Preparation and application of metal complex mixed matrix membrane

By preparing carboxy functional groups-containing polyimide and cobalt nitrate hexahydrate to form a metal-coordinated polymer film, and using swelling to introduce 2-methylimidazole molecules, the problem of complex preparation of inorganic membranes and difficult to balance the selective permeability of polymer films is solved, and efficient helium separation performance is achieved.

CN120532322APending Publication Date: 2025-08-26ZINGKE (CHONGQING) ADVANCED MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510818450.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-18
Publication Date
2025-08-26

AI Technical Summary

Technical Problem

The preparation process of existing inorganic membranes is complex and costly. It is difficult to balance the selectivity and permeability of polymer membranes in gas separation, resulting in insufficient separation performance and difficulty in preparing an ideal hybrid matrix membrane.

Method used

By preparing a polyimide containing carboxyl functional groups, combining cobalt nitrate hexahydrate and 2-methylimidazole solution, a metal coordination polymer film is formed, and the 2-methylimidazole molecules are brought into the membrane through swelling to coordinate with cobalt to form a metal complex mixed matrix film.

Benefits of technology

It improves the interface compatibility of the metal complex hybrid matrix membrane, reduces interface voids, improves the separation performance and selectivity of He/CH4, and promotes the extraction of helium in natural gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120532322A_ABST
    Figure CN120532322A_ABST
Patent Text Reader

Abstract

The invention provides preparation and application of a metal complex mixed matrix membrane, and belongs to the fields of material science and gas separation. The preparation process comprises the following steps: preparing polyimide containing carboxyl functional groups; preparing a metal coordination polymer film; and preparing the metal complex mixed matrix membrane. The preparation method comprises the following steps: synthesizing a polyimide polymer containing a carboxyl functional group, coordinating the polyimide polymer with cobalt nitrate hexahydrate in a dissolved state to preliminarily form a metal coordinated polymer film, soaking the metal coordinated polymer film in a ligand solution formed by dissolving 2-methylimidazole in methanol, and carrying out vacuum drying to obtain the metal coordination polymer film. 2-methylimidazole molecules are brought into the membrane by utilizing the swelling effect of methanol on the membrane, and are subjected to coordination reaction with cobalt in a swelling space to form the metal complex mixed matrix membrane with ultrahigh selectivity, so that the separation performance and selectivity of the metal complex mixed matrix membrane on He / CH4 are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the fields of material science and gas separation, and in particular to the preparation and application of a metal complex mixed matrix membrane. Background Art

[0002] Helium plays an irreplaceable and important role in defense, healthcare, semiconductors, and industry. Extracting helium primarily from helium-rich natural gas is the only way to recycle helium resources. With the advancement of membrane separation technology, the future direction of helium extraction technology is to directly utilize membrane separation processes to enrich and recover helium from feed gas and low-grade helium in LNG tail gas.

[0003] Currently, membrane materials used for helium recovery and extraction include polymer membranes and inorganic membranes. Inorganic membranes, such as ceramic membranes and molecular sieve membranes, possess high thermal and chemical stability and exhibit certain advantages in the field of gas separation. However, inorganic membranes are complex to prepare and costly, and membrane defects and grain boundary problems are difficult to completely avoid, leading to non-selective gas permeation and reduced membrane separation performance. Polymer membranes, with their advantages of simple preparation and low cost, have been widely studied and applied in the field of gas separation. While they have the potential to overcome the trade-off between selectivity and permeability, achieving separation performance above the Robeson upper limit, the preparation of ideal mixed-matrix membranes is very difficult due to the differences in properties between the polymer and inorganic phases and the strong aggregation tendency of inorganic fillers.

[0004] Therefore, it is necessary to propose the preparation and application of a metal complex mixed matrix membrane with good separation performance and high selectivity. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a preparation and application of a metal complex mixed matrix membrane.

[0006] A process for preparing a metal complex mixed matrix membrane comprises the following steps:

[0007] S1: Preparation of polyimide containing carboxyl functional groups

[0008] 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid are dissolved in N-methylpyrrolidone, 4,4'-(hexafluoroisopropyl)diphthalic anhydride is added to react, and then acetic anhydride and pyridine are added to continue the reaction to obtain a polyimide containing a carboxyl functional group;

[0009] S2: Preparation of Metal Coordination Polymer Films

[0010] The carboxyl functional group-containing polyimide and cobalt nitrate hexahydrate are dissolved in N,N-dimethylformamide to prepare a polyimide solution and a cobalt nitrate solution, respectively. The polyimide solution is then added to the cobalt nitrate solution, stirred and mixed, and cast to obtain a metal coordination polymer film.

[0011] S3: Preparation of Metal Complex Mixed Matrix Membranes

[0012] 2-Methylimidazole is dissolved in anhydrous methanol, and the metal coordination polymer membrane is added thereto for soaking, and then rinsed with deionized water and vacuum dried to obtain a metal complex mixed matrix membrane.

[0013] Furthermore, S1 specifically includes the following steps:

[0014] S1.1: Under a nitrogen atmosphere, add equimolar amounts of 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid to N-methylpyrrolidone and stir thoroughly to dissolve. Then, add 4,4'-(hexafluoroisopropyl)phthalic anhydride at 0-5°C and continue stirring at room temperature for 16-32 hours to obtain a high molecular weight polyamic acid solution.

[0015] S1.2: Add acetic anhydride and pyridine to the above high molecular weight polyamic acid solution and continue stirring to react for 16-32 hours. Then pour it into anhydrous ethanol for precipitation, and then filter, wash and vacuum dry to obtain a polyimide containing carboxyl functional groups.

[0016] Furthermore, S2 specifically includes the following steps:

[0017] S2.1: Add the carboxyl-functional polyimide prepared in step S1.2 to N,N-dimethylformamide, stir thoroughly to dissolve, and prepare a 3-5 wt% polyimide solution;

[0018] S2.2: Add cobalt nitrate hexahydrate to N,N-dimethylformamide in a mass ratio of 1:(4-10), stir thoroughly to dissolve, and obtain a cobalt nitrate solution;

[0019] S2.3: Add the above polyimide solution to the above cobalt nitrate solution, stir for 3-8 hours, then cast it on a 5 cm × 5 cm glass plate, vacuum dry it at 90-110 ° C for 8-12 hours, elute with deionized water and vacuum dry it to obtain a metal coordination polymer film.

[0020] Furthermore, S3 specifically includes the following steps:

[0021] S3.1: Add 2-methylimidazole to anhydrous methanol at a solid-liquid ratio of 1 g:(20-30) mL and stir thoroughly to dissolve to obtain a 2-methylimidazole solution.

[0022] S3.2: Immerse the metal coordination polymer membrane obtained in step S2.3 in the above-mentioned 2-methylimidazole solution for 24-48 hours, take it out and rinse it with deionized water, then place it in a vacuum drying oven at 90-110°C and dry it for 24-48 hours to obtain a metal complex mixed matrix membrane.

[0023] Furthermore, the solid-liquid ratio of 2,4,6-trimethyl-1,3-diaminobenzene to N-methylpyrrolidone is 1 g: (30-36) mL.

[0024] Furthermore, the solid-liquid ratio of 4,4'-(hexafluoroisopropyl)phthalic anhydride to N-methylpyrrolidone is 1 g: (5.6-6) mL.

[0025] Furthermore, the volume ratios of acetic anhydride and pyridine to N-methylpyrrolidone are 1:(23-25) and 1:(2.6-2.8), respectively.

[0026] Furthermore, the volume ratio of the polyimide solution to the cobalt nitrate solution is (1-2):1.

[0027] Furthermore, the molar ratio of 2-methylimidazole to cobalt nitrate hexahydrate in the 2-methylimidazole solution is 10:1.

[0028] Furthermore, a metal complex mixed matrix membrane prepared by any of the above-mentioned processes for preparing metal complex mixed matrix membranes is used for selective separation and recovery of helium.

[0029] Compared with the prior art, the present invention has at least the following beneficial effects:

[0030] The present invention first synthesizes a polyimide polymer containing a carboxyl functional group, and then uses cobalt nitrate hexahydrate to coordinate with the polymer in a dissolved state to preliminarily form a metal-coordinated polymer membrane. The metal-coordinated polymer membrane is then immersed in a ligand solution formed by dissolving 2-methylimidazole in methanol. The swelling effect of methanol on the membrane is utilized to bring 2-methylimidazole molecules into the membrane, and a coordination reaction occurs with cobalt in the swelling space to form a metal complex mixed matrix membrane with ultra-high selectivity. The interface compatibility is improved, the generation of interface voids is reduced, and the separation performance and selectivity of the metal complex mixed matrix membrane for He / CH4 are improved, thereby facilitating helium extraction from natural gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable one skilled in the relevant art to make and use the present disclosure.

[0032] Figure 1This is a flow chart for preparing the metal complex mixed matrix membrane used in the embodiments of the present invention.

[0033] Figure 2 Schematic diagram of the He / CH4 selectivity of the membrane materials prepared in Examples 1-3 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The preparation and application of a metal complex mixed matrix membrane provided by the present invention are described in detail below with reference to the accompanying drawings and specific examples.

[0035] Example 1

[0036] A process for preparing a metal complex mixed matrix membrane, such as Figure 1 As shown, the following steps are included:

[0037] S1: Preparation of polyimide containing carboxyl functional groups

[0038] S1.1: Under a nitrogen atmosphere, add equimolar amounts of 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid to N-methylpyrrolidone and stir thoroughly to dissolve. Then, add 4,4'-(hexafluoroisopropyl)diphthalic anhydride at 0°C and continue stirring at room temperature for 16 hours to obtain a high molecular weight polyamic acid solution, wherein the solid-to-liquid ratio of 2,4,6-trimethyl-1,3-diaminobenzene to N-methylpyrrolidone is 1 g:30 mL, and the solid-to-liquid ratio of 4,4'-(hexafluoroisopropyl)diphthalic anhydride to N-methylpyrrolidone is 1 g:5.6 mL.

[0039] S1.2: Adding acetic anhydride and pyridine to the high molecular weight polyamic acid solution and continuing the reaction with stirring for 16 hours, then pouring the mixture into anhydrous ethanol for precipitation, filtering, washing, and vacuum drying to obtain a carboxyl-functional polyimide, wherein the volume ratios of acetic anhydride and pyridine to N-methylpyrrolidone are 1:23 and 1:2.6, respectively;

[0040] S2: Preparation of Metal Coordination Polymer Films

[0041] S2.1: Add the carboxyl functional group-containing polyimide prepared in step S1.2 to N,N-dimethylformamide, stir thoroughly to dissolve, and prepare a 3 wt% polyimide solution;

[0042] S2.2: Add cobalt nitrate hexahydrate to N,N-dimethylformamide in a mass ratio of 1:4 and stir thoroughly to dissolve to obtain a cobalt nitrate solution;

[0043] S2.3: Add the polyimide solution to the cobalt nitrate solution, stir for 3 h, and cast the resulting mixture onto a 5 cm × 5 cm glass plate. Dry the mixture in a vacuum at 90°C for 8 h, then wash with deionized water and dry in a vacuum to obtain a metal coordination polymer film. The volume ratio of the polyimide solution to the cobalt nitrate solution is 1:1.

[0044] S3: Preparation of Metal Complex Mixed Matrix Membranes

[0045] S3.1: Add 2-methylimidazole to anhydrous methanol at a solid-liquid ratio of 1 g:20 mL and stir thoroughly to dissolve to obtain a 2-methylimidazole solution.

[0046] S3.2: Immerse the metal coordination polymer membrane obtained in step S2.3 in the above-mentioned 2-methylimidazole solution. After soaking for 24 hours, take it out and rinse it with deionized water. Then place it in a vacuum drying oven at 90°C and dry it for 24 hours to obtain a metal complex mixed matrix membrane, wherein the molar ratio of 2-methylimidazole to cobalt nitrate hexahydrate in the 2-methylimidazole solution is 10:1.

[0047] Example 2

[0048] A process for preparing a metal complex mixed matrix membrane, such as Figure 1 As shown, the following steps are included:

[0049] S1: Preparation of polyimide containing carboxyl functional groups

[0050] S1.1: Under a nitrogen atmosphere, add equimolar amounts of 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid to N-methylpyrrolidone and stir thoroughly to dissolve. Then, add 4,4'-(hexafluoroisopropyl)diphthalic anhydride at 3°C ​​and continue stirring at room temperature for 24 hours to obtain a high molecular weight polyamic acid solution, wherein the solid-to-liquid ratio of 2,4,6-trimethyl-1,3-diaminobenzene to N-methylpyrrolidone is 1 g:33 mL, and the solid-to-liquid ratio of 4,4'-(hexafluoroisopropyl)diphthalic anhydride to N-methylpyrrolidone is 1 g:5.8 mL.

[0051] S1.2: Adding acetic anhydride and pyridine to the high molecular weight polyamic acid solution and continuing the reaction with stirring for 24 hours, then pouring the mixture into anhydrous ethanol for precipitation, filtering, washing, and vacuum drying to obtain a carboxyl-functional polyimide, wherein the volume ratios of acetic anhydride and pyridine to N-methylpyrrolidone are 1:24 and 1:2.7, respectively;

[0052] S2: Preparation of Metal Coordination Polymer Films

[0053] S2.1: Add the carboxyl-functional polyimide prepared in step S1.2 to N,N-dimethylformamide, stir thoroughly to dissolve, and prepare a 4 wt% polyimide solution;

[0054] S2.2: Add cobalt nitrate hexahydrate to N,N-dimethylformamide in a mass ratio of 1:7 and stir thoroughly to dissolve to obtain a cobalt nitrate solution;

[0055] S2.3: Add the polyimide solution to the cobalt nitrate solution, stir for 5 h, and cast the resulting mixture onto a 5 cm × 5 cm glass plate. Dry the mixture under vacuum at 100°C for 10 h, then wash with deionized water and dry the mixture under vacuum to obtain a metal coordination polymer film. The volume ratio of the polyimide solution to the cobalt nitrate solution is 1.5:1.

[0056] S3: Preparation of Metal Complex Mixed Matrix Membranes

[0057] S3.1: Add 2-methylimidazole to anhydrous methanol at a solid-liquid ratio of 1 g:25 mL and stir thoroughly to dissolve to obtain a 2-methylimidazole solution.

[0058] S3.2: Immerse the metal coordination polymer membrane obtained in step S2.3 in the above-mentioned 2-methylimidazole solution. After soaking for 36 hours, take it out and rinse it with deionized water. Then place it in a vacuum drying oven at 100°C and dry it for 36 hours to obtain a metal complex mixed matrix membrane, wherein the molar ratio of 2-methylimidazole to cobalt nitrate hexahydrate in the 2-methylimidazole solution is 10:1.

[0059] Example 3

[0060] A process for preparing a metal complex mixed matrix membrane, such as Figure 1 As shown, the following steps are included:

[0061] S1: Preparation of polyimide containing carboxyl functional groups

[0062] S1.1: Under a nitrogen atmosphere, add equimolar amounts of 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid to N-methylpyrrolidone and stir thoroughly to dissolve. Then, add 4,4'-(hexafluoroisopropyl)phthalic anhydride at 5°C and continue stirring at room temperature for 32 hours to obtain a high molecular weight polyamic acid solution, wherein the solid-to-liquid ratio of 2,4,6-trimethyl-1,3-diaminobenzene to N-methylpyrrolidone is 1 g:36 mL, and the solid-to-liquid ratio of 4,4'-(hexafluoroisopropyl)phthalic anhydride to N-methylpyrrolidone is 1 g:6 mL.

[0063] S1.2: Adding acetic anhydride and pyridine to the high molecular weight polyamic acid solution and continuing the reaction with stirring for 16-32 hours, then pouring into anhydrous ethanol for precipitation, filtering, washing, and vacuum drying to obtain a carboxyl-functional polyimide, wherein the volume ratios of acetic anhydride and pyridine to N-methylpyrrolidone are 1:25 and 1:2.8, respectively;

[0064] S2: Preparation of Metal Coordination Polymer Films

[0065] S2.1: Add the carboxyl functional group-containing polyimide prepared in step S1.2 to N,N-dimethylformamide, stir thoroughly to dissolve, and prepare a 5 wt% polyimide solution;

[0066] S2.2: Add cobalt nitrate hexahydrate to N,N-dimethylformamide in a mass ratio of 1:10 and stir thoroughly to dissolve to obtain a cobalt nitrate solution;

[0067] S2.3: Add the polyimide solution to the cobalt nitrate solution and stir for 8 h. Then, cast the solution onto a 5 cm × 5 cm glass plate and vacuum dry at 110°C for 12 h. Then, wash with deionized water and vacuum dry to obtain a metal coordination polymer film. The volume ratio of the polyimide solution to the cobalt nitrate solution is 2:1.

[0068] S3: Preparation of Metal Complex Mixed Matrix Membranes

[0069] S3.1: Add 2-methylimidazole to anhydrous methanol at a solid-liquid ratio of 1 g:30 mL and stir thoroughly to dissolve to obtain a 2-methylimidazole solution.

[0070] S3.2: Immerse the metal coordination polymer membrane obtained in step S2.3 in the above-mentioned 2-methylimidazole solution. After soaking for 48 hours, take it out and rinse it with deionized water. Then place it in a vacuum drying oven at 110°C and dry it for 48 hours to obtain a metal complex mixed matrix membrane, wherein the molar ratio of 2-methylimidazole to cobalt nitrate hexahydrate in the 2-methylimidazole solution is 10:1.

[0071] Comparative Example 1

[0072] The difference between this comparative example 1 and embodiment 1 is:

[0073] The cobalt nitrate solution in step S2.3 was removed, and the polyimide solution was directly cast on a 5 cm × 5 cm glass plate to make a membrane material, and the membrane material was directly immersed in methanol to make a polymer membrane. The other processes were the same.

[0074] Performance testing:

[0075] The He / CH4 selectivity of the membranes prepared in Examples 1-3 and Comparative Example 1 was tested respectively. The results are as follows: Figure 2shown.

[0076] from Figure 2 It can be seen that the He / CH4 selectivity of the polymer membrane prepared in Comparative Example 1 without using a metal complex is significantly lower than that in Example 1. This shows that by first synthesizing a polyimide polymer containing a carboxyl functional group, and then using cobalt nitrate hexahydrate to coordinate with it in a dissolved state, a metal-coordinated polymer membrane is preliminarily formed, and then the metal-coordinated polymer membrane is immersed in a ligand solution formed by dissolving 2-methylimidazole in methanol. By utilizing the swelling effect of methanol on the membrane, 2-methylimidazole molecules are brought into the membrane, and a coordination reaction occurs with cobalt in the swelling space to form a metal complex mixed matrix membrane with ultra-high selectivity, which improves the interface compatibility and reduces the generation of interface voids, thereby improving the separation performance and selectivity of the metal complex mixed matrix membrane for He / CH4, thereby contributing to helium extraction from natural gas.

[0077] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical principles disclosed herein are intended to be covered by the claims of the present invention.

Claims

1. A process for preparing a metal complex mixed matrix membrane, characterized in that: The steps include: S1: Preparation of polyimide containing carboxyl functional groups 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid are dissolved in N-methylpyrrolidone, 4,4'-(hexafluoroisopropyl)diphthalic anhydride is added to react, and then acetic anhydride and pyridine are added to continue the reaction to obtain a polyimide containing a carboxyl functional group; S2: Preparation of Metal Coordination Polymer Films The carboxyl functional group-containing polyimide and cobalt nitrate hexahydrate are dissolved in N,N-dimethylformamide to prepare a polyimide solution and a cobalt nitrate solution, respectively. The polyimide solution is then added to the cobalt nitrate solution, stirred and mixed, and cast to obtain a metal coordination polymer film. S3: Preparation of Metal Complex Mixed Matrix Membranes 2-Methylimidazole is dissolved in anhydrous methanol, and the metal coordination polymer membrane is added thereto for soaking, and then rinsed with deionized water and vacuum dried to obtain a metal complex mixed matrix membrane.

2. The process for preparing a metal complex mixed matrix membrane according to claim 1, characterized in that: S1 specifically includes the following steps: S1.1: Under a nitrogen atmosphere, add equimolar amounts of 2,4,6-trimethyl-1,3-diaminobenzene and 3,5-diaminobenzoic acid to N-methylpyrrolidone and stir thoroughly to dissolve. Then, add 4,4'-(hexafluoroisopropyl)phthalic anhydride at 0-5°C and continue stirring at room temperature for 16-32 hours to obtain a high molecular weight polyamic acid solution. S1.2: Add acetic anhydride and pyridine to the above high molecular weight polyamic acid solution and continue stirring to react for 16-32 hours. Then pour it into anhydrous ethanol for precipitation, and then filter, wash and vacuum dry to obtain a polyimide containing carboxyl functional groups.

3. The process for preparing a metal complex mixed matrix membrane according to claim 2, wherein: S2 specifically includes the following steps: S2.1: Add the carboxyl-functional polyimide prepared in step S1.2 to N,N-dimethylformamide, stir thoroughly to dissolve, and prepare a 3-5 wt% polyimide solution; S2.2: Add cobalt nitrate hexahydrate to N,N-dimethylformamide in a mass ratio of 1:(4-10), stir thoroughly to dissolve, and obtain a cobalt nitrate solution; S2.3: Add the above polyimide solution to the above cobalt nitrate solution, stir for 3-8 hours, then cast it on a 5 cm × 5 cm glass plate, vacuum dry it at 90-110 ° C for 8-12 hours, elute with deionized water and vacuum dry it to obtain a metal coordination polymer film.

4. The process for preparing a metal complex mixed matrix membrane according to claim 3, wherein: S3 specifically includes the following steps: S3.1: Add 2-methylimidazole to anhydrous methanol at a solid-liquid ratio of 1 g:(20-30) mL and stir thoroughly to dissolve to obtain a 2-methylimidazole solution. S3.2: Immerse the metal coordination polymer membrane obtained in step S2.3 in the above-mentioned 2-methylimidazole solution for 24-48 hours, take it out and rinse it with deionized water, then place it in a vacuum drying oven at 90-110°C and dry it for 24-48 hours to obtain a metal complex mixed matrix membrane.

5. The process for preparing a metal complex mixed matrix membrane according to claim 2, wherein: The solid-liquid ratio of 2,4,6-trimethyl-1,3-diaminobenzene to N-methylpyrrolidone is 1g:(30-36)mL.

6. The process for preparing a metal complex mixed matrix membrane according to claim 2, wherein: The solid-liquid ratio of 4,4'-(hexafluoroisopropyl)phthalic anhydride to N-methylpyrrolidone is 1g:(5.6-6)mL.

7. The process for preparing a metal complex mixed matrix membrane according to claim 2, wherein: The volume ratios of acetic anhydride and pyridine to N-methylpyrrolidone are 1:(23-25) and 1:(2.6-2.8), respectively.

8. The process for preparing a metal complex mixed matrix membrane according to claim 3, characterized in that: The volume ratio of the polyimide solution to the cobalt nitrate solution is (1-2):

1.

9. The process for preparing a metal complex mixed matrix membrane according to claim 4, characterized in that: The molar ratio of 2-methylimidazole to cobalt nitrate hexahydrate in the 2-methylimidazole solution is 10:

1.

10. A metal complex mixed matrix membrane prepared by the process for preparing a metal complex mixed matrix membrane according to any one of claims 1 to 9, characterized in that: Applied to the selective separation and recovery of helium.