High-performance positive electrode material, and preparation method therefor and use thereof
By using doped nanometal elements in lithium batteries to catalyze lithium-containing compounds and porous materials to accelerate lithium ion conduction, the problem of low Coulombic efficiency of silicon anode materials in lithium batteries is solved for the first time, improving the energy density and safety performance of the battery, and realizing Safe, low-cost battery capacity and cycle life extension.
Patent Information
- Application Number
- PCT/CN2023/113243
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-08-16
- Publication Date
- 2024-10-24
AI Technical Summary
When silicon anode materials are used in lithium batteries, the first problem is low Coulombic efficiency, which leads to capacity fading and short cycle life of lithium batteries. Existing lithium replenishment technology has high environmental requirements and high costs, making it difficult to achieve large-scale application.
Doped nanometal elements are used to catalyze lithium-containing compounds during the charge and discharge process, completely decomposing lithium ions, and accelerating the internal conduction of lithium ions through porous materials, improving the conductive properties of the cathode material, and achieving safe and low-cost battery capacity. and cycle life extension.
It improves the energy density and safety performance of lithium batteries, avoids gas production problems during battery use, reduces production costs, and improves battery capacity and cycle life.
Smart Images

Figure CN2023113243_24102024_PF_FP_ABST
Abstract
Description
A high-performance cathode material and its preparation method and application
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 19, 2023, with application number 202310426149.5 and invention name “A high-performance positive electrode material, its preparation method and application”. Technical Field
[0002] The present invention relates to the technical field of lithium battery materials, and in particular to a high-performance positive electrode material and a preparation method and application thereof. Background Art
[0003] With the rapid development of green and low-carbon industries in my country and the increasing penetration of new energy vehicles, energy storage batteries are experiencing rapid growth. Lithium batteries, with their advantages of high voltage, large specific capacity, high energy density, no memory effect, long cycle life, and environmental friendliness, have become the primary choice for rechargeable power sources in portable electronic products, new energy vehicles, and other applications.
[0004] To meet current development needs, electrode materials with high energy density and high specific capacity have become a primary consideration for battery companies. Silicon-based materials, due to their abundant reserves and ultra-high theoretical specific capacity, have become the top choice for battery companies as anode materials, representing one of the most promising anode materials for next-generation lithium-ion batteries.
[0005] However, after adopting silicon negative electrodes, the problem of low initial coulombic efficiency becomes more prominent. This is because the large expansion of silicon causes the solid electrolyte interface (SEI) film on the silicon surface to be in a dynamic process of "destruction-reconstruction", which ultimately leads to a continuous increase in SEI film thickness, increased interfacial impedance, and consumption of active materials, resulting in capacity decay and reduced initial efficiency. Therefore, in order to ensure the capacity of the battery, it is necessary to replenish the lost lithium and extend the cycle life of the lithium battery.
[0006] Currently, many companies are using negative electrode lithium replenishment technology. These methods generally include simple and effective methods such as pre-lithiation of silicon-based negative electrode materials with metallic lithium powder, electrochemical pre-lithiation, and direct contact short-circuiting. However, these methods require high environmental standards, such as an oxygen-free, water-free, and dry environment. The metallic lithium negative electrode lithium replenishment process places extremely high demands on the production environment, requiring sealed slurry mixing equipment and high costs, making it difficult to implement on a large scale.
[0007] Therefore, major battery companies and battery material companies are actively exploring and seeking technological breakthroughs in how to safely, cost-effectively and simply replenish lithium to improve overall battery capacity and cycle life.
[0008] Summary of the Invention
[0009] The present invention aims to provide a high-performance positive electrode material, its preparation method, and its application. By utilizing doped nano-metal elements, inactive lithium-containing compounds at room temperature are catalyzed during the charge and discharge process, causing the lithium-containing compounds to completely decompose into lithium ions, thereby increasing the battery's energy density. Simultaneously, the gas produced by the completely catalytically decomposed lithium-containing compounds is also discharged during the battery formation process, avoiding gas production during normal battery use and improving battery safety. Furthermore, the doped metal elements and porous materials can accelerate the internal conduction rate of lithium ions, improving the conductivity of the positive electrode material, ultimately achieving the goal of increasing overall battery capacity and cycle life using a safe, low-cost, and simple process.
[0010] To this end, in a first aspect, an embodiment of the present invention provides a high-performance positive electrode material, which is used in a lithium battery. The positive electrode material includes: a porous material, a lithium-containing compound, metal element nanoparticles, and a positive electrode active material;
[0011] The lithium-containing compound includes: an inorganic lithium source material and / or an organic lithium source material; the inorganic lithium source material includes: one or more of lithium carbonate, lithium oxide, lithium phosphate, lithium manganate, lithium hydroxide or lithium iodide; the organic lithium source material includes: one or more of butyl lithium, phenyl lithium, cyclopentadiene dilithium, and lithium acetate;
[0012] The metal element nanoparticles include: one or more elements and / or alloys of Al, Ti, Mn, Co, Ni, Cu, Zn, Zr, Mo, Ge, and Sn; the particle size D V100 ≤500nm;
[0013] During the first charge and discharge cycle of the lithium battery, the reaction active sites on the metal surface of the metal element nanoparticles adsorb inert lithium-containing compounds, causing the chemical bonds in the lithium-containing materials to deform or break, producing a catalytic effect on the lithium-containing compounds. The active centers of the electrocatalytic reaction provided by the specific surface area of the metal element nanoparticles enhance the catalytic effect, jointly promoting the complete decomposition of lithium-containing compounds into lithium ions, thereby improving the energy density and safety performance of the lithium battery.
[0014] Preferably, the average particle size D of the porous material is V50 The pore size is between 100nm-100μm, the pore size distribution is between 1nm-500nm, and the porosity distribution is between 30%-95%;
[0015] The particle size D of the lithium-containing compound 50 Between 0.5nm-10μm;
[0016] The particle size D of the positive electrode active material V50Between 5-20μm.
[0017] Preferably, the porous material comprises: one or more of porous carbon, graphene microspheres, single-walled carbon nanotubes and multi-walled carbon nanotubes;
[0018] The positive electrode active material includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide.
[0019] Preferably, the mass of the positive electrode active material accounts for 80%-99.9% of the total mass of the positive electrode material;
[0020] The total mass of the porous material, the lithium-containing compound, and the metal element nanoparticles accounts for 0.1%-20% of the total mass of the positive electrode material.
[0021] Preferably, the mass of the positive electrode active material accounts for 70%-94% of the total mass of the positive electrode material;
[0022] The total mass of the porous material, the lithium-containing compound, and the metal element nanoparticles accounts for 6% to 30% of the total mass of the positive electrode material;
[0023] The porous material accounts for 0.5%-15% of the total mass of the positive electrode material; the metal element nanoparticles account for 0.5%-10% of the total mass of the positive electrode material; and the lithium element-containing compound accounts for 5%-20% of the total mass of the positive electrode material.
[0024] In a second aspect, an embodiment of the present invention provides a method for preparing the high-performance cathode material described in the first aspect, wherein the preparation method is a liquid phase method:
[0025] uniformly dispersing metal element nanoparticles and lithium-containing compounds in an organic solvent to obtain a premixed solution;
[0026] Adding the porous material to the premixed solution and fully and evenly dispersing it for 2-10 hours to obtain a mixed solution;
[0027] The mixed solution is placed in a high-temperature furnace, heated to 600° C.-1000° C. in an inert atmosphere, and kept warm for 2 hours-10 hours. After the material is discharged, it is crushed and sieved to obtain a precursor material;
[0028] The precursor material and the positive electrode active material are placed in a mixing device and mixed for 0.5 hours to 5 hours. After the mixture is evenly mixed, a high-performance positive electrode material is obtained.
[0029] Preferably, the organic solvent includes one or more of toluene, isopropyl alcohol, anhydrous ethanol, dimethylformamide, acetone, ethylene glycol dimethyl ether or tetrahydrofuran.
[0030] Preferably, the mixing equipment includes one or more of a stirrer, a disperser, a ball mill, and an ultrasonic machine;
[0031] The heating furnace includes one or more of a box-type heating furnace, a tubular heating furnace, and a rotary furnace.
[0032] In a third aspect, an embodiment of the present invention provides a positive electrode plate, which includes the high-performance positive electrode material described in the first aspect.
[0033] In a fourth aspect, an embodiment of the present invention provides a lithium battery comprising the positive electrode sheet described in the third aspect.
[0034] The high-performance positive electrode material provided by the embodiment of the present invention utilizes doped nano-metal elements to catalyze lithium-containing compounds that are inactive at room temperature during the charge and discharge process, so that the lithium-containing compounds are completely decomposed into lithium ions, thereby improving the battery energy density; at the same time, the gas generated by the lithium-containing compounds that are completely catalytically decomposed is also discharged during the battery formation process, avoiding the problem of gas production during normal use of the battery and improving the safety performance of the battery; in addition, the doped metal elements and porous materials can accelerate the internal conduction rate of lithium ions and improve the conductive properties of the positive electrode material, ultimately achieving the purpose of using a safe, low-cost, and simple process to achieve the purpose of increasing the overall battery capacity and cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] FIG1 is a flow chart of a method for preparing a high-performance cathode material according to an embodiment of the present invention;
[0036] FIG2 is a cycle curve diagram of a battery assembled with the high-performance positive electrode material prepared in Example 1 of the present invention and a battery assembled with the positive electrode material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0037] The present invention is described in detail below through the accompanying drawings and specific embodiments, but it should be understood that these embodiments are only used for more detailed explanation and should not be understood as limiting the present invention in any form, that is, they are not intended to limit the scope of protection of the present invention.
[0038] An embodiment of the present invention provides a high-performance positive electrode material, comprising: a porous material, a lithium-containing compound, metal element nanoparticles, and a positive electrode active material.
[0039] The lithium-containing compound includes: inorganic lithium source materials and / or organic lithium source materials; wherein the inorganic lithium source materials include: one or more of lithium carbonate, lithium oxide, lithium phosphate, lithium manganate, lithium hydroxide or lithium iodide; the organic lithium source materials include: one or more of butyl lithium, phenyl lithium, cyclopentadiene dilithium, lithium acetate. The particle size D of the lithium-containing compound 50Between 0.5nm-10μm.
[0040] Metal element nanoparticles include: one or more elements and / or alloys of Al, Ti, Mn, Co, Ni, Cu, Zn, Zr, Mo, Ge, Sn; particle size D V100 ≤500nm.
[0041] During the first charge and discharge cycle of a lithium battery, the reactive sites on the metal surface of the metal nanoparticles adsorb inert lithium-containing compounds, causing the chemical bonds in the lithium-containing materials to deform or break, catalyzing the lithium-containing compounds and promoting the decomposition of lithium ions from the lithium-containing compounds, thereby improving the first cycle efficiency of the lithium battery.
[0042] The porous material includes one or more of porous carbon, graphene microspheres, single-walled carbon nanotubes and multi-walled carbon nanotubes; the average particle size D V50 The pore size is between 100nm-100μm, the pore size distribution is between 1nm-500nm, and the porosity distribution is between 30%-95%.
[0043] The positive electrode active material includes: one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide; the particle size DV50 of the positive electrode active material is between 5-20 μm.
[0044] Among the above materials, the total mass of the porous material, lithium-containing compound, and metal element nanoparticles accounts for 0.1%-20% of the total mass of the positive electrode material; the mass of the positive electrode active material accounts for 80%-99.9% of the total mass of the positive electrode material.
[0045] Preferably, the total mass of the porous material, the lithium-containing compound, and the metal element nanoparticles accounts for 6%-30% of the total mass of the positive electrode material; the mass of the positive electrode active material accounts for 70%-94% of the total mass of the positive electrode material;
[0046] Among them, in the preferred embodiment, the porous material accounts for 0.5%-15% of the total mass of the positive electrode material; the metal element nanoparticles account for 0.5%-10% of the total mass of the positive electrode material; and the lithium element compound accounts for 5%-20% of the total mass of the positive electrode material.
[0047] More preferably, the porous material accounts for 0.5%-15% of the total mass of the positive electrode material; the metal element nanoparticles account for 2%-8% of the total mass of the positive electrode material; and the lithium element-containing compound accounts for 7%-15% of the total mass of the positive electrode material.
[0048] During the first charge-discharge cycle of a lithium battery, the metal elements and / or alloys can catalyze lithium-containing compounds, promoting the decomposition of lithium ions from these compounds and thus improving the battery's initial cycle efficiency. This is because the metal elements and / or alloys employed in the present invention are transition metal elements. Except for Cu, the outermost d electron layer of each metal element is not fully filled, i.e., it contains d holes. For Cu, during the charge-discharge cycle, since its adjacent s orbital is not fully filled, d electrons will jump to the s orbital, forming d holes. Active sites on the surfaces of transition metal elements are typically associated with d orbitals and d holes that are densely populated with d electrons. These d orbitals and d holes can form coordination bonds with groups in the molecule, thereby promoting reactions and providing a strong catalytic effect. The d% value is commonly used to indicate the proportion of d electrons in a transition metal atom in a compound or material, and it significantly influences the reactivity and adsorption capacity of the metal surface. This is because the reactivity of a metal surface is closely related to its electronic structure. On the one hand, on the metal surface, d electrons tend to participate in chemical reactions more easily because they are closer to the metal surface than other electrons and are more easily affected by external substances. Therefore, the more d electrons there are on the metal surface, the stronger the reaction activity of the metal surface tends to be. On the other hand, d electrons may also affect chemical adsorption on the metal surface. The d holes on the surface of transition metals can make molecules on the surface more easily adsorbed because they can form coordination bonds with the d holes. Therefore, the number of d holes may also affect the adsorption capacity of molecules on the metal surface. Therefore, during the first charge and discharge process, the surface of the metal element has active sites to catalyze the release of lithium ions in the lithium-containing compound.
[0049] Under the first cycle of charge and discharge voltage, the reaction active sites on the metal surface can adsorb lithium-containing compounds that are inert in themselves, causing the deformation or breaking of chemical bonds in the lithium-containing compounds, and accelerating the charge transfer between the catalyst (metal) and the adsorbent (lithium-containing compound). Moreover, due to the large specific surface area of the nanoparticles, they have a large number of active centers for electrocatalytic reactions, which can greatly improve the catalytic effect, thereby activating the lithium-containing compounds and completely dissociating active lithium ions.
[0050] The high-performance positive electrode material of the above embodiment of the present invention can be prepared by the liquid phase method as shown in FIG1 .
[0051] Step 110, uniformly dispersing the metal element nanoparticles and the lithium element-containing compound in an organic solvent to obtain a premixed solution;
[0052] In this step, the organic solvent includes one or more of toluene, isopropyl alcohol, anhydrous ethanol, dimethylformamide, acetone, ethylene glycol dimethyl ether or tetrahydrofuran.
[0053] Step 120, adding the porous material to the premixed solution and fully and evenly dispersing it for 2-10 hours to obtain a mixed solution;
[0054] Step 130 , placing the mixed solution in a high-temperature furnace, heating it to 600° C.-1000° C. in an inert atmosphere, and keeping the temperature for 2 hours-10 hours. After discharging, the mixed solution is crushed and sieved to obtain a precursor material.
[0055] The heating furnace includes one or more of a box-type heating furnace, a tubular heating furnace, and a rotary furnace.
[0056] Step 140 , placing the precursor material and the positive electrode active material in a mixing device and mixing them for 0.5 hours to 5 hours. After the mixture is evenly mixed, a high-performance positive electrode material is obtained.
[0057] The mixing equipment includes one or more of a stirrer, a disperser, a ball mill, and an ultrasonic machine.
[0058] The high-performance positive electrode material of the embodiment of the present invention can be used in a positive electrode plate as a positive electrode active material, and the positive electrode plate can be used in a lithium battery.
[0059] In order to better understand the technical solution provided by the present invention, the preparation process and characteristics of the high-performance positive electrode material of the present invention are respectively described below with multiple specific examples.
[0060] Example 1
[0061] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0062] 1) 20 g of metallic copper powder and 50 g of lithium carbonate were placed in anhydrous ethanol solution and dispersed in a disperser at a speed of 1500 r / min. The mixture was stirred and dispersed for 8 hours at room temperature to obtain a premixed solution, wherein the metallic copper powder had a D V100 It is 205nm.
[0063] 2) 15 g of porous carbon was added to the premixed solution, and the mixture was uniformly dispersed in a disperser at a speed of 2000 rpm. Stirring was continued at room temperature for 8 hours to obtain a mixed solution.
[0064] 3) placing the mixed solution in a box-type heating furnace, heating it to 800° C. in an argon atmosphere, and keeping it warm for 6 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0065] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in a disperser at a speed of 1300 r / min and stirred at room temperature for 3 hours to obtain a high-performance positive electrode material.
[0066] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing:
[0067] Preparation and testing of coin-type half-cells: The high-performance cathode material, conductive additive carbon black, and binder polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 96%:2%:2%. A slurry was prepared using a blender. The slurry was then coated, dried, and cut into sheets. The cells were then assembled with lithium sheets in a glove box. Constant current charge and discharge testing was performed using a charge-discharge instrument, with a discharge cut-off voltage of 2.5V and a charge cut-off voltage of 3.65V. The first week of charge and discharge testing was conducted at a current density of 0.1C. The initial efficiency and reversible capacity test data for the coin-type cells are shown in Table 1.
[0068] Preparation and testing of full batteries:
[0069] Preparation of negative electrode sheets: A silicon oxide negative electrode material containing a carbon coating layer is configured with graphite to form a composite with a specific capacity of 450 mAg / h, and the conductive additive carbon black and the adhesive polyvinylidene fluoride (PVDF) are weighed and mixed in a ratio of 95%:2%:3%; at room temperature, the mixed material and solvent are placed in a beater to prepare a slurry; the prepared slurry is evenly coated on a copper foil at a coating speed between 2.2 m / min and 3.5 m / min, and the coating machine baking track temperature is between 70-100°C. After double-sided drying by the coater, the negative electrode sheet is obtained.
[0070] Preparation of positive electrode sheets: High-performance positive electrode materials, conductive additives and binders are weighed and mixed in a ratio of 96%:2%:2%; at room temperature, the mixed materials and solvent N-methylpyrrolidone are placed in a beater to prepare a slurry; the prepared slurry is evenly coated on aluminum foil at a coating speed between 2.0m / min-3.0m / min and a coating machine baking track temperature between 90-120°C; after double-sided coating and drying by the coater, the positive electrode sheet is obtained.
[0071] Preparation of the battery: Use aluminum tabs as exposed tabs for the positive electrode of the positive electrode sheet, and use copper-plated nickel tabs as exposed tabs for the negative electrode of the negative electrode sheet. The prepared positive and negative electrode sheets and separators are wound into naked battery cells, and then the battery cells are encapsulated with aluminum-plastic film through a heat sealing process. High-temperature vacuum baking is performed to remove moisture in the battery, and then 1 mole of electrolyte is injected. The electrolyte is a mixed solution of LiPF6 and ethylene carbonate / dimethyl carbonate (EC / DMC) to make a battery cell. After vacuum sealing, a full battery is prepared.
[0072] Test: The prepared full battery was tested in constant current charge and discharge mode using a charge and discharge instrument. The discharge cut-off voltage was 2.5V and the charge cut-off voltage was 3.65V. The discharge tests after the first week were all performed at a current density of 1C.
[0073] The test results of the initial efficiency, 0.1C reversible capacity and cycle retention rate of 300 and 600 cycles at 1C rate of the full battery prepared in this example are detailed in Table 1.
[0074] Example 2
[0075] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0076] 1) 13 g of aluminum powder and 68 g of lithium oxide were placed in an isopropyl alcohol solution and placed in a ball mill. The speed was set to 1000 r / min, and the ball mill was rotated forward and reversed at room temperature for 10 hours to obtain a premixed solution. The D of the aluminum powder was V100 It is 228nm.
[0077] 2) 24 g of single-walled carbon nanotubes were added to the premixed solution, and the mixture was uniformly dispersed in a ball mill at a speed of 1600 rpm and stirred at room temperature for 8 hours to obtain a mixed solution.
[0078] 3) placing the mixed solution in a rotary furnace, heating it to 700° C. in an argon atmosphere, and keeping the temperature for 8 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0079] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in a ball mill at a rotation speed of 800 r / min and stirred at room temperature for 2.5 hours to obtain a high-performance positive electrode material.
[0080] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0081] Example 3
[0082] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0083] 1) 37 g of metallic zinc powder and 137 g of lithium phosphate were placed in a toluene solution, placed in an ultrasonic machine, and ultrasonically stirred at a frequency of 50 kHz for 9 hours to obtain a premixed solution, wherein the D of the metallic zinc powder was V100 It is 138nm.
[0084] 2) 56 g of multi-walled carbon nanotubes were added to the premixed solution, and the mixture was stirred in an ultrasonic machine with the ultrasonic frequency set to 70 kHz for 3 hours to obtain a mixed solution.
[0085] 3) placing the mixed solution in a rotary kiln, heating it to 900° C. in an argon atmosphere, and keeping it warm for 3 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0086] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in an ultrasonic machine at a frequency of 70 kHz and stirred at room temperature for 2 hours to obtain a high-performance positive electrode material.
[0087] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0088] Example 4
[0089] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0090] 1) 42 g of metal molybdenum powder and 245 g of lithium manganate were placed in a solution of ethylene glycol dimethyl ether, placed in a ball mill, set the speed to 2000 r / min, forward and reverse, and ball milled at room temperature for 5 hours to obtain a premixed solution, wherein the D of the metal molybdenum powder was V100 It is 286nm.
[0091] 2) 38 g of graphene microspheres were added to the premixed solution, and the mixture was uniformly dispersed in a ball mill at a speed of 1300 rpm and stirred at room temperature for 10 hours to obtain a mixed solution.
[0092] 3) placing the mixed solution in a rotary kiln, heating it to 750° C. in an argon atmosphere, and keeping it warm for 5 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0093] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in a ball mill at a rotation speed of 600 r / min and stirred at room temperature for 4 hours to obtain a high-performance positive electrode material.
[0094] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0095] Example 5
[0096] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0097] 1) 60 g of aluminum-nickel alloy powder and 210 g of lithium hydroxide were placed in a tetrahydrofuran solution and dispersed in a disperser at a speed of 1100 r / min. The mixture was stirred and dispersed at room temperature for 3.5 hours to obtain a premixed solution. V100 It is 85nm.
[0098] 2) 50 g of single-walled carbon nanotubes were added to the premixed solution, and the mixture was uniformly dispersed in a disperser at a speed of 1390 r / min. Stirring was continued at room temperature for 7 hours to obtain a mixed solution.
[0099] 3) placing the mixed solution in a tubular heating furnace, heating it to 860° C. in an argon atmosphere, and keeping the temperature for 3.5 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0100] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in a disperser at a speed of 900 r / min and stirred at room temperature for 0.5 hours to obtain a high-performance positive electrode material.
[0101] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0102] Example 6
[0103] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0104] 1) 37g of metallic tin powder and 359g of butyl lithium were placed in dimethylformamide solution, placed in an ultrasonic machine, and ultrasonically stirred for 5 hours at an ultrasonic frequency of 40KHz to obtain a premixed solution, wherein the D of the metallic tin powder was V100 It is 53nm.
[0105] 2) Add 206 g of porous carbon to the premixed solution, continue stirring in an ultrasonic machine with the ultrasonic frequency set to 80 kHz, and stir for 10 hours to obtain a mixed solution.
[0106] 3) placing the mixed solution in a rotary furnace, heating it to 1000° C. in an argon atmosphere, and keeping it warm for 2 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0107] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in an ultrasonic machine at a frequency of 40 kHz and stirred at room temperature for 4 hours to obtain a high-performance positive electrode material.
[0108] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0109] Example 7
[0110] This embodiment provides a preparation process and performance test of a high-performance positive electrode material. The specific preparation process is as follows:
[0111] 1) 40 g of copper-tin alloy powder and 457 g of lithium acetate were placed in a solution of ethylene glycol dimethyl ether and dispersed in a disperser at a speed of 1400 r / min. The mixture was stirred and dispersed for 2 hours at room temperature to obtain a premixed solution, wherein the D of the aluminum-nickel alloy powder was 0.05. V100 It is 39nm.
[0112] 2) 170 g of graphene microspheres were added to the premixed solution, and the mixture was uniformly dispersed in a disperser at a speed of 2000 rpm and stirred at room temperature for 2 hours to obtain a mixed solution.
[0113] 3) placing the mixed solution in a tubular heating furnace, heating it to 950° C. in an argon atmosphere, and keeping it warm for 4.5 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0114] 4) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in a disperser at a speed of 700 r / min and stirred at room temperature for 5 hours to obtain a high-performance positive electrode material.
[0115] The high-performance positive electrode material prepared in this example was used to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0116] Comparative Example 1
[0117] In this comparative example, lithium iron phosphate, the same positive electrode material as in the example, was used as the positive electrode material to prepare positive electrode sheets, and button-type half-cells and full-cells were assembled for testing. The specific process was the same as in Example 1. The test data is detailed in Table 1.
[0118] Comparative Example 2
[0119] This comparative example provides a preparation process and performance test of a positive electrode material that is not doped with metal elements but does contain lithium. The specific preparation process is as follows:
[0120] 1) 210 g of lithium hydroxide was placed in a tetrahydrofuran solution and dispersed in a disperser at a speed of 1100 rpm. The mixture was stirred and dispersed at room temperature for 3.5 hours to obtain a premixed solution.
[0121] 2) 50 g of single-walled carbon nanotubes were added to the premixed solution, and the mixture was uniformly dispersed in a disperser at a speed of 1390 r / min. Stirring was continued at room temperature for 7 hours to obtain a mixed solution.
[0122] 4) placing the mixed solution in a tubular heating furnace, heating it to 860° C. in an argon atmosphere, and keeping the temperature for 3.5 hours. After discharging, the material is crushed and sieved to obtain a precursor material;
[0123] 3) 2 kg of lithium iron phosphate and the precursor material were further uniformly dispersed in a disperser at a speed of 900 r / min and stirred at room temperature for 0.5 hours to obtain a positive electrode material without doping with metal elements but with added lithium elements.
[0124] Positive electrode sheets were prepared using the lithium-doped, metal-free cathode material prepared in this comparative example. Coin-type half-cells and full cells were then assembled for testing, following the same procedures as in Example 1. The test data are detailed in Table 1. Cycling curves for a battery assembled with the high-performance cathode material prepared in Example 1 and a battery assembled with the cathode material prepared in Comparative Example 2 are shown in Figure 2.
[0125] The positive electrode materials in Examples 1-7 and Comparative Examples 1-2 were tested for initial efficiency and reversible capacity after charging, and cycle retention rates after 300 and 600 cycles of full charging, respectively. The results are shown in Table 1.
[0126] Table 1
[0127] From the comparison of the test data in Table 1, it can be seen that under the same test conditions, the first-week charging specific capacity and cycle retention rate of the positive electrode materials prepared in Examples 1-7 are much higher than those of the positive electrode materials in Comparative Examples 1-2. This is because Examples 1-7 use porous materials as skeletons, and metal elements and lithium elements are distributed in the pores of the porous skeleton materials. The doped nano-metal elements catalyze the complete decomposition of lithium ions from the inactive lithium-containing compounds at room temperature during the charging process, thereby increasing the lithium decomposition capacity of the positive electrode material and improving the energy density of the battery. At the same time, the gas generated by the lithium-containing compounds that are completely catalytically decomposed will also be discharged during the battery formation process, avoiding the gas production problem caused by the continuous decomposition of the lithium-containing compounds during normal use of the battery, thereby improving the safety performance of the battery. In addition, the doped metal elements and porous materials can accelerate the internal conduction rate of lithium ions, improve the conductivity of the positive electrode material, and ultimately achieve the purpose of using a safe, low-cost, and simple process to improve the overall battery capacity and cycle life.
[0128] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A high-performance cathode material, characterized in that: The positive electrode material is used in a lithium battery, and the positive electrode material comprises: a porous material, a lithium-containing compound, metal element nanoparticles and a positive electrode active material; The lithium-containing compound includes: an inorganic lithium source material and / or an organic lithium source material; the inorganic lithium source material includes: one or more of lithium carbonate, lithium oxide, lithium phosphate, lithium manganate, lithium hydroxide or lithium iodide; the organic lithium source material includes: one or more of butyl lithium, phenyl lithium, cyclopentadiene dilithium, and lithium acetate; The metal element nanoparticles include: one or more single substances and / or alloys of Al, Ti, Mn, Co, Ni, Cu, Zn, Zr, Mo, Ge, Sn; the particle size D V100 ≤500nm; During the first charge and discharge cycle of the lithium battery, the reaction active sites on the metal surface of the metal element nanoparticles adsorb inert lithium-containing compounds, causing the chemical bonds in the lithium-containing materials to deform or break, thereby catalyzing the lithium-containing compounds. The active centers of the electrocatalytic reaction provided by the specific surface area of the metal element nanoparticles enhance the catalytic effect, jointly promoting the complete decomposition of lithium-containing compounds into lithium ions, thereby improving the energy density and safety performance of the lithium battery.
2. The high performance cathode material according to claim 1, characterized in that: The average particle size D of the porous material V50 The pore size is between 100nm-100μm, the pore size distribution is between 1nm-500nm, and the porosity distribution is between 30%-95%; The particle size D of the lithium-containing compound 50 Between 0.5nm-10μm; The particle size D of the positive electrode active material V50 Between 5-20μm.
3. The high performance cathode material according to claim 1, characterized in that: The porous material includes: one or more of porous carbon, graphene microspheres, single-walled carbon nanotubes and multi-walled carbon nanotubes; The positive electrode active material includes: one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide.
4. The high performance cathode material according to claim 1, characterized in that: The mass of the positive electrode active material accounts for 80%-99.9% of the total mass of the positive electrode material; The total mass of the porous material, the lithium-containing compound and the metal element nanoparticles accounts for 0.1%-20% of the total mass of the positive electrode material.
5. The high performance cathode material according to claim 4, characterized in that: The mass of the positive electrode active material accounts for 70%-94% of the total mass of the positive electrode material; The total mass of the porous material, the lithium-containing compound, and the metal element nanoparticles accounts for 6% to 30% of the total mass of the positive electrode material; The porous material accounts for 0.5%-15% of the total mass of the positive electrode material; the metal element nanoparticles account for 0.5%-10% of the total mass of the positive electrode material; and the lithium-containing compound accounts for 5%-20% of the total mass of the positive electrode material.
6. A method for preparing a high-performance cathode material according to any one of claims 1 to 5, characterized in that: The preparation method is a liquid phase method: uniformly dispersing metal element nanoparticles and lithium element-containing compounds in an organic solvent to obtain a premixed solution; Adding the porous material to the premixed solution and fully and evenly dispersing it for 2-10 hours to obtain a mixed solution; The mixed solution is placed in a high-temperature furnace, heated to 600° C.-1000° C. in an inert atmosphere, and kept warm for 2 hours-10 hours. After the material is discharged, it is crushed and sieved to obtain a precursor material; The precursor material and the positive electrode active material are placed in a mixing device and mixed for 0.5 hour to 5 hours. After the mixture is evenly mixed, a high-performance positive electrode material is obtained.
7. The preparation method according to claim 6, characterized in that: The organic solvent includes one or more of toluene, isopropanol, anhydrous ethanol, dimethylformamide, acetone, ethylene glycol dimethyl ether or tetrahydrofuran.
8. The preparation method according to claim 6, characterized in that: The mixing equipment includes one or more of a stirrer, a disperser, a ball mill, and an ultrasonic machine; The heating furnace includes: one or more of a box-type heating furnace, a tubular heating furnace, and a rotary furnace.
9. A positive electrode sheet, characterized in that: The positive electrode plate comprises the high-performance positive electrode material described in any one of claims 1 to 5.
10. A lithium battery, characterized in that: The lithium battery comprises the positive electrode sheet as described in claim 9 above.
Citation Information
Patent Citations
Method for preparing presoma of active electrode material of nano-lithium ion battery and application thereof
CN102082264A
Nanometer composite material and preparation method thereof, positive electrode material and battery
CN103137976A
Porous carbon material for lithium air cell, preparation and application thereof
CN104518225A
Graphene combined multilayered perforated spheroidic lithium manganese oxide electrode material and lithium ion battery prepared therefrom
CN107331853A
Nanometer transition metal-nanometer lithium oxide-porous carbon composite material, fabrication method of lithium ion capacitor and lithium ion capacitor
CN107799321A
Cited By
Silicon-oxygen negative electrode pre-lithiation method based on lithium locene solution and application
CN121709548A
Silicon-oxygen negative electrode prelithiation method based on lithium metallocene solution and application
CN121709548B