Method for preparing Anti-adhesion membrane by electrostatic spinning
By dissolving chitosan and toughening agent in a dilute acid solution and using electrospinning technology to prepare an anti-adhesion membrane, the problem of insufficient toughness of the fiber membrane and solvent residue is solved, high porosity and mechanical properties are improved, and it meets the needs of clinical prevention. adhesion requirements, and improves environmental protection and safety.
Patent Information
- Application Number
- PCT/CN2023/093262
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-05-10
- Publication Date
- 2024-10-24
AI Technical Summary
When preparing anti-adhesion membranes with the existing technology, the fiber membrane has insufficient toughness, solvent residue problems, poor environmental safety, and poor mechanical properties, making it difficult to meet clinical needs.
Using electrospinning technology, chitosan and toughening agent are dissolved in a dilute acid solution to form a transparent solution, and then a fiber membrane is formed through electrospinning. A low-toxic and volatile solvent system is selected and removed through vacuum drying and ventilation. Residual solvent, adjust spinning parameters to obtain high porosity and suitable mechanical properties.
The prepared fibrous membrane has good biocompatibility, anti-tissue adhesion and mechanical strength, can effectively prevent adhesion, and self-degrades after wound healing, meets clinical use requirements, and is environmentally friendly and safe.
Smart Images

Figure CN2023093262_24102024_PF_FP_ABST
Abstract
Description
A method for preparing anti-adhesion film by electrostatic spinning Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and particularly relates to a method for preparing an anti-adhesion film by electrostatic spinning. Background Art
[0002] Adhesions are a phenomenon in which previously separate tissues or organs become fused together due to the deposition of abnormal connective tissue around the wound after surgery or other tissue damage. Adhesions occur frequently (approximately 60% to 90%) and can lead to complications such as chronic abdominal pain and bloating, intestinal obstruction, and infertility, severely impacting patients' physical and mental health. Therefore, treatment must be timely and effective. Adhesions are abnormal repair processes triggered by an immune response following tissue damage. Minimizing the adhesion of tissue cells at the injured interface or regulating their activity is key to addressing this problem.
[0003] In clinical practice, a "short-term barrier" approach is often used to address adhesions. This involves applying a barrier material to areas where adhesions may occur. Ideally, these materials should be biocompatible, non-toxic, and biodegradable, thus avoiding secondary surgeries. Furthermore, they should remain in the body long enough for the injury to heal, and their degradation products should be absorbed by the body without causing adverse reactions.
[0004] Chitosan is a naturally amino-containing homogeneous linear polysaccharide. It contains free amino groups. Its final product in the body is glucosamine, which can be absorbed by the body. Chitosan is insoluble in water and organic solvents, but soluble in dilute acid with a pH of <6.5. In dilute acid, its glucosamine is converted into R-NH3 + , forming a polycationic gel solution. Chitosan has excellent biodegradability, low toxicity, and biocompatibility, making it widely used in the fields of biomaterials and medicine.
[0005] Chitosan is an excellent anti-adhesion material, and its anti-adhesion mechanism is as follows: (1) It can act as a polymer barrier to prevent adhesion between tissues and isolate damage; (2) It can selectively promote the growth of epithelial cells and inhibit the growth rate of fibroblasts, induce fibroblast apoptosis, reduce collagen deposition, and inhibit scar formation; (3) It can downregulate the expression of inflammatory factors, enhance the activity of the fibrinolytic system and matrix metalloproteinase system, and reduce the occurrence of adhesion; (4) It has a hemostatic effect and reduces adhesion caused by hematoma; (5) It has an antibacterial effect, reduces the risk of local infection, and reduces local adhesion caused by infection and inflammation.
[0006] Compared to gel- and solution-based anti-adhesion products, membrane-based products offer advantages such as a superior physical barrier and a longer duration of action, making them widely used in the field of postoperative adhesion prevention. Among membrane-based anti-adhesion materials, electrospun membranes have high porosity and a large surface area, which facilitates the infiltration of nutrients and suppresses inflammation. Furthermore, fibroblasts cannot grow into them due to their smaller pores, making them an ideal anti-adhesion material.
[0007] Electrospinning is a commonly used method for preparing micro-nano fibers. Its principle is: under the action of a high-voltage electric field, the surface of charged polymer droplets generates an electrostatic force opposite to the surface tension. When the electric field force is large enough, the polymer droplets overcome the surface tension to form a jet stream. During the jetting process, the solvent evaporates or solidifies, and finally forms a fiber mat similar to a non-woven fabric on the receiving device.
[0008] Electrospinning is widely used in the field of anti-adhesion membranes for postoperative adhesion prevention due to its simple process, mature technology, low spinning cost, adjustable and uniform diameter, high porosity, and large specific surface area. Currently, the main methods for forming postoperative adhesion membranes are cast film and electrospinning. Compared with cast film, which is complex, produces films with poor flexibility and adhesion, and typically requires surgical suture fixation, electrospinning is a mature process with simple operation, relatively uniform fiber size, and excellent mechanical properties. Its microporous structure facilitates the transport of nutrients.
[0009] Solution electrospinning also requires consideration of residual solvent in the finished product. Residual solvent in the fiber membrane should be removed as much as possible. This issue can be addressed in two ways: first, choosing a low-toxic solution system for dissolution; second, selecting a solute that is volatile or easy to handle without damaging the membrane structure, thus facilitating the removal of residual solvent during post-processing. A solution system that meets these requirements should be considered ideal.
[0010] Chitosan electrospinning alone is difficult to achieve. Even if a membrane is spun, it is very brittle and has almost no toughness. A light pinch of the finger will break it into pieces, making it unusable for clinical use. Therefore, to increase the toughness of the material, a toughening agent must be added. A wide range of toughening agents are available, including but not limited to the following: polycaprolactone, gelatin, collagen, polylactic acid, poly(lactic-co-glycolic acid), poly(lactic-co-caprolactone), and polyvinyl alcohol.
[0011] Chinese patent publication number CN115607732A discloses a biomimetic nerve graft and its preparation method. The graft's nanofiber membrane consists solely of chitosan, dissolved in polyethylene oxide. This system lacks a toughening agent, resulting in a poorly tough fiber membrane and requiring improved mechanical properties. Residual polyethylene oxide in the fiber membrane is removed by washing, which may affect the membrane's morphology and hinder uniform production.
[0012] Chinese patent publication number CN115624648A discloses a method for preparing chitosan / mesoporous silica-modified medical hemostatic gauze and its product. Chitosan and cellulose acetate are dissolved in a 1:1 volume ratio of acetone and DMF solution, and mesoporous silica is added to produce a spinning solution. Acetone, a precursor chemical, is a potential threat to manufacturers and poses a risk to the environment. Its environmental friendliness and safety are inferior to acids.
[0013] Chinese patent application publication number CN115364284A discloses an absorbable composite anti-adhesion membrane consisting of three layers. The outermost layer is a dense PLA (polylactic acid) membrane. This structure poses certain obstacles to nutrient exchange. The layer in contact with tissue is a PLA electrospun membrane. Although it can prevent the growth of fibroblasts, the polylactic acid will produce acidic degradation products during the degradation process, which may irritate the body's tissues and organs.
[0014] Chinese patent application publication number CN 100525778C discloses a novel postoperative anti-adhesion material and its preparation method. The material comprises chitosan and a polyanion or polyethylene glycol. The preparation method comprises: 1) dissolving chitosan in acid to form a chitosan solution; 2) mixing the polyethylene glycol or polyanion with distilled water to form a solution. The anti-adhesion material of the invention is obtained by mixing the solutions in 1) and 2) above. This material is in a liquid or gel state and, compared to electrospun membranes, has poorer structural stability, is difficult to fix in the body, and is prone to dislocation.
[0015] The Chinese patent application with publication number CN111012950A discloses a composite repair patch and its preparation method. The materials involved in the patch include chitosan, graphene oxide, hexafluoroisopropanol, trifluoroethanol, etc., and the method has complicated steps, which will increase a lot of additional costs in industrial production.
[0016] Summary of the Invention
[0017] In response to the existing technical problems, the present invention aims to provide a method for preparing an anti-adhesion membrane through electrospinning. The electrospun membrane of this invention has a porous structure, which facilitates the flow of nutrients and other substances. Furthermore, the pores are smaller than the size of fibroblasts, preventing them from accumulating and inhibiting their migration, thereby suppressing the development of inflammation.
[0018] In order to solve the above problems, the technical solutions adopted by the present invention are as follows:
[0019] A method for preparing an anti-adhesion membrane through electrospinning involves dissolving chitosan and a toughening agent in a dilute acid solution to form a stable, transparent solution, which is then electrospun into a fiber membrane. The solution, which includes chitosan, a toughening agent, and a dilute acid solution, provides ionizable hydrogen ions that bind to amino groups in the chitosan molecules, altering the hydrogen bonds between and within the chitosan molecules and causing them to dissolve.
[0020] The method for preparing an anti-adhesion film by electrospinning comprises preparing a dilute acid solution using pure acid and pure water, with a volume percentage of 10% to 90% and a pH of <6.5. The acid is selected based on toxicity, and acids that are highly toxic and difficult to remove through post-treatment are not considered.
[0021] In the method for preparing the anti-adhesion film by electrospinning, the dilute acid solution is a mixed solution of one or more of acetic acid, formic acid, hydrochloric acid, dichloroacetic acid or trifluoroacetic acid.
[0022] In the method for preparing the anti-adhesion film by electrostatic spinning, the usage ratio of chitosan, dissolved toughening agent and dilute acid solution is 1-9 g:1-9 g:10 mL.
[0023] In the method for preparing an anti-adhesion film by electrospinning, the chitosan is any one of carboxymethylated chitosan, hydroxypropylated chitosan, sulfated chitosan, quaternized chitosan, chitosan derived from microbial fermentation, or chitosan derived from shrimp shells; and the molecular weight of the chitosan ranges from hundreds of thousands to millions.
[0024] In the method for preparing an anti-adhesion film by electrostatic spinning, the toughening agent is any one of polycaprolactone, gelatin, collagen, polylactic acid, polylactic acid-co-glycolic acid, polylactic acid-caprolactone copolymer or polyvinyl alcohol or a composite system thereof.
[0025] The method for preparing an anti-adhesion film by electrospinning comprises placing chitosan and a toughening agent into a prepared dilute acid solution and stirring the solution until it becomes transparent and uniform; the stirring temperature is between 15°C and 35°C. The stirring temperature should be neither too low nor too high. If the temperature is too low, a uniform and transparent solution system will not be formed. If the temperature is too high, the degradation of the chitosan and toughening agent in the dilute acid solution will be accelerated, thereby changing the properties of the solution.
[0026] The method for preparing an anti-adhesion membrane by electrospinning comprises: drawing a dissolved transparent solution into a syringe or placing it into a spinning solution storage component, spinning in a suitable temperature and humidity environment, and removing the spinning membrane from a collecting device; the spinning process is any one of solution electrospinning, needle electrospinning, needleless electrospinning, single-needle electrospinning, multi-needle electrospinning, unilateral electrospinning or opposite-side electrospinning, or a combination of the above processes; the spinning temperature is 20-26°C; and the spinning humidity is 35% to 68%.
[0027] A method for preparing an anti-adhesion film by electrospinning, comprising the following steps:
[0028] (1) Solution preparation: Dissolve chitosan and toughening agent in a dilute acid solution system and stir to obtain a transparent and uniform spinning solution;
[0029] (2) electrospinning: placing the spinning solution obtained in step (1) into the injector of the electrospinning machine, adjusting the ambient temperature and humidity of the spinning process, and then spinning to obtain an electrospun fiber membrane;
[0030] (3) Place the fiber membrane collected in step (2) in a vacuum drying oven for 72 hours, then take it out and place it in a ventilated place for 48 hours.
[0031] The anti-adhesion fiber membrane is prepared by the above method.
[0032] Beneficial effects: Compared with the existing technology, the advantages of the present invention include:
[0033] The present invention selects a low-toxic and volatile solvent system, and the residual solvent in the spinning membrane can be removed by a simple drying method. The residual solvent is less than 5000ppm, and it is more environmentally friendly and safer than acetone.
[0034] The electrospun anti-adhesion membrane prepared by the present invention can adjust the mechanical properties by controlling the spinning solution ratio and spinning parameters, and can be used to prepare fiber membranes with various mechanical differences required for different tissue repair.
[0035] The fiber membrane prepared by the present invention has good biocompatibility and better anti-tissue adhesion, and can be attached to tissue damage without irritation;
[0036] Because the anti-adhesion membrane is a degradable material, it basically does not degrade before the wound heals (the initial degradation time is greater than 30 days), can fully play a barrier role, and can degrade itself after the tissue heals.
[0037] The mechanical strength of the membrane can meet normal clinical use and is easy for doctors to operate;
[0038] The membrane has high porosity and its thickness can be flexibly adjusted by controlling the spinning parameters and spinning time to meet the needs of different tissues.
[0039] The fiber formation in the fiber membrane is stable, and the fiber diameter is controlled between 30 and 4000 nm.
[0040] The electrospun micro-nano fiber membrane of the present invention is used for postoperative adhesion prevention in vivo. It has excellent tissue compatibility and pore structure, can play a necessary physical barrier role at the site of postoperative tissue damage, and has excellent performance in reducing adhesion between tissues in corresponding parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 shows the appearance of an electrospun membrane prepared with a mass ratio of polycaprolactone to chitosan of 7:3:
[0042] Figure 2 is an electron micrograph of an electrospun membrane prepared with a mass ratio of polycaprolactone to chitosan of 7:3:
[0043] Figure 3 shows the stress-strain curves of pure PCL membrane and CS / PCL blended membrane:
[0044] Figure 4 shows the adhesion of an electrospun membrane made with a polycaprolactone and chitosan mass ratio of 7:3 after implantation into rats on day 14:
[0045] Figure 5 is an H&E staining image of an electrospun membrane made with a mass ratio of polycaprolactone to chitosan of 7:3 after implantation into rats on day 14:
[0046] Figure 6 shows the cytotoxicity test results of fiber membranes with different PCL / CS contents. DETAILED DESCRIPTION
[0047] To make the above-mentioned objects, features and advantages of the present invention more clearly understood, the following describes the specific embodiments of the present invention in detail with reference to specific examples. Note: The chitosan used in the following examples is all shrimp shell chitosan with a molecular weight of 400,000 to 500,000.
[0048] Example 1
[0049] A raw material compounding system and solvent system for preparing an anti-adhesion film by electrospinning are as follows:
[0050] Raw material compounding system: gelatin and chitosan mass ratio is 8:2, totaling 10g;
[0051] Solvent system: acetic acid and pure water in a volume ratio of 8:2, a total of 10 ml;
[0052] The above two systems were mixed and stirred at 30°C to obtain a transparent and uniform spinning solution.
[0053] Take the spinning solution prepared above and use needle electrospinning for spinning. The needle specification is 20G, single needle, voltage is 25kV, temperature is 26℃, humidity is 45%, injection speed is 1.0mL / h, spinning time is 10 hours, and finally a fiber membrane with a fiber diameter of 60 to 2000nm is obtained.
[0054] Example 2
[0055] A raw material compounding system and solvent system for preparing an anti-adhesion film by electrospinning are as follows:
[0056] Raw material compound system: gelatin, collagen and chitosan mass ratio is 4:4:2, totaling 10g;
[0057] Solvent system: acetic acid and pure water in a volume ratio of 9:1, a total of 10 ml;
[0058] The above two systems were mixed and stirred at 30°C to obtain a transparent and uniform spinning solution.
[0059] Take the spinning solution prepared above and use needle electrospinning for spinning. The needle specification is 20G, single needle, voltage is 25kV, temperature is 26℃, humidity is 45%, injection speed is 1.0mL / h, spinning time is 10 hours, and finally a fiber membrane with a fiber diameter of 60 to 2000nm is obtained.
[0060] Example 3
[0061] Take the spinning solution prepared in Example 2 and use needle electrospinning for spinning. The needle specification is 21G, with double needles on the same side, the voltage is 22-28kV, the temperature is 22°C, the humidity is 44%-68%, the injection speed is 1.5mL / h, and the spinning time is 8 hours. Finally, a fiber membrane with a fiber diameter of 50-1800nm is obtained.
[0062] Example 4
[0063] Take the spinning solution prepared in Example 2 and use needle electrospinning for spinning. The needle specification is 21G, with double needles on the opposite side, the voltage is 22-28kV, the temperature is 20°C, the humidity is 48%-62%, the injection speed is 1.3mL / h, and the spinning time is 8 hours. Finally, a fiber membrane with a fiber diameter of 40-2000nm is obtained.
[0064] Example 5
[0065] A method for preparing an anti-adhesion film by electrospinning, comprising the following steps:
[0066] (1) Solution preparation: Dissolve polycaprolactone and chitosan (mass ratio: 7:3, total 10 g) in a mixed solvent of acetic acid and water (volume ratio: 9:1, total 10 ml) and stir at 20°C to obtain a transparent and uniform spinning solution;
[0067] (2) Electrospinning: Using needle electrospinning, the spinning solution obtained in step (1) was placed in the injector of the electrospinning machine, the distance between the spinneret (21G) and the drum was adjusted to 16 cm, the spinning environment temperature was 25 ° C, the ambient humidity was 45% to 50%, the voltage was adjusted to 25 kV, the solution feed rate was 1.2 mL / h, and spinning was carried out for 10 hours. An electrospun fiber membrane was obtained on the drum, and the fiber diameter was between 80 and 2000 nm;
[0068] (3) The fiber membrane collected in step (2) was placed in a vacuum drying oven at a drying temperature of 37°C for 72 hours, and then taken out and placed in a ventilated place for 48 hours.
[0069] Figure 1 is the appearance of the electrospun membrane prepared by the above method. As can be seen from Figure 1, the material has good film-forming properties and its mechanical properties meet the requirements of clinical operation. Figure 2 is an electron microscope image of the electrospun membrane prepared by the above method. As can be seen from Figure 2, the material has the characteristics of large specific surface area and large porosity, which is conducive to the exchange of substances. Figure 3 is a stress-strain curve diagram of pure PCL membrane and CS / PCL blended membrane: the mechanical properties of the material prepared by this method can be flexibly controlled by changing the ratio of the two solvents. Figure 4 is a diagram of the adhesion of the above electrospun membrane after implantation in rats on the 14th day: the material prepared by this method can achieve an anti-adhesion effect. Figure 5 is an H&E staining image of the above electrospun membrane after implantation in rats on the 14th day: the material prepared by this method can play an anti-adhesion role.
[0070] Example 6
[0071] A method for preparing an anti-adhesion film by electrospinning, comprising the following steps:
[0072] (1) Solution preparation: Gelatin and chitosan (mass ratio: 7:3, total 10 g) were dissolved in a mixed solvent of formic acid and water (volume ratio: 9:1, total 10 ml) and stirred at 20°C to obtain a transparent and uniform spinning solution;
[0073] (2) Electrospinning: Using needle electrospinning, the spinning solution obtained in step (1) was placed in the injector of the electrospinning machine, the distance between the spinneret (20G) and the drum was adjusted to 16 cm, the spinning environment temperature was 20°C, the ambient humidity was 40% to 65%, the voltage was adjusted to 24 kV, the solution feed rate was 1.3 mL / h, and spinning was carried out for 10 h. An electrospun fiber membrane was obtained on the drum, and the fiber diameter was between 100 and 2000 nm.
[0074] (3) The fiber membrane collected in step (2) was placed in a vacuum drying oven at a drying temperature of 37°C for 72 hours, and then taken out and placed in a ventilated place for 48 hours.
[0075] Example 7
[0076] A method for preparing an anti-adhesion film by electrospinning, comprising the following steps:
[0077] (1) Solution preparation: Dissolve polycaprolactone, gelatin, and chitosan (mass ratio: 4:3:3, total 10 g) in a mixed solvent of acetic acid and water (volume ratio: 9:1, total 10 ml) and stir at 25°C to obtain a transparent and uniform spinning solution;
[0078] (2) Electrospinning: Using needle electrospinning, the spinning solution obtained in step (1) was placed in the injector of the electrospinning machine, the distance between the spinneret (19G) and the drum was adjusted to 16 cm, the spinning environment temperature was 23 ° C, the ambient humidity was 35% to 60%, the voltage was adjusted to 26 kV, the solution feed rate was 1.5 mL / h, and spinning was carried out for 10 hours. An electrospun fiber membrane was obtained on the drum, and the fiber diameter was between 70 and 2000 nm;
[0079] (3) The fiber membrane collected in step (2) was placed in a vacuum drying oven at a drying temperature of 37°C for 72 hours, and then taken out and placed in a ventilated place for 48 hours.
[0080] Example 8
[0081] Fibroblast toxicity test
[0082] L-929 fibroblasts were cultured in 24-well plates using complete culture medium containing 10% FBS and 1% double-antibody in a sterile environment of 5% CO2 and 37°C. When the cells reached 90% confluence, the culture medium was discarded, the cells were washed with sterile PBS solution, 1 mL of fresh culture medium was added to each well, and an experimental sample was gently placed on the upper layer of cells in each well, covering approximately one-tenth of the cell layer surface. High-density polyethylene of the same thickness and area size was used as a negative control for synthetic polymers, and polyvinyl chloride stabilized with organotin was used as a positive control. Culture was continued for 24 hours. The cytotoxicity of the material was measured using the CCK-8 method.
[0083] The cell survival rates of the anti-adhesion membranes prepared by electrospinning with PCL / CS content of 9 / 1, 8 / 2, 7 / 3, and 6 / 4 were all greater than 95% ( Figure 6 ). The results showed that the blended membranes had good cell compatibility and low cytotoxicity.
[0084] Example 9
[0085] In vitro degradation experiment of fiber membrane (PBS solution)
[0086] Dissolve PBS powder in deionized water to prepare 0.2 M PBS (pH 7.4) solution. Carefully weigh 10 × 2 (diameter × thickness) mm 2 The disc-shaped specimens were then immersed in a PBS solution in a sealed glass tube with a 0.02% mass fraction of sodium azide. These tubes were degraded in a shaking incubator at 37°C and 80 rpm for different times without changing the solution. At the end of the predetermined degradation interval (weekly), three samples from each group were taken for degradation analysis and pH measurement. The removed samples were washed with deionized water, dehydrated with 99.9% ethanol, and vacuum dried to constant weight under ambient conditions before gravimetric determination.
[0087] The mass loss rate (W loss) is calculated by the following formula: W 损 =
(W 初 -W 损 ) / W 初
[0088] Where W 初 is the initial weight of the sample before degradation, W 损 is the remaining weight of samples at different intervals after degradation.
[0089] The results showed that the mass loss rate was about 2% at 28 days and about 6% at 70 days. The mass loss rate increased linearly with the extension of degradation time.
Claims
1. A method for preparing an anti-adhesion film by electrospinning, characterized in that: Chitosan and toughening agent are dissolved in a dilute acid solution system to form a stable transparent solution, and then a fiber membrane is formed by electrospinning technology.
2. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: Use pure acid and pure water to prepare a dilute acid solution, the volume percentage of the dilute acid is 10% to 90%, and the pH of the dilute acid solution is <6.
5.
3. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: The dilute acid solution is a mixed solution of one or more of acetic acid, formic acid, hydrochloric acid, dichloroacetic acid or trifluoroacetic acid.
4. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: The dosage ratio of chitosan, dissolved toughening agent and dilute acid solution is 1-9g:1-9g:10mL.
5. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: The chitosan is any one of carboxymethylated chitosan, hydroxypropylated chitosan, sulfated chitosan, quaternized chitosan, chitosan derived from microbial fermentation, or chitosan derived from shrimp shells.
6. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: The toughening agent is any one of polycaprolactone, gelatin, collagen, polylactic acid, polylactic acid-glycolic acid copolymer, polylactic acid-caprolactone copolymer or polyvinyl alcohol or a composite system thereof.
7. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: Chitosan and toughening agent are placed in the prepared dilute acid solution, and stirred to make the solution transparent and uniform; the stirring temperature is 15-35°C.
8. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: The dissolved transparent solution is drawn into a syringe or placed into a spinning solution storage component, spinning is carried out in a suitable temperature and humidity environment, and the spinning membrane is removed from the collecting device; the spinning process is any one of solution electrospinning, needle electrospinning, needleless electrospinning, single-needle electrospinning, multi-needle electrospinning, single-side electrospinning or opposite-side electrospinning, or a combination of the above processes; the spinning temperature is 20-26°C; the spinning humidity is 35% to 68%.
9. The method for preparing an anti-adhesion film by electrospinning according to claim 1, characterized in that: The following steps are involved: (1) Solution preparation: dissolving chitosan and toughening agent in a dilute acid solution system and stirring to obtain a transparent and uniform spinning solution; (2) electrospinning: placing the spinning solution obtained in step (1) in the injector of an electrospinning machine, adjusting the spinning environment temperature and humidity, and then spinning to obtain an electrospun fiber membrane; (3) The fiber membrane collected in step (2) is placed in a vacuum drying oven for 72 hours, and then taken out and placed in a ventilated place for 48 hours.
10. The anti-adhesion fiber membrane prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing chitosan-based superfine fiber carrier material for medical dressing
CN103394114A
A polyvinyl alcohol / collagen / quaternized chitosan electrospun composite fiber film and a preparing method thereof
CN107693835A
Preparation method of chitosan / polyvinyl alcohol nanofiber containing nanocellulose
CN111304779A
Chitosan / polycaprolactone composite nanofiber membrane material and application thereof
CN111793900A
Nanometer ultrafine fibre film material of chitose and its preparation method
CN1569254A
Cited By
Polyelectrolyte composite nanofiber membrane prepared by using coaxial double-row electrostatic spinning process and preparation method of polyelectrolyte composite nanofiber membrane
CN119265803A