A vertical graphene-based silicon-carbon composite material, a preparation method thereof and a lithium ion battery
By employing a composite structure of nano-silicon core, metal nanoclusters, vertical graphene, and carbon coating in lithium-ion batteries, the volume expansion problem of silicon-based materials during charge and discharge processes is solved, improving the initial charge and discharge efficiency and cycle stability of the battery, and constructing a highly efficient conductive network.
Patent Information
- Application Number
- CN202610188028.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-10
- Publication Date
- 2026-05-26
AI Technical Summary
Traditional lithium-ion battery anode material graphite has low specific capacity, while silicon-based materials suffer from severe volume expansion during charging and discharging, leading to connection failure and SEI film thickening, which affects battery performance.
A silicon-carbon composite material based on vertical graphene is used. The structure consists of a nano-silicon core, metal nanoclusters, vertical graphene, and a carbon-coated outer layer from the inside out. A stable carbon layer and metal nanoclusters are formed by PECVD deposition to construct a three-dimensional conductive network, which alleviates volume expansion and enhances conductivity.
It significantly improves the initial charge-discharge efficiency of lithium-ion batteries, reduces the formation of SEI film, enhances electron conduction efficiency and material cycle stability, and improves the overall performance of the battery.
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, and in particular to a silicon-carbon composite material based on vertical graphene, its preparation method, and a lithium-ion battery. Background Technology
[0002] With the rapid development of new energy technologies, lithium-ion batteries have been widely used in portable electronic devices, electric bicycles, and electric vehicles due to their advantages such as high capacity and long cycle life. However, the traditional commercial lithium-ion battery anode materials mainly use graphite-based carbon materials, with a theoretical specific capacity of only 372 mAh / g, which can no longer meet the ever-increasing demand for high energy density.
[0003] To improve the energy density of lithium-ion batteries, researchers have begun to focus on the potential of silicon-based materials as anode materials, as silicon has a theoretical specific capacity of up to 4200 mAh / g, more than ten times that of graphite. However, silicon-based materials suffer from severe volume expansion (300%–400%) during charge and discharge, leading to numerous technical challenges. First, volume expansion causes silicon-based materials to pulverize and detach, affecting the connection between the active material and the current collector and reducing electron transport efficiency. Second, volume changes lead to a gradual thickening of the solid electrolyte interphase (SEI) film, which is detrimental to improving lithium battery capacity and causes a sharp decline in the cycle performance of lithium batteries. In addition, the low conductivity of silicon-based materials makes the volume expansion effect more pronounced during charge and discharge, further exacerbating the pulverization of the material and the rupture of the SEI film. To address these problems, researchers have tried various modification methods, such as carbon coating, nanostructuring, and constructing special structures. However, these methods still have some limitations, such as the rigid connection between the carbon layer and the silicon-based material, and the poor uniformity of the dispersion of nano-silicon. Therefore, developing a novel silicon-based material that can effectively alleviate the volume expansion of silicon-based materials, improve conductivity, and enhance cycle stability is of great significance for promoting the development of lithium-ion battery technology.
[0004] Patent document CN109616630A discloses a silicon-carbon composite material with a uniform carbon film and vertically oriented graphene double coating, its preparation method, and its application in lithium-ion batteries. The method employs thermochemical vapor deposition to form a carbon coating layer on the surface of silicon particles, followed by the re-growth of vertically oriented graphene nanosheets. In this silicon-carbon composite structure, the vertical graphene grows on the outer surface of the carbon coating layer, and its connection to the silicon core is indirect. This makes the connection prone to loosening or failure when the silicon undergoes drastic volume changes during charging and discharging. Consequently, the flexible vertical graphene is not effective in mitigating volume expansion during overcharging and over-discharging. Furthermore, the vertical graphene is located on the outside, and its exposed edges can violently catalyze electrolyte decomposition during the first charge and discharge cycle, forming a thick and unstable SEI that consumes a large amount of lithium. Summary of the Invention
[0005] The present invention aims to solve the above-mentioned problems by providing a silicon-carbon composite material based on vertical graphene, a method for its preparation, and a lithium-ion battery that can effectively alleviate the volume expansion of silicon-based materials and improve their electrical properties.
[0006] The technical solution to the problem of the present invention is, in a first aspect, to provide a silicon-carbon composite material based on vertical graphene, wherein the silicon-carbon composite material comprises, in sequence from the inside to the outside, a nano-silicon core, a metal nanocluster, vertical graphene, and a carbon-coated outer layer; wherein the metal is selected from at least one of Pt and Pd.
[0007] In this invention, a carbon-coated outer layer covering the entire surface isolates the nano-silicon core from the electrolyte. Next, vertical graphene is introduced between the carbon-coated outer layer and the nano-silicon core, enhancing not only the material's conductivity and mechanical properties but also ensuring the connection between the silicon particles and the carbon layer remains intact during expansion and contraction. Finally, metal nanoclusters are introduced to achieve directional interface reconstruction, acting as a "bridge" to establish a strong chemical / electrical connection between silicon and the vertical graphene. This structural design not only alleviates the volume expansion problem of silicon-based materials during charging and discharging but also provides a buffer space for silicon particle expansion, effectively preventing repeated SEI film formation due to overall particle deformation and significantly improving the first charge / discharge efficiency (first-time efficiency). Simultaneously, a three-dimensional, multi-level, continuous conductive network is constructed, significantly enhancing electron conduction efficiency.
[0008] The metal is selected from at least one of Pt and Pd. Other metals, such as Fe, Ni, Cu, Co, Pt, Pd, and Ru, will form compounds with silicon and affect the electrical properties of the composite material, and are therefore unsuitable for use.
[0009] Preferably, the height of the vertical graphene is 3 to 5 times the diameter of the nano-silicon. An appropriate height ensures that the vertical graphene has sufficient "buffer space" to accommodate the volume expansion of silicon particles during charging and discharging (up to 300%); avoids excessive graphene growth leading to particle agglomeration or structural collapse; and achieves a synergistic effect of spatial confinement and elastic buffering mechanisms.
[0010] The diameter of the silicon nanoparticles should not be too large, and needs to be less than 150 nm; if the diameter of the silicon nanoparticles is too large, the silicon particles are prone to breakage during cycling. For example, the diameter of the silicon nanoparticles is 100–150 nm. Correspondingly, the height of the vertical graphene is 300–750 nm.
[0011] In some implementation methods As a preferred embodiment of the present invention, a PECVD-deposited carbon layer is further provided between the vertical graphene and the carbon-coated outer layer.
[0012] PECVD-deposited carbon layers can passivate active sites perpendicular to the graphene edge, forming the most stable initial SEI, laying the foundation for long-term cycling, and enhancing the interfacial stability between graphene and silicon. On this basis, the carbon-coated outer layer provides a thick and continuous secondary protection and conductive network, constructing a three-dimensional continuous conductive network. This achieves a dual-functional carbon layer structure of "inner carbon anchoring + outer carbon protection", which combines electrochemical stability and mechanical toughness.
[0013] As a preferred embodiment of the present invention, the thickness of the PECVD deposited carbon layer is 2 to 5 nm.
[0014] Secondly, another objective of this invention is to provide a method for preparing the silicon-carbon composite material based on vertical graphene, comprising the following steps:
[0015] S1. In a PECVD furnace, after cleaning and preheating the nano-silicon, the precursor vapor of the metal is introduced through an inert carrier gas of 20-50 sccm, while hydrogen is introduced at the same time. After deposition for 10-30 min, nano-silicon cores MNCs / Si with metal nanoclusters on the surface are obtained.
[0016] The total gas flow rate is 50–100 sccm; the volume concentration of hydrogen in the total gas flow is 1 vol%–10 vol%.
[0017] When the metal is Pt, the deposition temperature is 350℃~600℃; when the metal is Pd, the deposition temperature is 300℃~500℃.
[0018] S2. After preheating and cleaning the surface, the first carbon source and hydrogen are introduced, and vertical graphene is grown at 700℃~800℃ to obtain vertical graphene and nano-silicon cores VG / MNCs / Si connected by metal nanoclusters.
[0019] S3. The VG / MNCs / Si is mixed with a solution of a second carbon source, spray-dried, and sintered to obtain the silicon-carbon composite material C / VG / MNCs / Si.
[0020] In some implementation methods As a preferred embodiment of the present invention, in step S3, 2-5 nm of carbon is first deposited on the surface of the VG / MNCs / Si to obtain the PECVD deposited carbon layer; then it is mixed with the solution of the second carbon source, spray-dried, and sintered.
[0021] Preferably, the method for depositing 2-5 nm of carbon is as follows: in a PECVD furnace, when the temperature of VG / MNCs / Si is reduced to 200℃-400℃, a third carbon source is introduced, and 2-5 nm of carbon is deposited on the graphene surface using a PECVD low-pressure plasma environment.
[0022] The third carbon source can be a commonly used carbon source, for example, at least one of methane, acetylene, and ethylene. Preferably, the third carbon source is at least one of methane and acetylene.
[0023] The amount of the third carbon source is related to its carbonization yield. When methane is selected as the third carbon source, the flow rate is 5 to 15 sccm. For example, it can be 5 sccm, 6 sccm, 7 sccm, 8 sccm, 9 sccm, 10 sccm, 11 sccm, 12 sccm, 13 sccm, 14 sccm, or 15 sccm.
[0024] When acetylene is selected as the third carbon source, the flow rate is 3 to 10 sccm. For example, it can be 3 sccm, 4 sccm, 5 sccm, 6 sccm, 7 sccm, 8 sccm, 9 sccm, or 10 sccm.
[0025] Based on this, the deposition rate can be controlled between 0.02 and 0.08 nm / s, and the thickness of the carbon layer deposited by PECVD can be controlled by controlling the deposition time.
[0026] In step S1 After cleaning and preheating the nano-silicon, metal nanoclusters were obtained on the surface of the nano-silicon core using CVD.
[0027] The method of cleaning nano-silicon is not limited. As a preferred embodiment of the present invention, after placing the nano-silicon in the PECVD furnace, an inert gas is introduced to purge the air. The inert gas is not limited; for example, it can be argon.
[0028] The method of preheating and activating nano-silicon is not limited. Preferably, a protective gas is introduced, followed by heating to 150°C–250°C. Preferably, the protective gas is at least one of argon and nitrogen. Preferably, the protective gas is a mixture of argon and nitrogen. Preferably, the flow rate of argon is 5–15 sccm, for example, 5 sccm, 6 sccm, 7 sccm, 8 sccm, 9 sccm, 10 sccm, 11 sccm, 12 sccm, 13 sccm, 14 sccm, or 15 sccm; while the flow rate of nitrogen is 2.5–7.5 sccm, for example, 2.5 sccm, 3 sccm, 3.5 sccm, 4 sccm, 4.5 sccm, 5 sccm, 5.5 sccm, 6 sccm, 6.5 sccm, 7 sccm, or 7.5 sccm. The temperature is raised to 150℃~250℃, for example, 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃, 250℃.
[0029] The precursor of the metal is used to have sufficient volatility and to completely vaporize before the inert carrier gas. For example, when the metal is Pt, the precursor is selected from trimethyl(methylcyclopentadienyl)platinum (MeCpPtMe3); when the metal is Pd, the precursor is selected from at least one of palladium diethyldithiocarbamate (Pd(dmit)2) and bis(acetylacetone)palladium(II) (Pd(acac)2).
[0030] To control the acquisition of metal nanoclusters, the concentration of metal precursor vapor, hydrogen concentration, deposition temperature, and time should be limited.
[0031] The precursor vapor of the metal is introduced into the PECVD reaction tube by an inert carrier gas. The flow rate of the inert carrier gas is 20–50 sccm, for example, 20 sccm, 25 sccm, 30 sccm, 35 sccm, 40 sccm, 45 sccm, or 50 sccm. This flow rate controls the concentration of the metal precursor vapor entering the reaction tube. Too low a concentration can lead to insufficient coverage, while too high a concentration can result in the formation of large particles or continuous films. The inert carrier gas is not limited; for example, it can be at least one of argon or nitrogen.
[0032] Hydrogen gas is simultaneously introduced to promote the reduction of the metal precursor to its metallic state. Hydrogen can also be introduced via an inert carrier gas.
[0033] The final control of the total airflow is 50 to 100 sccm, for example, it can be 50 sccm, 60 sccm, 70 sccm, 80 sccm, 90 sccm, or 100 sccm.
[0034] The volume concentration of hydrogen in the total gas flow is 1 vol% to 10 vol%, for example, it can be 1 vol%, 2 vol%, 3 vol%, 4 vol%, 5 vol%, 6 vol%, 7 vol%, 8 vol%, 9 vol%, 10 vol%, preferably 5 to 10 vol%. If the hydrogen concentration is too low, it is insufficient for reduction, and if the concentration is too high, it can easily lead to silicon reduction and / or metal diffusion.
[0035] When the metal is Pt, the deposition temperature is 350°C to 600°C; for example, it can be 350°C, 400°C, 450°C, 500°C, 550°C, or 600°C; preferably 400°C to 550°C.
[0036] When the metal is Pd, the deposition temperature is 300℃~500℃; for example, it can be 300℃, 350℃, 400℃, 450℃, or 500℃; preferably 350~450℃.
[0037] Too low a deposition temperature can lead to incomplete decomposition of the precursor and a low deposition rate; too high a deposition temperature can lead to agglomeration of nanodots, increased diffusion, and increased size.
[0038] The deposition time is 10 to 30 min, for example, 10 min, 13 min, 15 min, 17 min, 20 min, 22 min, 25 min, 27 min, or 30 min, preferably 10 to 20 min; by controlling the density and size of nanodots with appropriate time, agglomeration is avoided.
[0039] As a preferred embodiment of the present invention, in step S1, a synchronous pulse is introduced into the precursor vapor of the metal and hydrogen gas. Compared to continuous gas flow, pulsed gas flow is beneficial for obtaining more uniform nanoclusters.
[0040] Preferably, the pulse duration is 0.1 to 1 s; for example, the pulse duration can be 0.1 s, 0.2 s, 0.3 s, 0.4 s, 0.5 s, 0.6 s, 0.7 s, 0.8 s, 0.9 s, or 1 s; preferably 0.4 to 0.6 s; and more preferably 0.5 s.
[0041] Preferably, the frequency is 0.1 to 10 Hz; for example, the frequency can be 0.1 Hz, 0.2 Hz, 0.3 Hz, 0.4 Hz, 0.5 Hz, 0.6 Hz, 0.7 Hz, 0.8 Hz, 0.9 Hz, 1 Hz, 2 Hz, 3 Hz, 4 Hz, 5 Hz, 6 Hz, 7 Hz, 8 Hz, 9 Hz, or 10 Hz; preferably 0.1 to 2 Hz, and more preferably 0.1 to 1 Hz.
[0042] For example, a pulse of 0.5 s and a frequency of 1 Hz means that a complete cycle is 1 (1 / 1 Hz) s, in which the pulse introduces the metal precursor and hydrogen for 0.5 s, and after the pulse is turned off, it is left to stand or purge with an inert carrier gas (such as argon) for 0.5 s.
[0043] In step S2 Vertical graphene is generated on the MNCs / Si obtained in step S1 by directional induction of metal nanoclusters.
[0044] The method of preheating and cleaning MNCs / Si is not limited. Preferably, an inert carrier gas is introduced, and the temperature is raised to 700°C–800°C; hydrogen is then introduced at 700°C–800°C for 5–15 minutes. For example, the temperature can be raised to 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, or 800°C. The hydrogen introduction time can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, or 15 minutes. This step also facilitates controlled, slight remodeling of the clusters, resulting in a more stable crystal shape.
[0045] Preferably, the heating rate is 3 to 8 °C / min; for example, it can be 3 °C / min, 4 °C / min, 5 °C / min, 6 °C / min, 7 °C / min, or 8 °C / min.
[0046] Preferably, the flow rate of hydrogen is 150 to 250 sccm; for example, it can be 150 sccm, 160 sccm, 170 sccm, 180 sccm, 190 sccm, 200 sccm, 210 sccm, 220 sccm, 230 sccm, 240 sccm, or 250 sccm.
[0047] After preheating and cleaning, a first carbon source and hydrogen are introduced to grow vertical graphene. The first carbon source can be any commonly used carbon source for growing vertical graphene; for example, it can be at least one of methane, acetylene, and ethylene. Preferably, acetylene is used as the first carbon source in this invention.
[0048] The amount and ratio of the first carbon source and hydrogen are preferably controlled, and the flow rate of the first carbon source should not be too high to avoid the formation of multilayer, non-vertical, or carbon nanotube structures. Preferably, the flow rate of the first carbon source is 15–25 sccm, and the flow rate of the hydrogen is 150–250 sccm. For example, the flow rate of the first carbon source can be 15 sccm, 16 sccm, 17 sccm, 18 sccm, 19 sccm, 20 sccm, 21 sccm, 22 sccm, 23 sccm, 24 sccm, or 25 sccm; and the flow rate of the hydrogen can be 150 sccm, 160 sccm, 170 sccm, 180 sccm, 190 sccm, 200 sccm, 210 sccm, 220 sccm, 230 sccm, 240 sccm, or 250 sccm.
[0049] Preferably, the volume ratio of the first carbon source to hydrogen is 1:(10-15). For example, it can be 1:10, 1:11, 1:12, 1:13, 1:14, or 1:15; this can suppress non-vertical growth and improve the quality of graphene.
[0050] Under the above conditions, the growth rate of the vertical graphene is controlled at 10–25 nm / min. Excessive growth rate can easily lead to defects.
[0051] The growth time is related to the growth rate and affects the height of the vertical graphene. Based on the above, as a preferred embodiment of the present invention, the growth time is 15 to 30 minutes, and the height of the vertical graphene is controlled to be 3 to 5 times the diameter of the nano-silicon.
[0052] As a preferred embodiment of the present invention, after growth is completed, the carbon source is turned off, and hydrogen is continuously introduced for 5 to 15 minutes to remove residual carbon. For example, the time intervals can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, or 15 minutes.
[0053] As a preferred embodiment of the present invention, after growth is completed, argon gas is introduced for cooling. The argon gas flow rate is 100–200 sccm, and the cooling rate is 1–5 °C / min. Slow cooling allows the entire heterostructure time to relax and shrink uniformly, avoiding the generation of large shear and tensile stresses in silicon, metal nanoclusters, and vertical graphene due to uneven shrinkage. Using an appropriate flow rate of argon gas keeps the VG surface clean without affecting the cooling rate. For example, the argon gas flow rate can be 100 sccm, 110 sccm, 120 sccm, 130 sccm, 140 sccm, 150 sccm, 160 sccm, 170 sccm, 180 sccm, 190 sccm, or 200 sccm; the cooling rate can be 1 °C / min, 2 °C / min, 3 °C / min, 4 °C / min, or 5 °C / min.
[0054] In step S3 A carbon-coated outer layer is coated onto the VG / MNCs / Si obtained in step S2, or onto the VG / MNCs / Si with a PECVD-deposited carbon layer.
[0055] The second carbon source is not limited, but is preferably a carbon source that can be carbonized at the selected sintering temperature. Preferably, the carbonization temperature of the second carbon source is 500℃ to 600℃. Choosing a low-temperature carbon source avoids damage to the already formed vertical graphene structure caused by high-temperature carbonization; ensures a uniform, dense, and crack-free carbon layer; improves granulation efficiency and particle sphericity, facilitating electrode slurry coating and compaction. Preferably, the second carbon source is selected from at least one of glucose, sucrose, polyvinyl alcohol, citric acid, and chitosan.
[0056] The amount of VG / MNCs / Si or VG / MNCs / Si with a PECVD-deposited carbon layer (hereinafter collectively referred to as "particles") and the second carbon source is preferably limited. Preferably, the mass ratio of particles to the second carbon source is 1:2 to 2:1, specifically set based on the carbonization yield of the second carbon source. The carbonization yields of glucose, sucrose, polyvinyl alcohol, citric acid, and chitosan are 40%, 40%, 50%, 30%, and 50%, respectively.
[0057] As a preferred embodiment of the present invention, the solid content of the slurry mixture of particles and the solution of the second carbon source is 20% to 40%; for example, it can be 20%, 25%, 30%, 35%, or 40%. This ensures that the particles dry quickly after spraying and do not clog the nozzle.
[0058] During spray drying, the feed rate is preferably 250–350 mL / h; for example, it can be 250 mL / h, 260 mL / h, 270 mL / h, 280 mL / h, 290 mL / h, 300 mL / h, 310 mL / h, 320 mL / h, 330 mL / h, 340 mL / h, or 350 mL / h.
[0059] Preferably, the spray gas pressure is 1.5 to 3 bar; for example, it can be 1.5 bar, 2 bar, 2.5 bar, or 3 bar.
[0060] Preferably, the nozzle diameter is 80–150 μm; for example, it can be 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, or 150 μm.
[0061] Preferably, the drying temperature is 140°C to 180°C; for example, it can be 140°C, 150°C, 160°C, 170°C, or 180°C.
[0062] After spray drying, sintering is performed. Preferably, the sintering process involves heating to 500℃~600℃ under inert gas protection and holding at that temperature for 0.5~2 h. For example, the temperature can be 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, or 600℃; and the time can be 0.5 h, 1 h, 1.5 h, or 2 h.
[0063] Preferably, the inert gas is argon.
[0064] Preferably, the heating rate is 2 to 5 °C / min, for example, it can be 2 °C / min, 3 °C / min, 4 °C / min, or 5 °C / min.
[0065] Thirdly, another objective of the present invention is to provide a lithium-ion battery, comprising a positive electrode, a negative electrode, an electrolyte, and a separator; wherein the negative electrode comprises the aforementioned silicon-carbon composite material based on vertical graphene.
[0066] There are no restrictions on the positive electrode, separator, electrolyte, etc.
[0067] The beneficial effects of this invention are:
[0068] 1. This invention provides a silicon-carbon composite material with a C / VG / MNCs / Si structure, wherein: First, the outermost complete carbon layer coating structure effectively isolates the direct contact between silicon and the electrolyte, reducing the continuous reaction between the fresh silicon surface and the electrolyte to form an unstable SEI film, significantly improving the initial charge-discharge efficiency (first-time efficiency); simultaneously, the carbon coating layer can effectively reduce irreversible lithium loss and suppress excessive SEI formation during the initial charge-discharge process, thereby improving the overall performance of the lithium-ion battery. Second, the introduction of vertical graphene between the carbon coating layer and silicon enhances the conductivity and mechanical properties of the material, ensuring that the connection between the silicon particles and the carbon layer remains unbroken during expansion and contraction. Third, metal nanoclusters act as a "bridge" to achieve a strong chemical / electrical connection between silicon and vertical graphene.
[0069] This structural design not only alleviates the volume expansion problem of silicon-based materials during charging and discharging, but also provides a buffer space for the expansion of silicon particles, effectively preventing the deformation of the overall particles from causing repeated formation of SEI film, and significantly improving the first charge and discharge efficiency (first efficiency); at the same time, it constructs a three-dimensional multi-level continuous conductive network, which significantly improves the electron conduction efficiency.
[0070] In some implementations, a PECVD-deposited carbon layer is also present between the vertical graphene and the carbon-coated outer layer. The dual-carbon-layer structure achieves interface stability and SEI film suppression. The multi-scale carbon protection structure is synergistically designed, possessing both electrochemical stability and mechanical toughness, far exceeding the single carbon coating strategy.
[0071] 2. This invention provides a method for preparing silicon-carbon composite materials with the above-mentioned structure. Metal nanoclusters are prepared by CVD, and vertical graphene is generated by the directional induction of metal nanoclusters. A complete carbon-coated outer layer is formed by PECVD. By precisely controlling the preparation process parameters, such as temperature, time, and gas flow rate, a good bond between the carbon layer and the silicon-based material is achieved, forming a stable composite structure, which effectively improves the structural stability and conductivity of the material.
[0072] In some implementations, a step-by-step composite material construction process based on pulsed PECVD and step-by-step annealing achieves an integrated process of "material growth - structure control - interface optimization"; effectively preventing side reactions, agglomeration or carbon layer fracture.
[0073] 3. The silicon-carbon composite material provided by this invention has excellent cycle stability and first-time efficiency, and can be used as a high-performance lithium-ion battery anode material. Detailed Implementation
[0074] The following are specific embodiments of the present invention, and the technical solutions of the present invention will be further described, but the present invention is not limited to these embodiments.
[0075] Example 1
[0076] A silicon-carbon composite material based on vertical graphene comprises, from the inside out, a nano-silicon core, palladium nanoclusters, vertical graphene, a PECVD-deposited carbon layer, and a carbon-coated outer layer.
[0077] Prepared by the following steps:
[0078] S1. Place the nano-silicon into a PECVD furnace. The average diameter of the nano-silicon is 120 nm. Then, introduce N2 to purge the air. Then, introduce Ar (10 sccm) + N2 (5 sccm) and heat to 200℃.
[0079] Pd(acac)2 was placed in the vaporization chamber and heated to 135°C to completely vaporize it. Pd(acac)2 was carried into the reaction tube by 35 sccm of Ar carrier gas, while 5 sccm of H2 was carried into the reaction tube by 40 sccm of Ar carrier gas, for a total flow rate of approximately 80 sccm.
[0080] In this process, Pd(acac)2 and H2 are simultaneously pulsed into the reactor, and Ar is continuously introduced between the two pulses. The reaction temperature is 400℃, the pulse duration is 0.5 s, the frequency is 1 Hz, the pulse duration is 900 times, and the reaction is carried out for 15 min to obtain palladium nanoclusters.
[0081] S2. Stop introducing Pd(acac)2 and H2, continue introducing Ar, raise the temperature to 750℃ at a rate of 5℃ / min, maintain the temperature at 750℃, introduce 200 sccm H2 for 10min, and clean the surface.
[0082] Then, C2H2 (20 sccm) + H2 (200 sccm) was introduced to grow vertical graphene for 15 min, yielding vertical graphene with a height of approximately 375 nm. After growth, the carbon source was turned off, and H2 was introduced again for 10 min to remove residual carbon.
[0083] S3. Introduce Ar (150 sccm), slowly cool down to 300℃ at a rate of 1℃ / min, then introduce 10 sccm CH4, and deposit a carbon layer of about 4 nm on the graphene surface in a PECVD low-pressure plasma environment for 80 s.
[0084] The mixture was then cooled to room temperature, and the resulting granules were added to an aqueous solution containing glucose to obtain a slurry. The mass ratio of granules to glucose was 1:2, and the solid content of the slurry was 30%. The slurry was then spray-dried and granulated at a feed rate of 300 mL / h, a spray gas pressure of 2 bar, a nozzle diameter of 100 μm, and a drying temperature of 160 °C.
[0085] Finally, under Ar protection, the temperature was increased to 550℃ at a heating rate of 3℃ / min and held for 1 h to obtain the silicon-carbon composite material.
[0086] Example 2
[0087] A silicon-carbon composite material based on vertical graphene comprises, from the inside out, a nano-silicon core, palladium nanoclusters, vertical graphene, and a carbon-coated outer layer.
[0088] The preparation method is basically the same as that in Example 1, except that no carbon is deposited in step S3.
[0089] Specifically: S3. Ar (150 sccm) was introduced, and the mixture was slowly cooled to room temperature at a rate of 1 °C / min. The resulting particles were then added to an aqueous solution containing glucose to obtain a slurry. The mass ratio of particles to glucose was 1:2, and the solid content of the slurry was 30%. The slurry was then spray-dried and granulated at a feed rate of 300 mL / h, a spray gas pressure of 2 bar, a nozzle diameter of 100 μm, and a drying temperature of 160 °C. Finally, under Ar protection, the temperature was increased to 550 °C at a rate of 3 °C / min and held for 1 h to obtain the silicon-carbon composite material.
[0090] Example 3
[0091] This embodiment is basically the same as embodiment 1, except that in step S1, pulse ventilation is adjusted to continuous ventilation.
[0092] Specifically: Pd(acac)2 and H2 were introduced simultaneously and continuously for a total ventilation time of 450 s.
[0093] Example 4
[0094] This embodiment is basically the same as embodiment 1, except that in step S1, Pd(acac)2 and H2 are pulsed in steps.
[0095] Specifically, one cycle consists of: first, Pd(acac)₂ is introduced into the reaction tube via 35 sccm Ar carrier gas, while simultaneously 40 sccm Ar is introduced, for 0.5 s; then, 5 sccm H₂ is introduced into the reaction tube via 40 sccm Ar carrier gas, while simultaneously 35 sccm Ar is introduced, for 0.5 s. A total of 900 cycles are performed, each lasting 15 minutes.
[0096] Example 5
[0097] This embodiment is basically the same as embodiment 1, except that the pulse conditions are different in step S1.
[0098] Specifically: pulse duration 0.5 s, frequency 0.2 Hz, 900 pulses, duration 75 min.
[0099] Example 6
[0100] This embodiment is basically the same as embodiment 1, except that the pulse conditions are different in step S1.
[0101] Specifically: 0.2 s pulse, 1 Hz frequency, 2250 pulses, for 37.5 min.
[0102] Examples 7-10
[0103] This embodiment is basically the same as embodiment 1, except that the growth time of vertical graphene in step S2 is different, which affects the height of vertical graphene, as shown in Table 1 below.
[0104] Table 1.
[0105] Example Growth time (min) Example 1 15 Example 7 25 Example 8 30 Example 9 5 Example 10 40
[0106] Example 11
[0107] A silicon-carbon composite material based on vertical graphene comprises, from the inside out, a nano-silicon core, platinum nanoclusters, vertical graphene, a PECVD-deposited carbon layer, and a carbon-coated outer layer.
[0108] The preparation method is basically the same as in Example 1, except that Pd(acac)2 is replaced with trimethyl(methylcyclopentadienyl)platinum; and the reaction temperature in step S1 is 500℃.
[0109] Blank example
[0110] The blank example is nano-silicon.
[0111] Comparative Example 1
[0112] This comparative example is basically the same as Example 1, except that it does not have platinum nanoclusters.
[0113] The preparation method is as follows:
[0114] S1. Place the nano-silicon into a PECVD furnace. The average diameter of the nano-silicon is 120 nm. Then, introduce N2 to purge the air. Then, introduce Ar (10 sccm) + N2 (5 sccm) and heat to 200℃.
[0115] S2. Introduce Ar and heat to 750℃ at a rate of 5℃ / min, maintain at 750℃, and then introduce 200 sccm of H2 for 10 min to clean the surface. Then introduce C2H2 (20 sccm) + H2 (200 sccm) and grow for 15 min. After growth, turn off the carbon source and continue to introduce H2 for 10 min to remove residual carbon.
[0116] S3. Ar (150 sccm) was introduced, and the temperature was slowly lowered to 300℃ at a rate of 1℃ / min. Then, 10 sccm of CH4 was introduced, and graphene was deposited on the surface for 80 s using a PECVD low-pressure plasma environment. The mixture was then cooled to room temperature, and the resulting particles were added to an aqueous solution containing glucose to obtain a slurry. The mass ratio of particles to glucose was 1:2, and the solid content of the slurry was 30%. The slurry was then spray-dried and granulated at a feed rate of 300 mL / h, a spray gas pressure of 2 bar, a nozzle diameter of 100 μm, and a drying temperature of 160℃. Finally, under Ar protection, the temperature was increased to 550℃ at a rate of 3℃ / min and held for 1 h to obtain the silicon-carbon composite material.
[0117] Comparative Example 2
[0118] This comparative example is basically the same as Example 1, except that copper nanoclusters are used.
[0119] The preparation method is basically the same as in Example 1, except that Pd(acac)2 is replaced with copper acetylacetonate.
[0120] Performance testing
[0121] The composite materials prepared in the examples, blank examples, and comparative examples were assembled into batteries for testing.
[0122] Battery Assembly: The composite material, conductive agent SP, and binder PVDF are mixed in a mass ratio of 8:1:1 to form a slurry, which is then uniformly coated onto a copper foil current collector. After drying and rolling, the slurry is punched into working electrode sheets. Electrolyte Preparation: A 1.0 mol / L LiPF6 EC / DEC / EMC solution (volume ratio 1:1:1) containing 2% fluoroethylene carbonate is prepared. In an argon-filled glove box (water and oxygen content <0.1ppm), the following components are assembled in sequence: negative electrode shell, working electrode (coated side up), Celgard 2400 separator, electrolyte, lithium sheet, gasket, spring, and positive electrode shell. The assembly is then sealed using a sealing machine.
[0123] Coulomb efficiency test: At 25°C, the first charge and discharge test is performed at a rate of 0.1C within a voltage range of 0.01 to 1.5 V. The capacity is recorded and the first coulomb efficiency is calculated.
[0124] Long-cycle performance (>500 cycles) testing: After activating the battery for 2 cycles at 0.1C rate, a constant current charge-discharge long-cycle test was conducted at 1C rate, with a voltage range of 0.01–1.5 V. The discharge capacity was recorded, and the capacity retention rate at 500 cycles was calculated based on the discharge capacity of the second cycle.
[0125] Specific capacity testing: Charge and discharge tests were performed at a rate of 0.1C and a voltage window of 0.01 to 1.5 V, and the discharge specific capacity after stable cycling was recorded.
[0126] The test results are shown in Table 2 below.
[0127] Table 2.
[0128] experimental group First Coulomb efficiency @ 1.5V (%) Discharge capacity @ 1.5V (mAh / g) 1C cycle 500 cycles capacity retention rate (%) Example 1 93.5 2160 93.1 Example 2 93.8 2210 60.5 Example 3 92.5 1850 80.4 Example 4 92 2120 83.5 Example 5 92.5 1935 79.1 Example 6 93.3 2020 84.8 Example 7 93.6 1950 94.5 Example 8 93.8 1860 93.6 Example 9 91.6 2230 58.2 Example 10 93.6 1560 90.7 Example 11 93.4 2170 93.2 Blank example 70 2950 45.9 Comparative Example 1 91.5 2215 53.5 Comparative Example 2 93.4 2150 70.4
[0129] As shown in Table 2, comparing Example 1, the blank example, and Comparative Examples 1-2, it can be seen that the structural design of the silicon-carbon composite material of the present invention alleviates the volume expansion problem of silicon-based materials during charging and discharging. The PECVD-deposited carbon layer and the carbon-coated outer layer suppress the side reactions at the vertical graphene edges, forming a stable SEI, ensuring high first-efficiency, and exhibiting excellent long-cycle stability. In Comparative Example 1, the lack of palladium nanoclusters makes it difficult to effectively grow vertical graphene. The poor connectivity between the carbon layer and the nano-silicon core results in the inability to provide expansion buffering performance and poor conductivity. In Comparative Example 2, copper nanoclusters are used. Although they can be used to grow vertical graphene, they also form compounds with silicon, affecting the electrical properties of the material.
[0130] Furthermore, as can be seen from the comparison within the embodiments, further controlling the preparation steps of the silicon-carbon composite material of the present invention can optimize the structural morphology of the silicon-carbon composite material and further improve its electrical properties.
[0131] As can be seen from the comparison of Example 1 and Example 2, the carbon layer deposited by PECVD directly and densely coats the VG surface, which can effectively fix the VG, improve the material structure stability, and improve the long cycle life.
[0132] Comparing Examples 1 and 3-6, it can be seen that the growth of palladium nanoclusters is affected by the steps. In Example 3, continuous ventilation easily leads to cluster coarsening. In Example 4, distributed pulses easily lead to uneven clusters. In Example 5, low-frequency pulses result in a large amount of single deposition, resulting in larger cluster size. In Example 6, high-frequency pulses lead to denser clusters. The morphology of palladium nanoclusters affects the subsequent growth morphology and quality of vertical graphene, thereby ultimately affecting the electrical properties of the material.
[0133] Comparing Examples 1 and 7-10, it can be seen that the growth time of vertical graphene affects the height of vertical graphene. In Example 9, the vertical graphene is severely insufficient, and the structure is similar to carbon-coated silicon. During charging, the silicon particles do not have enough space to expand, resulting in a decrease in cycle performance. In Example 10, the vertical graphene is overgrown, resulting in a low overall volumetric capacity of the material.
[0134] The specific embodiments described herein are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.
Claims
1. A silicon-carbon composite material based on vertical graphene, characterized in that: The carbon-silicon composite material comprises, from the inside out, a nano-silicon core, metal nanoclusters, vertical graphene, and a carbon-coated outer layer. The metal is selected from at least one of Pt and Pd.
2. The carbon-silicon composite material based on vertical graphene according to claim 1, characterized in that: A PECVD-deposited carbon layer is also present between the vertical graphene and the carbon-coated outer layer.
3. The carbon-silicon composite material based on vertical graphene according to claim 1, characterized in that: The height of the vertical graphene is 3 to 5 times the diameter of the nano-silicon.
4. A method for preparing a silicon-carbon composite material based on vertical graphene as described in any one of claims 1 to 3, characterized in that: Includes the following steps: S1. In a PECVD furnace, after cleaning and preheating the nano-silicon, the precursor vapor of the metal is introduced through an inert carrier gas of 20-50 sccm, while hydrogen is introduced at the same time. After deposition for 10-30 min, nano-silicon cores MNCs / Si with metal nanoclusters on the surface are obtained. The total gas flow rate is 50–100 sccm; the volume concentration of hydrogen in the total gas flow is 1 vol%–10 vol%. When the metal is Pt, the deposition temperature is 350℃~600℃; when the metal is Pd, the deposition temperature is 300℃~500℃. S2. After preheating and cleaning the surface, the first carbon source and hydrogen are introduced, and vertical graphene is grown at 700℃~800℃ to obtain vertical graphene and nano-silicon cores VG / MNCs / Si connected by metal nanoclusters. S3. The VG / MNCs / Si is mixed with a solution of a second carbon source, spray-dried, and sintered to obtain the silicon-carbon composite material C / VG / MNCs / Si.
5. The method for preparing a silicon-carbon composite material based on vertical graphene according to claim 4, characterized in that: In step S3, the VG / MNCs / Si is first cooled to 200℃~400℃, a third carbon source is introduced, and 2~5 nm of carbon is deposited on the surface to obtain a PECVD deposited carbon layer; then it is cooled to room temperature, mixed with the solution of the second carbon source, spray dried, and sintered.
6. The method for preparing a silicon-carbon composite material based on vertical graphene according to claim 4, characterized in that: In step S2, the growth rate of the vertical graphene is controlled at 10–25 nm / min.
7. A method for preparing a silicon-carbon composite material based on vertical graphene according to claim 4 or 6, characterized in that: In step S2, the flow rate of the first carbon source is 15-25 sccm, and the flow rate of the hydrogen is 150-250 sccm.
8. The method for preparing a silicon-carbon composite material based on vertical graphene according to claim 4, characterized in that: In step S1, a synchronization pulse is introduced into the precursor vapor of the metal and hydrogen gas.
9. The method for preparing a silicon-carbon composite material based on vertical graphene according to claim 8, characterized in that: The pulse duration is 0.1–1 s, and the frequency is 0.1–10 Hz.
10. A lithium-ion battery, characterized in that: The negative electrode includes a silicon-carbon composite material based on vertical graphene as described in any one of claims 1 to 3.
Citation Information
Patent Citations
Uniform carbon film and vertical graphene dual-coated silicon-carbon composite material, preparation method thereof and application in lithium ion battery
CN109616630A