are difficult to simultaneously meet the requirements of mechanical properties and functional properties;

[0126] This solution: The composite material combines high mechanical properties and multifunctionality and is suitable for integrated structure-function design.

[0127] It should be noted that in this article, the terms "including", "comprising" or any other variant thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements not only includes those elements, but also includes other elements not explicitly listed, or further includes elements inherent to such a process, method, article or device.

[0128] Although the embodiments of this solution have been shown and described, for those of ordinary skill in the art, it can be understood that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this solution, and the scope of this solution is defined by the appended claims and their equivalents.

Claims

1. A new method for surface modification of silica fume, characterized in that, It includes the following steps: Step 1, pretreatment of silica powder: The silica powder is surface-modified with a titanate coupling agent; Step 2, preparation of MXene: Etch the MAX phase with hydrofluoric acid or a lithium fluoride / hydrochloric acid mixed solution to prepare multi-layer MXene, and obtain few-layer MXene nanosheets by ultrasonic exfoliation; Step 3, preparation of composite material: Use the hydrothermal in-situ growth method to coat the MXene nanosheets on the silica powder to form a core-shell structure, with the pretreated silica powder as the core and MXene as the shell, to obtain the silica powder / MXene composite material; Step 4, post-treatment and forming: (1) Heat treatment: Heat-treat the composite material in an inert atmosphere to remove residual solvents and enhance interfacial bonding; (2) Compression molding: Coat the heat-treated composite material on a substrate or form it through a tablet press to prepare thin films, coatings or bulk materials, and obtain a high-density, uniform composite material suitable for different application scenarios; Step 5, antioxidant treatment: Coat a borate ester protective layer on the surface of the composite material.

2. A novel method for surface modification of silica powder according to claim 1, characterized in that, The specific process of the silica powder pretreatment is: Disperse the silica powder in an ethanol aqueous solution with an ethanol concentration of 10 wt%, add tetra-neoalkoxy bis(didecylphosphite) titanate coupling agent, and the dosage is 1-2% of the mass of the silica powder; Magnetically stir at 60 °C for 6 hours to introduce active functional groups on the surface of the silica powder; Centrifuge and wash, with a centrifuge speed of 3500 rpm and a time of 5 minutes, to remove the unreacted coupling agent, and dry in vacuum for standby.

3. A novel surface modification method for silica fume according to claim 1, characterized in that, The specific process of the MXene preparation is: Add 2.4 g of LiF and 1.5 g of Ti3AlC2 to 30 mL of HCl in sequence, with the HCl concentration of 9 M, and then magnetically stir at 40 °C for at least 30 min to etch off the Al layer in Ti3AlC2; When the Al layer is completely etched and the Ti3AlC2 nanosheets are converted into Ti3C2Tx nanosheets, centrifugal washing is carried out at 3500 rpm for 5 minutes at room temperature of 25 °C until the upper layer of the liquid turns dark green; x When the Al layer is completely etched and the Ti3AlC2 nanosheets are converted into Ti3C2Tx nanosheets, centrifugal washing is carried out at 3500 rpm for 5 minutes at room temperature of 25 °C until the upper layer of the liquid turns dark green; Ultrasonically treat the above liquid in an ultrasonic treatment device at 40 °C for 15 minutes under the conditions of a power of 500 W and a frequency of 40 kHz; Alternately centrifuge and ultrasonically treat a total of 8 times to increase the MXene yield and obtain a few-layer MXene nanosheet dispersion.

4. A novel surface modification method for silica fume according to claim 1, characterized in that, The specific process of the composite material preparation is: Adopt hydrothermal in-situ growth, mix the modified silica powder and the MXene nanosheet dispersion in a mass ratio of 1:4, and ultrasonically disperse for 30 minutes; Transfer the mixed solution to a hydrothermal reaction kettle, control the filling degree at 70%-80%, and carry out hydrothermal reaction at 180 °C for 12 hours to enable the MXene nanosheets to grow in-situ on the surface of the silica powder to form a core-shell structure; Wash the reaction product 3 times with deionized water, centrifuge to remove the unreacted MXene, and freeze-dry or dry in vacuum to obtain the silica powder / MXene composite material.

5. A novel surface modification method for silica powder according to claim 1, characterized in that In Step 1, the coupling agent is tetra-neoalkoxy bis(didecylphosphite) titanate.

6. A novel surface modification method for silica powder according to claim 1, characterized in that, In Step 2, the particle size of the silica powder is 1-10 μm.

7. A novel method for surface modification of silica fume according to claim 1, characterized in that, In Step 2, the Ti3AlC2 is in powder form and the particle size < 38 μm.

8. A novel surface modification method for silica fume according to claim 1, characterized in that, In Step 5, the borate ester is trimethyl borate; The coating process is: Disperse the composite material: Disperse the silica powder / MXene composite material in anhydrous ethanol and ultrasonically treat for 30 minutes; Add borate: Add borate at 1-2% of the mass of the composite material; under nitrogen protection, stir magnetically for 6 hours (at room temperature) to make the borate uniformly adsorbed on the surface of the composite material; Heat treatment: Vacuum-dry the coated composite material at 80 °C for 12 hours to form stable chemical bonds between the borate and the surface of the composite material; Washing and drying: Wash 3 times with absolute ethanol to remove the unreacted borate; vacuum-dry to obtain the composite material with antioxidant treatment.

9. Application of the silicon micro powder / MXene composite material obtained by the novel surface modification method of silicon micro powder described in claims 1-8 in electromagnetic shielding, energy storage and flexible electronics.

Citation Information

Cited By

  • High-ion-selectivity perfluorosulfonic acid ionic membrane for vanadium battery as well as preparation method and application of high-ion-selectivity perfluorosulfonic acid ionic membrane