Wear-resistant coating for bearing as well as preparation method and application of wear-resistant coating
By preparing polyamide-imide resin powder containing hydrophobic groups and a coating of modified reinforcing phase, the problem of high water absorption rate of amide-based materials in high humidity environments was solved, improving the tribological and mechanical properties of bearings and extending their service life.
Patent Information
- Application Number
- CN202511619354.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-06
- Publication Date
- 2026-04-10
AI Technical Summary
Existing amide-based bearing coatings have high water absorption rates and poor dimensional stability in high-humidity environments, leading to severe bearing wear, high frictional noise, and short service life. Furthermore, the existing polyamide-imide coatings have insufficient tribological and mechanical properties, making it difficult to meet the requirements of bearings using water as a lubricating medium.
Wear-resistant coatings are prepared by using polyamide-imide resin powder containing hydrophobic groups, modified fibrous and powdered reinforcing phases, and heat treatment, etching, coupling agent treatment and acid treatment. Combined with a lubricating phase, a self-lubricating and low water absorption coating is formed, which enhances the mechanical and tribological properties of the coating.
It significantly reduces the water absorption rate of the coating, improves the tribological and mechanical properties of the bearing, reduces wear, extends bearing life, reduces the probability of mechanical failure, and is suitable for bearing use in high humidity environments.
Smart Images

Figure SMS_2
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of high polymer coating and relates to a wear-resistant coating for bearings as well as a preparation method and application thereof. BACKGROUND
[0002] Compared with traditional oil-lubricated metal bearings, bearings using water as lubricating medium can avoid pollution of water bodies by lubricating oil and are important components of marine equipment transmission systems. However, water as lubricating medium has certain limitations compared with lubricating oil. Water has a low viscosity, and when the shaft system is in a low-speed or start-stop working condition, the load-carrying capacity in forming a hydrodynamic film is limited, and it is difficult to form a complete lubricating film on the bearing surface, which is in a boundary lubrication state, and the contact between the friction pairs cannot be avoided. This will cause excessive wear of the bearing material and generate a large amount of friction noise, which seriously threatens the reliability of the marine equipment transmission system and the service life of the bearing.
[0003] High polymer materials represented by amide-based materials can be used as wear-resistant coatings and applied to bearings due to their good friction resistance, which is a current research hotspot. However, existing amide-based materials have the characteristic of high water absorption, which makes it difficult to prove the dimensional stability of the coating in a high-humidity environment. Once the coating absorbs water and deforms, it will cause the bearing to seize, which makes it difficult to be applied to bearings using water as lubricating medium. In addition, under the action of the main shaft and water pressure, the bearing load-carrying part is prone to deformation, the bearing gap is reduced, the contact area between the bearing and the sleeve is increased, and the friction load is increased. However, the existing polyamide-imide wear-resistant coating cannot simultaneously have excellent tribological properties and mechanical properties, which leads to serious wear of the bearing substrate material and generates a large amount of friction noise, resulting in a short service life of the bearing. In addition, the content of polyamide-imide in the existing polyamide-imide wear-resistant coating is low, and as a result, when foreign hard points or detached debris wrap the bearing surface, the journal is easily scratched, which further causes frequent mechanical failure.
[0004] Therefore, it is necessary to propose a self-lubricating, low-water-absorption, high-load-bearing wear-resistant high polymer coating. SUMMARY
[0005] The technical problem to be solved by the present application is to overcome the shortcomings of the prior art and provide a wear-resistant coating for bearings with low water absorption, good self-lubricating performance and high load-carrying capacity as well as a preparation method and application thereof.
[0006] To solve the above technical problems, the present application adopts the following technical solutions: A wear-resistant coating for bearings, the preparation raw materials of the wear-resistant coating at least include a polyamide-imide resin powder containing a hydrophobic group, a lubricating phase and a modified reinforcing phase; the modified reinforcing phase includes a modified fibrous reinforcing phase and a modified powdery reinforcing phase; the modified fibrous reinforcing phase is prepared by treating a fibrous reinforcing phase with degumming, etching and a coupling agent; and the modified powdery reinforcing phase is prepared by treating a powdery reinforcing phase with surface pretreatment and acidification.
[0007] The wear-resistant coating for bearings is further improved, and the mass ratio of the modified fibrous reinforcing phase to the modified powdery reinforcing phase is 1-2:1-10.
[0008] The wear-resistant coating for bearings is further improved, and the modified fibrous reinforcing phase is prepared by treating a fibrous reinforcing phase with degumming, etching and a coupling agent, including the following steps: S11, heat treating the fibrous reinforcing phase to remove surface gum impurities; S12, etching the heat-treated fibrous reinforcing phase by mixing with an acid solution; S13, hydrolyzing the etched fibrous reinforcing phase by mixing with a coupling agent solution to obtain the modified fibrous reinforcing phase; The wear-resistant coating for bearings is further improved, and the modified powdery reinforcing phase is prepared by treating a powdery reinforcing phase with surface pretreatment and acidification, including the following steps: S21, surface pretreating the powdery reinforcing phase to remove surface impurities; S22, acidifying the surface pretreated powdery reinforcing phase by mixing with an acid solution to obtain the modified powdery reinforcing phase.
[0009] The wear-resistant coating for bearings is further improved, and the preparation method of the modified fibrous reinforcing phase at least meets at least one of the following preparation conditions (1.11) to (1.23): (1.11) In step S11, the diameter of the fibrous reinforcing phase is 4-12 μm, and the length is 0.1-1.5 mm; the fibrous reinforcing phase includes at least one of glass fiber powder, carbon fiber powder, basalt fiber powder, ceramic-based whisker and inorganic salt whisker; the ceramic-based whisker includes at least one of SiC, Si3N4, potassium titanate and aluminum borate; and the inorganic salt whisker includes at least one of calcium sulfate and calcium carbonate; (1.12) In step S11, the heat treatment is performed in an air atmosphere; (1.13) In step S11, the heat treatment is performed at a temperature of 350-450°C; (1.14) In step S11, the heat treatment is performed for 30 min to 60 min; (1.15) In step S12, the acid solution is at least one of nitric acid and sulfuric acid; (1.16) In step S12, the acid solution has a volume fraction of 10% to 30%; (1.17) In step S12, the etching is performed at a temperature of 60°C to 80°C; (1.18) In step S12, the etching is performed for 20 min to 30 min, and after the etching is completed, the etching product is washed with water until the pH value of the washing liquid is neutral; (1.19) In step S13, the coupling agent solution is prepared by dissolving a coupling agent in a mixed solvent of ethanol and water; the coupling agent is at least one of KH550, KH560, and KH570; and the mass ratio of ethanol to water in the mixed solvent of ethanol and water is 8 to 13:1; (1.20) In step S13, the coupling agent solution has a mass fraction of 3% to 8%; (1.21) In step S13, the hydrolysis reaction is performed for 2 h to 3 h; (1.22) In step S13, the hydrolysis reaction is performed under ultrasonic conditions; (1.23) In step S13, after the hydrolysis reaction is completed, the reaction product is subjected to a drying treatment; the drying treatment is performed at a temperature of 70°C to 90°C; and the drying treatment is performed for 2 h to 3 h.
[0010] The bearing wear-resistant coating described above is further improved, and the preparation method of the modified powder-shaped reinforcing phase at least meets at least one of the following preparation conditions (2.11) to (2.18): (2.11) In step S21, the particle size of the powder-shaped reinforcing phase is 500 nm to 50 μm; and the powder-shaped reinforcing phase includes at least one of carbon nanotubes, hexagonal boron nitride, graphene, and silicon carbide powder; (2.12) In step S21, the surface pretreatment is performed in an air atmosphere; (2.13) In step S21, the surface pretreatment is performed at a temperature of 500°C to 700°C; (2.14) In step S21, the surface pretreatment is performed for 1 h to 1.5 h; (2.15) In step S22, the acid solution is at least one of hydrofluoric acid, nitric acid, and sulfuric acid; (2.16) In step S22, the acid solution has a volume fraction of 10% to 30%; (2.17) In step S22, the acidification reaction takes 1 to 2 hours; (2.18) In step S12, the acidification reaction is completed and the following treatment is also included: washing the product after the acidification reaction with water until the pH value of the washing solution is neutral.
[0011] In a further improvement to the aforementioned wear-resistant coating for bearings, the hydrophobic groups in the polyamide-imide resin powder containing hydrophobic groups are at least one of ether bonds and fluorinated alkyl groups.
[0012] The aforementioned wear-resistant coating for bearings is further improved by wherein the polyamide-imide resin powder containing hydrophobic groups is prepared by imidization reaction using trimellitic anhydride acyl chloride and diamine monomers containing hydrophobic groups as raw materials.
[0013] The above-mentioned wear-resistant coating for bearings is further improved by a method for preparing the polyamide-imide resin powder containing hydrophobic groups, which includes the following steps: S31. A diamine monomer containing a hydrophobic group is mixed with an organic solvent A and stirred to obtain solution A; wherein the organic solvent A is an aprotic polar solvent. S32. Add trimellitic anhydride chloride to solution A in batches and stir to obtain solution B; S33. Add the acid-binding agent to solution B to react and obtain solution C; S34. The imidizing reagent is added to solution C to react and obtain solution D; S35. Add solution D to deionized water, precipitate, crush, wash with water, filter, and dry to obtain polyamide-imide resin powder containing hydrophobic groups.
[0014] The aforementioned wear-resistant coating for bearings is further improved by wherein the preparation method of the polyamide-imide resin powder containing hydrophobic groups satisfies at least one of the following preparation conditions (3.11) to (3.18): (3.11) In step S31, the diamine monomer containing a hydrophobic group is an ether-bonded diamine monomer and / or a trifluoromethyl diamine monomer; the ether-bonded diamine monomer includes at least one of m-phenylenediamine, 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, and 1,3-bis(4-aminophenoxy)benzene; the trifluoromethyl diamine monomer includes at least one of 2,2′-bis(trifluoromethyl)-4,4-diaminobiphenyl, 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether, 1,4-bis(2-trifluoromethyl4-aminophenoxy)benzene, and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane; (3.12) In step S31, the aprotic polar solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; (3.13) In step S32, the molar ratio of the diamine monomer containing a hydrophobic group to the trimellitic anhydride acyl chloride in solution A is 0.9:1 to 1.1:1; the temperature of solution A is 0 to 5°C; (3.14) In step S33, the molar ratio of the acid-binding agent to the trimellitic anhydride acyl chloride in solution B is 1 to 1.5:1; the acid-binding agent is triethylamine; (3.15) In step S33, the reaction is carried out at a temperature of 60℃~65℃; the reaction time is 12h~24h; (3.16) In step S34, the imidizing agent is a mixture of acetic anhydride and triethylamine; the molar ratio of acetic anhydride to triethylamine is 0.5 to 2:1; (3.17) In step S34, the reaction is carried out at a temperature of 60℃~65℃; the reaction time is 12h~24h; (3.18) In step S35, the drying is carried out under vacuum conditions; the drying temperature is 100℃~150℃; and the drying time is 10h~24h.
[0015] The above-mentioned wear-resistant coating for bearings is further improved by including the following raw materials for preparing the wear-resistant coating: organic solvent B, additives, and pigments and fillers.
[0016] The aforementioned wear-resistant coating for bearings is further improved in that the raw materials for preparing the wear-resistant coating are, by weight, the following: 90 to 200 parts of polyamide-imide resin powder containing hydrophobic groups. Lubricating phase: 5 to 50 parts 5 to 30 parts of modified reinforcing phase, Organic solvent B: 400-1500 parts 12 to 35 parts of auxiliary agent 1 to 4 parts pigment.
[0017] In a further improvement to the aforementioned wear-resistant coating for bearings, the lubricating phase includes at least one of polytetrafluoroethylene micropowder, graphite, molybdenum disulfide, and tungsten disulfide.
[0018] In a further improvement to the aforementioned wear-resistant coating for bearings, the organic solvent B is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.
[0019] In a further improvement to the aforementioned wear-resistant coating for bearings, the additives include at least one of a dispersant, a defoamer, a leveling agent, and an anti-settling agent.
[0020] The aforementioned wear-resistant coating for bearings is further improved by comprising at least one of chrome green, iron chromium black, and carbon black as the filler.
[0021] As a general technical concept, the present invention also provides a method for preparing the above-mentioned wear-resistant coating for bearings, comprising the following steps: S41. A polyamide-imide coating is prepared from raw materials including polyamide-imide resin powder containing hydrophobic groups, a lubricating phase, and a modified reinforcing phase. S42. Spray the polyamide-imide coating obtained in step S41 onto the bearing surface to form a polyamide-imide wet film on the bearing surface. S43. Dry the polyamide-imide wet film formed on the bearing surface in step S42 to form a polyamide-imide coating on the bearing surface; S44. Repeat steps S42 and S43 until the thickness of the polyamide-imide coating reaches the set target. S45. The polyamide-imide coating obtained in step S44 is cured to obtain a wear-resistant coating.
[0022] In a further improvement to the above preparation method, in step S41, the solid content of the polyamide-imide coating is 5wt% to 30wt%.
[0023] In a further improvement to the above preparation method, in step S41, when the raw materials are polyamide-imide resin powder containing hydrophobic groups, a lubricating phase and a modified reinforcing phase, organic solvent B, additives and pigments, the preparation method of the polyamide-imide coating includes the following steps: (1) Add the polyamide-imide resin powder containing hydrophobic groups to organic solvent B and stir at 150 rpm to 200 rpm to obtain a polyamide-imide resin solution. (2) Filter the polyamide-imide resin solution, add the lubricating phase, the modified reinforcing phase, the additives and the pigment, and stir at 600 rpm to 800 rpm for 2 to 3 hours to obtain the mixture. (3) Grind, filter and degas the mixture to obtain polyamide-imide coating.
[0024] In a further improvement to the above preparation method, in step S42, the polyamide-imide coating prepared in step S41 is sprayed onto the bearing surface using an air spraying method or an electrostatic spraying method; the bearing also includes the following pretreatment before use: removing grease and rust from the bearing surface, sandblasting the bearing surface, cleaning the surface, drying the bearing surface with compressed air, and preheating at 50℃~60℃ for 15min~20min.
[0025] In a further improvement to the above preparation method, in step S43, the drying temperature is 80℃~120℃; the drying time is 20min~30min; and the thickness of the polyamide-imide coating formed on the bearing surface in a single step is 10μm~50μm.
[0026] In a further improvement to the above preparation method, in step S44, the target thickness of the polyamide-imide coating is 30 μm to 50 μm.
[0027] In a further improvement to the above preparation method, in step S45, the curing is as follows: heating to 70℃~90℃ at a heating rate of 1℃ / min~3℃ / min and curing for 20min~40min; heating to 140℃~160℃ at a heating rate of 3℃ / min~5℃ / min and curing for 20min~40min; heating to 260℃~280℃ at a heating rate of 5℃ / min~10℃ / min and curing for 20min~40min.
[0028] As a general technical concept, the present invention also provides an application of a wear-resistant coating in bearing manufacturing, wherein the bearing surface is loaded with the above-mentioned wear-resistant coating; or the wear-resistant coating loaded on the bearing surface is prepared by the above-mentioned preparation method.
[0029] Compared with the prior art, the advantages of the present invention are as follows: (1) In view of the shortcomings of existing wear-resistant coatings for bearings, such as low load-bearing capacity, high friction and wear, high water absorption, and the resulting inability to meet the use requirements of bearings, this invention creatively proposes a wear-resistant coating for bearings. The raw materials for preparing the wear-resistant coating include at least polyamide-imide resin powder containing hydrophobic groups, a lubricating phase and a modified reinforcing phase. The modified reinforcing phase includes a modified fibrous reinforcing phase and a modified powder reinforcing phase. The modified fibrous reinforcing phase is prepared by degumming, etching and coupling agent treatment of the fibrous reinforcing phase. The modified powder reinforcing phase is prepared by surface pretreatment and acid treatment of the powder reinforcing phase. Compared to conventional polyamide-imide resins, this invention introduces hydrophobic groups into the polyamide-imide resin, enabling the wear-resistant coating to form a hydrophobic barrier. This reduces the coating's water absorption rate, effectively maintaining its dimensional stability and allowing it to operate in high-humidity environments. Simultaneously, a lubricating phase and a modified reinforcing phase are added to the coating formulation. Compared to conventional lubricating and reinforcing phases, the lubricating phase used in this invention exhibits better self-lubricating properties and a lower coefficient of friction, facilitating the formation of a friction film within the coating and significantly reducing the coefficient of friction. The modified reinforcing phase, with its higher strength, significantly improves the coating's mechanical properties and reduces wear. In particular, the fibrous and powdered modified reinforcing phases have a synergistic effect. The combined effect of powder reinforcement and fiber toughening achieves a balance between stiffness and toughness, while simultaneously improving fatigue resistance. Adding only fibers results in insufficient wear resistance, while adding only powder leads to brittleness, poor impact resistance, and weak adhesion to the substrate. More importantly, the combined effect of both significantly improves the performance of the wear-resistant coating. Specifically: (a) the resulting wear-resistant coating isolates the metal substrate from direct friction, providing a buffering and noise reduction effect; (b) the hardness of the resulting wear-resistant coating is lower than that of the bearing's metal substrate, exhibiting good frictional compliance and adapting to minor shaft deformation and eccentric loading; (c) it improves the tribological and mechanical properties of the wear-resistant coating, reduces the coating's friction coefficient and wear amount, and increases the bearing's service life. Furthermore, the combined action of polyamide-imide resin powder containing hydrophobic groups, the lubricating phase, and the modified reinforcing phase gives the wear-resistant coating excellent embedding properties, effectively encapsulating and embedding external hard particles or detached debris, protecting the journal from scratches and reducing the probability of mechanical failure. Furthermore, the synergistic effect of the polyamide-imide resin powder containing hydrophobic groups, the lubricating phase, and the modified reinforcing phase enables the coating to be used for extended periods under conditions of high humidity and heavy loads. Compared to conventional polyamide-imide resin-based wear-resistant materials, the wear-resistant coating of this invention exhibits lower water absorption, better self-lubrication, and higher load-bearing capacity. It can be widely used in bearing manufacturing, not only meeting the requirements for use in high-humidity environments but also significantly reducing the occurrence of mechanical failures, thus extending the service life of bearings.
[0030] (2) In the wear-resistant coating for bearings of the present invention, the mass ratio of modified fibrous reinforcing phase to modified powder reinforcing phase is optimized to be 1-2:1-10, with a preferred range of 1:1-3, which can achieve a balance between toughening and reinforcement and improve the service life of the coating. If there is too much modified fibrous reinforcing phase, the wear resistance of the coating will decrease. At the same time, too much modified fibrous reinforcing phase is not conducive to dispersion and is easy to agglomerate in the coating, which will reduce the performance of the coating. If there is too much modified powder reinforcing phase, the hardness of the coating will be too high and the overall friction coefficient of the coating will increase. Under impact or vibration, cracks are easily generated, resulting in large-area peeling.
[0031] (3) In the wear-resistant coating for bearings of the present invention, the hydrophobic groups in the polyamide-imide resin powder containing hydrophobic groups are at least one of ether bonds and fluorinated alkyl groups. The ether bonds are weakly polar, which can reduce the water absorption rate of the polyamide-imide coating. Moreover, the ether bonds can appropriately improve the flexibility of the polyamide-imide molecular chain, improve the mechanical properties of the material and the fluidity of the coating, and reduce defects such as pinholes and bubbles during spraying. At the same time, most of the fluorinated alkyl groups are non-polar groups, which can effectively reduce the water absorption rate of the coating and play a steric hindrance effect in the polyamide-imide molecular chain, hindering the movement between polyamide-imide molecular chain segments and improving the environmental stability of the polyamide-imide coating. At the same time, the introduction of ether bonds and fluorinated alkyl groups into the polyamide-imide resin can achieve the upgrading of the polyamide-imide coating's high temperature resistance, impact resistance, low water absorption, and chemical stability through their complementarity. In addition, other hydrophobic groups, such as long-chain alkyl groups, have poor compatibility with polyamide-imide molecular chains and poor high-temperature resistance, which will lead to a decrease in the mechanical properties and high-temperature resistance of the material; phenyl and substituted phenyl groups have weak hydrophobicity and strong rigidity, which will lead to a decrease in the impact resistance of the material, while the improvement in hydrophobicity is not significant, making it difficult to apply to bearings.
[0032] (4) In the wear-resistant coating for bearings of the present invention, the amount of polyamide-imide resin powder containing hydrophobic groups is optimized to 90-200 parts, and the solid content of the polyamide-imide coating is 5-30 wt%, which is more suitable for preparing the polyamide-imide coating by spraying process. At the same time, the thickness of the polyamide-imide coating is more matched with that of the wear-resistant coating. However, if the solid content is too low, the curing process will cause defects such as pinholes and shrinkage cavities in the coating, and the coating thickness will be too thin. To achieve the target thickness, multiple sprayings are required, which increases the cost. At the same time, sagging will occur, affecting the coating performance. If the solid content is too high, the viscosity of the coating will be too high, the fluidity will be poor, the spraying difficulty will be increased, and the coating thickness will be uneven, resulting in poor film quality. In particular, excessive local thickness of the coating will easily lead to incomplete curing and a decrease in mechanical properties. Detailed Implementation
[0033] The present invention will be further described below with reference to specific preferred embodiments, but this does not limit the scope of protection of the present invention.
[0034] Example 1 A wear-resistant coating for bearings, wherein the raw materials for preparing the wear-resistant coating include at least polyamide-imide resin powder containing hydrophobic groups, a lubricating phase, and a modified reinforcing phase. The modified reinforcing phase includes a modified fibrous reinforcing phase and a modified powdered reinforcing phase. The modified fibrous reinforcing phase is prepared by degumming, etching, and coupling agent treatment of the fibrous reinforcing phase. The modified powdered reinforcing phase is prepared by surface pretreatment and acidification treatment of the powdered reinforcing phase.
[0035] In this embodiment, the mass ratio of the modified fibrous reinforcing phase to the modified powdered reinforcing phase is 1:1.
[0036] In this embodiment, the modified fibrous reinforcing phase is prepared by desizing, etching, and coupling agent treatment of the fibrous reinforcing phase, including the following steps: S11. The fibrous reinforcing phase is heat-treated to remove surface colloidal impurities, specifically as follows: Carbon fiber powder (with a diameter of 7 μm and a length of 0.5 mm) was heat-treated at 400°C for 35 min in an air atmosphere to remove surface gelatinous impurities, thereby exposing the active groups and effectively reducing the adverse effects of these impurities on the coating performance.
[0037] In other embodiments, the heat treatment temperature may be 350°C, 360°C, 380°C, 390°C, 410°C, 420°C, 430°C, 440°C, or 450°C, and the heat treatment time may be 30 min, 32 min, 36 min, 38 min, 40 min, 43 min, 45 min, 49 min, 50 min, 52 min, 55 min, 56 min, 58 min, or 60 min.
[0038] In other embodiments, the fibrous reinforcing phase may also be glass fiber powder, basalt fiber powder, ceramic matrix whiskers, inorganic salt whiskers and mixtures thereof, wherein the ceramic matrix whiskers include SiC, Si3N4, potassium titanate, aluminum borate and mixtures thereof, and the inorganic salt whiskers include calcium sulfate, calcium carbonate and mixtures thereof.
[0039] In other embodiments, the diameter of the fibrous reinforcing phase is preferably in the range of 4μm to 12μm, specifically 4μm, 5μm, 8μm, 9μm, 10μm, or 12μm, and the length is preferably in the range of 0.1mm to 1.5mm, specifically 0.1mm, 0.3mm, 0.6mm, 0.8mm, 0.9mm, 1.0mm, 1.2mm, 1.3mm, or 1.5mm. By optimizing the length and diameter of the fibrous reinforcing phase, the uniformity of the coating can be optimized, the interfacial bonding strength between the coating and the substrate material can be enhanced, and the fatigue performance of the coating can be improved.
[0040] S12. The heat-treated fibrous reinforcing phase is mixed with an acid solution for etching, specifically: The degummed carbon fiber powder is added to an acid solution and roughened (etched) at 70°C for 25 minutes. The carbon fiber powder is then washed with water until it is neutral, i.e., the pH of the cleaning solution is 7, to obtain carbon fiber powder with surface etching.
[0041] In other embodiments, the etching temperature can be 60°C, 62°C, 65°C, 68°C, 69°C, 72°C, 75°C, 78°C, or 80°C, and the etching time can be 20 min, 22 min, 26 min, 28 min, or 30 min.
[0042] In step S12, the acid solution used is nitric acid, and the volume fraction of the acid solution is 20%. In other embodiments, the acid solution may also be sulfuric acid, and the volume fraction of the acid solution may also be 10%, 15%, 25%, or 30%.
[0043] S13. The etched fibrous reinforcing phase is mixed with a coupling agent solution and subjected to a hydrolysis reaction to obtain a modified fibrous reinforcing phase, specifically: The coupling agent was dissolved in a mixed solvent of ethanol and water to obtain a coupling agent solution with a mass fraction of 5%. Surface-etched carbon fiber powder was added, and the mixture was hydrolyzed under ultrasonic conditions for 2.5 hours. After drying at 80°C for 2 hours, grafted carbon fiber powder was obtained, which is the modified fibrous reinforcing phase.
[0044] In step S13, the coupling agent used is KH550. In other embodiments, the coupling agent may also be KH560, KH570, or a mixture thereof. In other embodiments, the mass fraction of the coupling agent solution may also be 3%, 4%, 6%, 7%, or 8%. In other embodiments, the hydrolysis reaction time may also be 2 h, 2.1 h, 2.4 h, 2.6 h, 2.8 h, or 3 h.
[0045] In this embodiment, the modified powdered reinforcing phase is prepared by surface pretreatment and acidification of the powdered reinforcing phase, including the following steps: S21. The powdered reinforcing phase undergoes surface pretreatment to remove residual organic matter and adsorbed dust impurities from the powder surface, while simultaneously forming a small amount of oxide layer on the powder surface to improve the interfacial bonding between the powder and the bearing metal. Specifically: By subjecting silicon carbide powder (with a particle size of 10 μm) to oxidation at 550 °C for 1.2 h in an air atmosphere, the adverse effects of these impurities on the coating performance can be effectively reduced.
[0046] In other embodiments, the oxidation treatment temperature can also be 500°C, 520°C, 530°C, 560°C, 580°C, 600°C, 620°C, 630°C, 660°C, 680°C, or 700°C, and the heat treatment time can be 1.0h, 1.1h, 1.3h, 1.4h, or 1.5h.
[0047] In other embodiments, the powdered reinforcing phase may also be carbon nanotubes, hexagonal boron nitride, graphene, and mixtures thereof.
[0048] In other embodiments, the particle size of the powdered reinforcing phase can also be 500 nm, 1 μm, 3 μm, 5 μm, 8 μm, 10 μm, 15 μm, 18 μm, 24 μm, 28 μm, 32 μm, 37 μm, 41 μm, 45 μm, 48 μm, or 50 μm. Optimizing the particle size of the powdered reinforcing phase is beneficial for obtaining coatings with excellent performance. However, if the particle size is too small, the powder has a large specific surface area and is prone to agglomeration, making it difficult to disperse in the coating; while if the particle size is too large, it will affect the interfacial bonding between the powder and other materials in the coating, leading to stress concentration and reduced coating uniformity.
[0049] S22. The heat-treated powdered reinforcing phase is mixed with an acid solution and subjected to an acidification reaction to obtain a modified powdered reinforcing phase, specifically: Nano-silicon carbide powder was poured into a concentrated acid solution and reacted for 1.2 hours under stirring. The reaction product was then washed with water until neutral, i.e., the pH of the washing solution was 7, to obtain surface-acidified nano-silicon carbide powder, which is the modified powdered reinforcing phase.
[0050] In step S22, the acid solution is hydrofluoric acid, and its volume fraction is 20%. In other embodiments, the acid solution may also be nitric acid or sulfuric acid, and the volume fraction of the acid solution may also be 10%, 15%, 25%, or 30%.
[0051] In this embodiment, the hydrophobic groups in the polyamide-imide resin powder containing hydrophobic groups are ether bonds and fluorinated alkyl groups, and its structural formula is as follows: , The molecular weight (Mw) of the aforementioned polyamide-imide resin powder containing hydrophobic groups is 3.6 × 10⁻⁶.5 In the above structural formula, n and m are positive integers.
[0052] In the aforementioned polyamide-imide resin powder containing hydrophobic groups, the molar ratio of "ether bonds" to "fluorinated alkyl groups" is 5:1. In other embodiments, the molar ratios of "ether bonds" to "fluorinated alkyl groups" in the polyamide-imide resin containing hydrophobic groups are 9:1, 8:1, 7:1, 6:1, 4:1, 3:1, 2:1, and 3:2. By optimizing the "ether bonds" and "fluorinated alkyl groups," the polyamide-imide resin containing hydrophobic groups exhibits more balanced overall performance, for example, demonstrating good performance in mechanical properties, tribological properties, and water absorption properties.
[0053] In this embodiment, the polyamide-imide resin powder containing hydrophobic groups is prepared by imidization reaction using trimellitic anhydride acyl chloride and diamine monomers containing hydrophobic groups as raw materials, including the following steps: S31. Mix 7 g of 4,4'-diaminodiphenyl ether (a diamine monomer containing an ether bond), 4.8 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (a trifluoromethyl diamine monomer), and 182.1 g of N-methylpyrrolidone (NMP). Stir at 200 rpm-600 rpm to disperse the monomer evenly and dissolve the solid completely to obtain solution A.
[0054] In step S31, the organic solvent A used is an aprotic polar solvent, specifically, N-methylpyrrolidone (NMP). In other embodiments, the aprotic polar solvent may also be N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), or dimethyl sulfoxide (DMSO).
[0055] In step S31 of other embodiments, the ether-containing diamine monomer used may also be at least one of m-phenylenediamine, 1,4-bis(4-aminophenoxy)benzene, and 1,3-bis(4-aminophenoxy)benzene; the trifluoromethyl diamine monomer used may also be at least one of 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether, 1,4-bis(2-trifluoromethyl4-aminophenoxy)benzene, and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.
[0056] S32. Control the temperature of the material to 0-5℃, add 10.95g trimellitic anhydride chloride to solution A in three batches, with an interval of 5-10 minutes between each addition, and stir to obtain solution B.
[0057] In step S32 of other embodiments, the molar ratio of the diamine monomer containing hydrophobic groups to trimellitic anhydride acyl chloride in solution A is 0.9:1 to 1.1:1. Specifically, the molar ratio can also be 0.9:1, 0.96:1, 1:1, 1.08:1, or 1.1:1. By optimizing the molar ratio of the diamine monomer containing hydrophobic groups to trimellitic anhydride acyl chloride to 0.9:1 to 1.1:1, especially the molar ratio of 0.96:1 to 1.08:1, the polyamide imide obtained in this range has a high molecular weight and few end group defects. However, when there is too much diamine monomer, the molecular weight will decrease and the reaction will be incomplete. On the other hand, too much acyl chloride will produce side reactions and affect the stability of the reaction.
[0058] S33. Heat to 60℃~65℃, add 5.26g of acid-binding agent (triethylamine) to solution B to react for 12h, and obtain solution C.
[0059] In step S33 of other embodiments, the molar ratio of the acid-binding agent to trimellitic anhydride acyl chloride in solution B is 1 to 1.5:1. Specifically, the molar ratio can be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, or 1.5:1. Optimizing the amount of acid-binding agent can promote the reaction of each material and make the reaction more complete. However, if the acid-binding agent is too little, the reaction is likely to be incomplete.
[0060] S34. Control the temperature of the material to 60℃~65℃, add 12.81g of imidizing reagent (a mixture of acetic anhydride and triethylamine) to solution C for reaction, and the reaction time is 12h to obtain solution D, which is a polyamide imide resin solution containing hydrophobic groups.
[0061] In step S34, a mixture of acetic anhydride and triethylamine is used, wherein the molar ratio of acetic anhydride to triethylamine is 1:1.
[0062] S35. The polyamide-imide resin solution containing hydrophobic groups is pulverized and refined to obtain polyamide-imide resin powder containing hydrophobic groups, specifically: Solution D was added to deionized water, precipitated, crushed, washed with water, filtered, dried at 120°C for 12 hours, and then dried under vacuum at 210°C for 2 hours to obtain polyamide-imide resin powder containing hydrophobic groups.
[0063] In this embodiment, the raw materials used to prepare the wear-resistant coating also include: organic solvent B, additives, and pigments and fillers.
[0064] In this embodiment, the raw materials used to prepare the wear-resistant coating are, by weight, as follows: 120 parts of polyamide-imide resin powder containing hydrophobic groups, 10 parts of lubricating phase, 20 parts of modified reinforcing phase, Organic solvent B813 parts, 25 parts of auxiliary agent, 3 parts pigment.
[0065] In this embodiment, the lubricating phase used is polytetrafluoroethylene micro powder.
[0066] In this embodiment, the organic solvent B used is N-methylpyrrolidone (NMP). In other embodiments, the organic solvent B may also be N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), or mixtures thereof.
[0067] In this embodiment, the additives used include 13 parts dispersant, 5 parts defoamer, 1 part leveling agent, and 6 parts anti-settling agent. Specifically, the dispersant is BYK110, the defoamer is Silok-4010, the leveling agent is BYK333, and the anti-settling agent is BENTONE SD-2.
[0068] In other embodiments, the dispersant may also be BYK 112, the defoamer may also be Silok-4013, the leveling agent may also be BYK358N, and the anti-settling agent may be BYK410.
[0069] In this embodiment, carbon black is used as the filler. In other embodiments, the filler may also be chrome green, iron chrome black, or mixtures thereof.
[0070] A method for preparing a wear-resistant coating for bearings according to the above embodiment includes the following steps: S41. A polyamide-imide coating is prepared from raw materials including polyamide-imide resin powder containing hydrophobic groups, a lubricating phase, and a modified reinforcing phase, specifically: (1) Add the polyamide-imide resin powder containing hydrophobic groups to organic solvent B and stir at 180 rpm to obtain a polyamide-imide resin solution.
[0071] (2) The polyamide-imide resin solution was filtered, and the lubricating phase, modified reinforcing phase, additives and pigments were added. The mixture was stirred at 700 rpm for 2.5 h to obtain the mixture.
[0072] (3) The mixture is ground, filtered, and degassed under vacuum to obtain a polyamide-imide coating. The solid content of the polyamide-imide coating is 20 wt%.
[0073] S42. The polyamide-imide coating obtained in step S41 is sprayed onto the bearing surface to form a polyamide-imide wet film on the bearing surface, specifically: Polyamide-imide coating is applied to the bearing surface using an air spraying method to form a polyamide-imide wet film on the bearing surface. By controlling the flow rate, moving speed, and spray distance of the spray gun, the dry film thickness of a single spray is maintained at 10-20 μm.
[0074] In this step, the bearings used also undergo the following pretreatment before use: removing grease and rust from the bearing surface, sandblasting the bearing surface, cleaning the surface, drying the bearing surface with compressed air, and preheating at 50℃~60℃ for 15min~20min.
[0075] S43. The polyamide-imide wet film formed on the bearing surface in step S42 is dried to form a polyamide-imide coating on the bearing surface, specifically: Place the bearing in a forced-air drying oven, set the temperature to 100℃, and keep it at that temperature for 20 minutes. After the surface coating dries, remove the bearing and measure the coating thickness.
[0076] S44. Repeat steps S42 and S43 until the thickness of the polyamide-imide coating reaches the target value. In this step, the thickness of the polyamide-imide coating is required to be 30-40 μm.
[0077] S45. The polyamide-imide coating obtained in step S44 is cured to obtain a wear-resistant coating, specifically: The coated bearings are placed in a forced-air drying oven and cured by programmed temperature increase. Specifically, the temperature is increased to 80°C at a rate of 2°C / min and cured for 20 minutes. Then, the temperature is increased to 150°C at a rate of 4°C / min and cured for 30 minutes. Finally, the temperature is increased to 270°C at a rate of 8°C / min and cured for 30 minutes. After cooling, the bearings are removed to obtain a wear-resistant coating.
[0078] In step S45, a three-stage curing process is adopted. Specifically, the temperature is raised to 70℃~90℃ at a heating rate of 1℃ / min~3℃ / min and cured for 20min~40min; the temperature is raised to 140℃~160℃ at a heating rate of 3℃ / min~5℃ / min and cured for 20min~40min; and the temperature is raised to 260℃~280℃ at a heating rate of 5℃ / min~10℃ / min and cured for 20min~40min. This three-stage curing process is more conducive to obtaining a coating with excellent performance. In particular, the slow heating in the initial stage can prevent the formation of bubbles, and the accelerated heating rate in the later stage can quickly crosslink and cure the coating.
[0079] The appearance and quality of the wear-resistant coating are inspected, any defects are repaired, and finally the coating is cleaned to obtain the finished bearing with the wear-resistant coating.
[0080] An application of the wear-resistant coating in the above embodiment in bearing manufacturing is specifically: the wear-resistant coating in the above embodiment is loaded onto the bearing surface.
[0081] Example 2 A wear-resistant coating for bearings is basically the same as in Example 1, except that in Example 2, the raw materials used to prepare the wear-resistant coating are, by weight, as follows: 110 parts of polyamide-imide resin powder containing hydrophobic groups, 20 parts of lubricating phase, 20 parts of modified reinforcing phase, Organic solvent B837 parts, 27 parts of auxiliary agents, 3 parts pigment.
[0082] In Example 2, the additives used included 15 parts dispersant, 5 parts defoamer, 1 part leveling agent, and 6 parts anti-settling agent.
[0083] Example 3 A wear-resistant coating for bearings is basically the same as in Example 1, except that: in Example 3, the raw materials used to prepare the wear-resistant coating are, by weight, the following proportions: 100 parts of polyamide-imide resin powder containing hydrophobic groups, 30 parts of lubricating phase, 20 parts of modified reinforcing phase, Organic solvent B862 parts, 30 parts of auxiliary agent, 3 parts pigment.
[0084] In Example 3, the additives used included 18 parts dispersant, 5 parts defoamer, 1 part leveling agent, and 6 parts anti-settling agent.
[0085] Example 4 A wear-resistant coating for bearings is basically the same as in Example 1, except that: in Example 4, the raw materials used to prepare the wear-resistant coating are, by weight, the following: 90 parts of polyamide-imide resin powder containing hydrophobic groups. 40 parts of lubricating phase, 20 parts of modified reinforcing phase, Organic solvent B887 parts, 32 parts of auxiliary agent, 3 parts pigment.
[0086] In Example 4, the additives used included 20 parts dispersant, 5 parts defoamer, 1 part leveling agent, and 6 parts anti-settling agent.
[0087] Example 5 A wear-resistant coating for bearings is basically the same as in Example 2, except that: in Example 5, the raw materials used to prepare the wear-resistant coating are, by weight, the following proportions: 110 parts of polyamide-imide resin powder containing hydrophobic groups, 20 parts of lubricating phase, 20 parts of modified reinforcing phase, Organic solvent B837 parts, 27 parts of auxiliary agents, 3 parts pigment.
[0088] In Example 5, the lubricating phase used was graphite.
[0089] In Example 5, the additives used included 15 parts dispersant, 5 parts defoamer, 1 part leveling agent, and 6 parts anti-settling agent.
[0090] Example 6 A wear-resistant coating for bearings is basically the same as that in Example 5, except that in Example 6, the lubricating phase used is molybdenum dioxide.
[0091] Example 7 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Example 7, the modified reinforcing phase used is 5 parts.
[0092] Example 8 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Example 8, the modified reinforcing phase used is 10 parts.
[0093] Example 9 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Example 9, the modified reinforcing phase used is 16 parts.
[0094] Example 10 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Example 10, the modified reinforcing phase used is 22 parts.
[0095] Example 11 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Example 11, the modified reinforcing phase used is 26 parts.
[0096] Example 12 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Example 12, the modified reinforcing phase used is 30 parts.
[0097] Examples 13-25 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Examples 13-25, the mass ratio of the modified fibrous reinforcing phase to the modified powdered reinforcing phase is 1:19, 1:9, 3:17, 1:4, 1:3, 3:7, 7:13, 2:3, 9:11, 11:9, 3:2, 13:7, and 7:3, respectively.
[0098] Comparative Example 1 A wear-resistant coating for bearings is basically the same as in Example 2, except that the raw materials used in Comparative Example 1 for preparing the wear-resistant coating are, by weight: 110 parts of polyamide-imide resin powder containing hydrophobic groups, 20 parts of lubricating phase, Organic solvent B, 742 parts, 24 parts of auxiliary agent, 3 parts pigment.
[0099] In Comparative Example 1, the additives used included 12 parts dispersant, 5 parts defoamer, 1 part leveling agent, and 6 parts anti-settling agent.
[0100] Comparative Example 2 A wear-resistant coating for bearings is basically the same as that in Example 2, except that the modified reinforcing phase used in Comparative Example 2 is a modified fibrous reinforcing phase.
[0101] Comparative Example 3 A wear-resistant coating for bearings is basically the same as that in Example 2, except that in Comparative Example 3, the modified reinforcing phase used is a modified powdered reinforcing phase.
[0102] Table 1. Performance differences of wear-resistant coatings in various embodiments and comparative examples.
[0103] As shown in Table 1, by optimizing the amounts of polyamide-imide resin powder, lubricating phase, and modified reinforcing phase, a balance can be achieved between the mechanical properties, tribological properties, hydrophobic properties, and service life of the coating. However, when the proportion of polyamide-imide resin powder is too high, the water absorption rate of the coating is low, but the coefficient of friction and wear need to be optimized; when the proportion of polyamide-imide resin powder is reduced, the coefficient of friction of the coating decreases, but the wear and water absorption rate increase; when the proportion of lubricating phase is too high, the coefficient of friction of the coating is very low, but the wear increases, and vice versa when the proportion of lubricating phase is reduced; when the proportion of modified reinforcing phase is too high, the mechanical properties of the coating are improved and the wear decreases, but the coefficient of friction increases, and vice versa when the proportion of modified reinforcing phase is reduced, the coefficient of friction of the coating decreases, but the wear increases.
[0104] As shown in Table 1, in this invention, by optimizing the mass ratio of modified fibrous reinforcing phase to modified powdered reinforcing phase, the mechanical properties and fatigue resistance of the coating can be balanced. However, when there is too much modified fibrous reinforcing phase, the wear resistance of the coating decreases. At the same time, too much modified fibrous reinforcing phase is not conducive to dispersion and is prone to agglomeration in the coating, which reduces the performance of the coating. When there is too much modified powdered reinforcing phase, the hardness of the coating will be too high, the overall friction coefficient of the coating will increase, and cracks will easily be generated under impact or vibration, leading to large-scale peeling.
[0105] As shown in Table 1, in Comparative Example 1, without the addition of modified reinforcing phase, the coating strength is not high. During bearing operation, the resin powder and lubricating phase form a lubricating film on the bearing surface, resulting in a low coefficient of friction. However, due to the low strength, the wear is relatively large. In Comparative Example 2, all the modified reinforcing phases are modified fibrous reinforcing phases. Due to the excessive content of modified fibrous reinforcing phases, they are prone to agglomeration in the coating, making it difficult to disperse evenly. Therefore, the coefficient of friction of the coating is relatively high. At the same time, during bearing operation, the undispersed modified fibrous reinforcing phases are prone to stress concentration, leading to large-scale peeling of the coating, increasing wear, and reducing mechanical properties. In Comparative Example 3, all the modified reinforcing phases are modified powdered reinforcing phases. The mechanical properties of the coating are very good, but the coating is too hard, which increases the coefficient of friction when rubbing against metal. At the same time, a large number of hard particles increase the brittleness of the coating, making it prone to local cracking, leading to large-scale peeling of the coating and increased wear.
[0106] As can be seen from the above results, compared with conventional polyamide-imide resin wear-resistant materials, the wear-resistant coating of the present invention has a lower water absorption rate, better self-lubrication, and higher load-bearing capacity. It can be widely used in the manufacture of bearings, not only meeting the requirements of high humidity environments, but also significantly reducing the occurrence of mechanical failures, thus extending the service life of bearings.
[0107] The above embodiments are merely preferred embodiments of the present invention, and the scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A wear-resistant coating for bearings, characterized in that, The raw materials for preparing the wear-resistant coating include at least polyamide-imide resin powder containing hydrophobic groups, a lubricating phase, and a modified reinforcing phase; the modified reinforcing phase includes a modified fibrous reinforcing phase and a modified powder reinforcing phase; The modified fibrous reinforcing phase is prepared by desizing, etching and coupling agent treatment of the fibrous reinforcing phase; The modified powdered reinforcing phase is prepared by surface pretreatment and acidification of the powdered reinforcing phase.
2. The wear-resistant coating for bearings according to claim 1, characterized in that, The mass ratio of the modified fibrous reinforcing phase to the modified powdered reinforcing phase is 1-2:1-10.
3. The wear-resistant coating for bearings according to claim 2, characterized in that, The modified fibrous reinforcing phase is prepared by desizing, etching, and coupling agent treatment of the fibrous reinforcing phase, including the following steps: S11. Heat-treat the fibrous reinforcing phase to remove surface colloidal impurities; S12. The heat-treated fibrous reinforcing phase is mixed with an acid solution and etched. S13. The etched fibrous reinforcing phase is mixed with a coupling agent solution and subjected to a hydrolysis reaction to obtain a modified fibrous reinforcing phase. The modified powdered reinforcing phase is prepared by surface pretreatment and acidification of the powdered reinforcing phase, including the following steps: S21. Pre-treat the powdered reinforcing phase to remove surface impurities; S22. The pretreated powdered reinforcing phase is mixed with an acid solution and subjected to an acidification reaction to obtain a modified powdered reinforcing phase.
4. The wear-resistant coating for bearings according to claim 3, characterized in that, The preparation method of the modified fibrous reinforcement shall satisfy at least one of the following preparation conditions (1.11) to (1.23): (1.11) In step S11, the diameter of the fibrous reinforcing phase is 4μm to 12μm and the length is 0.1mm to 1.5mm; the fibrous reinforcing phase includes at least one of glass fiber powder, carbon fiber powder, basalt fiber powder, ceramic matrix whiskers, and inorganic salt whiskers; the ceramic matrix whiskers include at least one of SiC, Si3N4, potassium titanate, and aluminum borate; the inorganic salt whiskers include at least one of calcium sulfate and calcium carbonate. (1.12) In step S11, the heat treatment is carried out in an air atmosphere; (1.13) In step S11, the heat treatment is carried out at a temperature of 350℃~450℃; (1.14) In step S11, the heat treatment time is 30 min to 60 min; (1.15) In step S12, the acid solution is at least one of nitric acid and sulfuric acid; (1.16) In step S12, the volume fraction of the acid solution is 10% to 30%; (1.17) In step S12, the etching is performed at a temperature of 60°C to 80°C; (1.18) In step S12, the etching time is 20 min to 30 min; after the etching is completed, the following treatment is also included: the etching product is washed with water until the pH value of the washing solution is neutral; (1.19) In step S13, the coupling agent solution is prepared by dissolving the coupling agent in a mixed solvent of ethanol and water; the coupling agent is at least one of KH550, KH560, and KH570; the mass ratio of ethanol to water in the mixed solvent of ethanol and water is 8 to 13:
1. (1.20) In step S13, the mass fraction of the coupling agent solution is 3% to 8%; (1.21) In step S13, the hydrolysis reaction takes 2 to 3 hours; (1.22) In step S13, the hydrolysis reaction is carried out under ultrasonic conditions; (1.23) In step S13, after the hydrolysis reaction is completed, the reaction product is dried. The drying process is carried out at a temperature of 70℃ to 90℃; the drying time is 2h to 3h. The preparation method of the modified powdered reinforcing phase shall satisfy at least one of the following preparation conditions (2.11) to (2.18): (2.11) In step S21, the particle size of the powdered reinforcing phase is 500 nm to 50 μm; the powdered reinforcing phase includes at least one of carbon nanotubes, hexagonal boron nitride, graphene, and silicon carbide powder; (2.12) In step S21, the surface pretreatment is carried out in an air atmosphere; (2.13) In step S21, the surface pretreatment is carried out at a temperature of 500℃~700℃; (2.14) In step S21, the surface pretreatment time is 1h to 1.5h; (2.15) In step S22, the acid solution is at least one of hydrofluoric acid, nitric acid, and sulfuric acid; (2.16) In step S22, the volume fraction of the acid solution is 10% to 30%; (2.17) In step S22, the acidification reaction takes 1 to 2 hours; (2.18) In step S12, the acidification reaction is completed and the following treatment is also included: washing the product after the acidification reaction with water until the pH value of the washing solution is neutral.
5. The wear-resistant coating for bearings according to claim 1, characterized in that, The hydrophobic group in the polyamide-imide resin powder is at least one of ether linkage and fluorinated alkyl group; the polyamide-imide resin powder containing hydrophobic groups is prepared by imidization reaction using trimellitic anhydride acyl chloride and diamine monomer containing hydrophobic groups as raw materials; the preparation method of the polyamide-imide resin powder containing hydrophobic groups includes the following steps: S31. A diamine monomer containing a hydrophobic group is mixed with an organic solvent A and stirred to obtain solution A; wherein the organic solvent A is an aprotic polar solvent. S32. Add trimellitic anhydride chloride to solution A in batches and stir to obtain solution B; S33. Add the acid-binding agent to solution B to react and obtain solution C; S34. The imidizing reagent is added to solution C to react and obtain solution D; S35. Add solution D to deionized water, precipitate, crush, wash with water, filter, and dry to obtain polyamide-imide resin powder containing hydrophobic groups.
6. The wear-resistant coating for bearings according to claim 5, characterized in that, The preparation method of the polyamide-imide resin powder containing hydrophobic groups shall satisfy at least one of the following preparation conditions (3.11) to (3.18): (3.11) In step S31, the diamine monomer containing a hydrophobic group is an ether-bonded diamine monomer and / or a trifluoromethyl diamine monomer; the ether-bonded diamine monomer includes at least one of m-phenylenediamine, 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, and 1,3-bis(4-aminophenoxy)benzene; the trifluoromethyl diamine monomer includes at least one of 2,2′-bis(trifluoromethyl)-4,4-diaminobiphenyl, 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether, 1,4-bis(2-trifluoromethyl4-aminophenoxy)benzene, and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane; (3.12) In step S31, the aprotic polar solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; (3.13) In step S32, the molar ratio of the diamine monomer containing a hydrophobic group to the trimellitic anhydride acyl chloride in solution A is 0.9:1 to 1.1:1; the temperature of solution A is 0 to 5°C; (3.14) In step S33, the molar ratio of the acid-binding agent to the trimellitic anhydride acyl chloride in solution B is 1 to 1.5:1; the acid-binding agent is triethylamine; (3.15) In step S33, the reaction is carried out at a temperature of 60℃~65℃; the reaction time is 12h~24h; (3.16) In step S34, the imidizing agent is a mixture of acetic anhydride and triethylamine; the molar ratio of acetic anhydride to triethylamine is 0.5 to 2:1; (3.17) In step S34, the reaction is carried out at a temperature of 60℃~65℃; the reaction time is 12h~24h; (3.18) In step S35, the drying is carried out under vacuum conditions; the drying temperature is 100℃~150℃; and the drying time is 10h~24h.
7. The wear-resistant coating for bearings according to any one of claims 1 to 6, characterized in that, The raw materials for preparing the wear-resistant coating also include: organic solvent B, additives, and pigments and fillers; the raw materials for preparing the wear-resistant coating are, by weight, as follows: 90 to 200 parts of polyamide-imide resin powder containing hydrophobic groups. Lubricating phase: 5 to 50 parts 5 to 30 parts of modified reinforcing phase, Organic solvent B: 400-1500 parts 12 to 35 parts of auxiliary agent 1 to 4 parts pigment; The lubricating phase includes at least one of polytetrafluoroethylene micro powder, graphite, molybdenum disulfide, and tungsten disulfide; The organic solvent B is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; The additives include at least one of dispersants, defoamers, leveling agents, and antisettling agents; The filler includes at least one of chrome green, iron chrome black, and carbon black.
8. A method for preparing a wear-resistant coating for bearings as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S41. A polyamide-imide coating is prepared from raw materials including polyamide-imide resin powder containing hydrophobic groups, a lubricating phase, and a modified reinforcing phase. S42. Spray the polyamide-imide coating obtained in step S41 onto the bearing surface to form a polyamide-imide wet film on the bearing surface. S43. Dry the polyamide-imide wet film formed on the bearing surface in step S42 to form a polyamide-imide coating on the bearing surface; S44. Repeat steps S42 and S43 until the thickness of the polyamide-imide coating reaches the set target. S45. The polyamide-imide coating obtained in step S44 is cured to obtain a wear-resistant coating.
9. The preparation method according to claim 8, characterized in that, In step S41, the solid content of the polyamide-imide coating is 5wt% to 30wt%; when the raw materials are polyamide-imide resin powder containing hydrophobic groups, lubricating phase and modified reinforcing phase, organic solvent B, additives and pigments, the preparation method of the polyamide-imide coating includes the following steps: (1) Add the polyamide-imide resin powder containing hydrophobic groups to organic solvent B and stir at 150 rpm to 200 rpm to obtain a polyamide-imide resin solution. (2) Filter the polyamide-imide resin solution, add the lubricating phase, the modified reinforcing phase, the additives and the pigment, and stir at 600 rpm to 800 rpm for 2 to 3 hours to obtain the mixture. (3) Grind, filter, and degas the mixture to obtain a polyamide-imide coating; In step S42, the polyamide-imide coating prepared in step S41 is sprayed onto the bearing surface using an air spraying method or an electrostatic spraying method. Before use, the bearing also includes the following pretreatment: removing grease and rust from the bearing surface, sandblasting the bearing surface, cleaning the surface, drying the bearing surface with compressed air, and preheating at 50℃~60℃ for 15min~20min. In step S43, the drying temperature is 80℃~120℃; the drying time is 20min~30min; and the thickness of the polyamide-imide coating formed on the bearing surface in a single step is 10μm~50μm. In step S44, the target thickness of the polyamide-imide coating is 30 μm to 50 μm; In step S45, the curing process includes: heating to 70℃~90℃ at a heating rate of 1℃ / min~3℃ / min and curing for 20min~40min; heating to 140℃~160℃ at a heating rate of 3℃ / min~5℃ / min and curing for 20min~40min; and heating to 260℃~280℃ at a heating rate of 5℃ / min~10℃ / min and curing for 20min~40min.
10. The application of a wear-resistant coating in bearing manufacturing, characterized in that, The bearing surface is loaded with a wear-resistant coating as described in any one of claims 1 to 7; or the wear-resistant coating on the bearing surface is prepared by the preparation method described in claim 8 or 9.