Perovskite compound and method for producing same
The method addresses the challenge of achieving uniform particle sizes in barium calcium titanate by adjusting the molar ratio and treatment processes, resulting in high-performance dielectric materials for multilayer ceramic capacitors with improved uniformity and electronic properties.
Patent Information
- Application Number
- PCT/JP2024/015916
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
Current methods for producing barium calcium titanate struggle to achieve uniform particle sizes and low CV values, which are essential for high-performance dielectric materials in multilayer ceramic capacitors.
A method involving the preparation of a barium titanate dispersion with a specific molar ratio of barium to titanium, followed by a barium removal treatment, and subsequent heat treatment with calcium or strontium salts to produce barium calcium titanate with improved particle uniformity and dispersibility.
The method results in barium calcium titanate with a CV value of 20% or less, suitable for forming uniform dielectric layers with enhanced electronic properties and improved sheet smoothness, suitable for advanced ceramic capacitor applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000027_0000
Abstract
Description
Perovskite-type compound and method for producing same
[0001] The present invention relates to a perovskite compound and a method for producing the same.
[0002] Barium calcium titanate is a dielectric material that has attracted attention as an electronic material that improves the temperature dependence and reliability of barium titanate's dielectric properties by partially substituting the barium sites of barium titanate with calcium, and is used in multilayer ceramic capacitors. In recent years, multilayer ceramic capacitors have become thinner, and sheet-forming dielectric materials have become increasingly important. Accordingly, dielectric materials used as raw materials are increasingly required to have a higher level of particle size uniformity than before. The CV value (standard deviation of particle size / average particle size) is known as a parameter that indicates particle size uniformity. Since most barium calcium titanate is produced through high-temperature heat treatment processes, it is currently difficult to obtain barium calcium titanate with a uniform particle size. Previously reported barium calcium titanate with average particle sizes of 620 nm and 252 nm has been reported (see Patent Documents 1 and 2), with CV values of 22% and 21%, respectively. Furthermore, BET specific surface areas of 11 to 60 m 2 / g of barium calcium titanate has been reported (see Patent Document 3).
[0003] Patent No. 4256117 Patent No. 4525788 Patent No. 6954501
[0004] As mentioned above, barium calcium titanate having an average particle size of 620 nm or 252 nm that has been reported so far does not have a sufficiently low CV value, and the BET specific surface area is 11 to 60 m 2 There is also room for improvement in barium calcium titanate with a CV value of 1 / g to be further reduced.
[0005] In view of the above-mentioned current situation, an object of the present invention is to provide barium calcium titanate having a high uniformity of particle size.
[0006] The inventors have investigated methods for obtaining barium calcium titanate with highly uniform particle size. They have found that a barium titanate dispersion prepared from a barium compound and an aqueous titanium compound solution is washed with water to reduce the molar ratio of barium to titanium to less than 1.00, and then mixed with a calcium salt. The resulting barium titanate is then heat-treated and deagglomerated in a solvent. In this method, barium and titanium sources are used to obtain the barium titanate dispersion, and the barium titanate concentration in the barium titanate dispersion before debarium ionization is adjusted to a predetermined value or higher. The resulting barium calcium titanate particles have a sufficiently low CV value and excellent dispersibility and sheet smoothness. This manufacturing method can also be applied to the production of barium strontium titanate. Note that barium titanate dispersions are sometimes referred to as barium titanate slurries.
[0007] That is, the present invention is as follows: [1] A compound represented by the following general formula (1): Ba (1-x) A x TiO 3 (1) A perovskite compound, represented by the formula (wherein A represents Ca or Sr, and x is a number satisfying 0.00<x≦0.30), characterized in that the CV value, which is expressed as the ratio of the standard deviation of particle diameter to the average particle diameter (equivalent circle diameter) obtained by observation with a scanning electron microscope (standard deviation of particle diameter / average particle diameter×100), is 20% or less.
[0008] [2] BET specific surface area is 5 to 70 m 2 The perovskite compound according to [1], wherein the SiO 2 content is 1 / g.
[0009] [3] A method for producing a perovskite compound, comprising: a barium titanate dispersion preparation step of mixing a barium compound with an aqueous titanium compound solution to obtain a barium titanate dispersion; a barium ion depletion step of washing the barium titanate dispersion obtained in the barium titanate dispersion preparation step to obtain barium titanate having a molar ratio of barium element to titanium element of less than 1.00; a heat treatment step of mixing the barium titanate obtained in the barium ion depletion step with a calcium salt or a strontium salt and heat treating the mixture; and a disintegration step of heating the compound obtained in the heat treatment step in a solvent to disintegrate the particles, wherein in the barium titanate dispersion preparation step, the barium compound and the aqueous titanium compound solution are used so that the molar ratio (Ba / Ti) of the barium element in the barium compound to the titanium element in the aqueous titanium compound solution is 4.5 or more, or the barium titanate concentration in the barium titanate dispersion used in the barium ion depletion step is 65 g / L or more.
[0010] The method for producing a perovskite compound of the present invention is a method capable of producing barium calcium titanate having a highly uniform particle size, and the barium calcium titanate obtained by this production method can be suitably used as a raw material for multilayer ceramic capacitors, etc.
[0011] 1 is a SEM photograph of a barium titanate precursor slurry having a concentration of 80 g / L obtained in the barium ion debarization treatment step of Example 1. 2 is a SEM photograph of barium calcium titanate obtained in Example 1. 3 is a SEM photograph of a barium titanate precursor slurry having a concentration of 60 g / L obtained in the barium ion debarization treatment step of Comparative Example 1. 4 is a SEM photograph of barium calcium titanate obtained in Comparative Example 1. 5 is a HAADF-STEM photograph of the barium calcium titanate obtained in Example 1. 6 is a HAADF-STEM photograph of the barium calcium titanate obtained in Example 1 (Ba: white, Ti: gray). 7 is an EDS mapping of the barium calcium titanate obtained in Example 1, performed in the same field of view as in FIG. 4 (Ba: only white is shown). 8 is an EDS mapping of the barium calcium titanate obtained in Example 1, performed in the same field of view as in FIG. 4 (Ca: only white is shown). 9 is an XRD measurement result of the barium calcium titanate obtained in Example 7.
[0012] Preferred embodiments of the present invention will be specifically described below, but the present invention is not limited to the following description and can be appropriately modified and applied within the scope that does not change the gist of the present invention.
[0013] 1. Perovskite Compound The perovskite compound of the present invention is represented by the following general formula (1): Ba (1-x) A x TiO 3(1) (wherein A represents Ca or Sr, and x is a number satisfying the condition 0.00<x≦0.30), and is characterized in that the CV value, expressed as the ratio of the standard deviation of particle diameter to the average particle diameter (circle-equivalent diameter) obtained by observation with a scanning electron microscope (standard deviation of particle diameter / average particle diameter × 100), is 20% or less. The use of such a perovskite compound with high particle size uniformity allows for the formation of a dielectric layer with uniform dielectric properties, making it suitable as a material for the dielectric layer of a ceramic capacitor. Furthermore, the perovskite compound of the present invention with high particle size uniformity is characterized by its high dispersibility in solvents and resins, making it suitable as a material for forming the dielectric layer of a ceramic capacitor by mixing it with a resin or the like. The CV value of the perovskite compound of the present invention may be 20% or less, but is preferably 19% or less. It is more preferably 18.5% or less, even more preferably 18% or less, particularly preferably 17.5% or less, especially preferably 17% or less, and most preferably 16% or less. The CV value of the perovskite compound can be measured by the method described in the examples below.
[0014] The perovskite compound of the present invention has a BET specific surface area of 5 to 70 m 2 / g. Particles with a small particle size and such a BET specific surface area are more suitable for electronic material applications such as multilayer ceramic capacitors. Furthermore, a small BET specific surface area is preferable in order to reduce re-aggregated components in the dispersion step and facilitate dispersion. The BET specific surface area of the perovskite compound is more preferably 8 to 35 m. 2 / g, and more preferably 10 to 30 m 2 / g, and most preferably 15 to 25m 2 The BET specific surface area of the perovskite compound can be measured by the method described in the examples below.
[0015] The perovskite compound of the present invention preferably has an average particle size of 10 to 210 nm. With such an average particle size, dispersion and handling are easy when forming a dielectric layer, and a uniform dielectric layer can be formed. The average particle size is more preferably 20 to 160 nm, even more preferably 30 to 150 nm, particularly preferably 35 to 130 nm, particularly preferably 40 to 100 nm, and most preferably 45 to 60 nm. The average particle size of the perovskite compound can be measured by the method described in the Examples below.
[0016] The perovskite compound of the present invention preferably has a particle circularity of 0.85 or more. With such a circularity, it is easy to produce a smooth dielectric layer. The circularity is more preferably 0.90 or more, and even more preferably 0.95 or more. The circularity of the perovskite compound particles can be measured by the method described in the examples below.
[0017] When a film equivalent to a green sheet is produced using particles produced according to the present invention and the surface smoothness of the film is evaluated, the arithmetic mean roughness (Ra) of the surface is preferably 0.110 μm or less. More preferably, it is 0.095 μm or less, even more preferably, it is 0.080 μm or less, and particularly preferably, it is 0.070 μm or less. Furthermore, the maximum height (Rz) is preferably 1.400 μm or less. More preferably, it is 1.200 μm or less, even more preferably, it is 0.085 μm or less, and particularly preferably, it is 0.080 μm or less. With such arithmetic mean roughness and maximum height, it is easy to produce a smooth surface. The method for producing a film equivalent to a green sheet using particles of a perovskite compound, and the arithmetic mean roughness and maximum height of the produced film are as described in the examples below. Thus, when a film equivalent to a green sheet is produced using the particles of the present invention, a very smooth surface can be obtained.
[0018] The perovskite-type compound represented by the general formula (1) may be either a compound where x is 0.00<x≦0.30, where x is 0.00<x≦0.15 and where the amount of solid solution of calcium or strontium is small, or a compound where x is 0.15<x≦0.30 and where the amount of solid solution of calcium or strontium is large. However, x is preferably 0.005≦x≦0.05. More preferably, x is 0.01≦x≦0.03. Perovskite-type compounds where x is 0.00<x≦0.15 and where the amount of solid solution of calcium or strontium is small are considered to be suitable for consumer capacitors (smartphones, tablets, etc.) that require a balance between small size, high capacitance, and improved reliability, such as maintaining high ferroelectricity while providing excellent temperature characteristics and reliability. Furthermore, perovskite compounds with a large amount of calcium or strontium dissolved therein, where x is a number in the range of 0.15<x≦0.30, are thought to have further improved temperature characteristics due to the increased amount of dissolved calcium or strontium, and are therefore considered suitable for automotive capacitors, which require heat resistance at higher temperatures.
[0019] 2. Method for Producing Perovskite Compound The method for producing a perovskite compound of the present invention uses a production method including: a barium titanate dispersion preparation step of mixing a barium compound with an aqueous titanium compound solution to obtain a barium titanate dispersion; a barium ion debarization treatment step of washing the barium titanate dispersion obtained in the barium titanate dispersion preparation step to obtain barium titanate having a molar ratio of barium element to titanium element of less than 1.00; a heat treatment step of mixing the barium titanate obtained in the barium ion debarization treatment step with a calcium salt or a strontium salt and heat treating the mixture; and a disintegration step of heating the compound obtained in the heat treatment step in a solvent to disintegrate the compound. The method is characterized in that, in the barium titanate dispersion preparation step, a barium compound and a titanium compound aqueous solution are used so that the molar ratio (Ba / Ti) of the barium element in the barium compound to the titanium element in the titanium compound aqueous solution is 4.5 or higher (hereinafter also referred to as the first condition), or the barium titanate concentration in the barium titanate dispersion used in the barium ion debarium treatment step is 65 g / L or higher (hereinafter also referred to as the second condition). The barium titanate dispersion preparation step is a step of preparing a barium titanate dispersion that serves as a precursor to the target barium calcium titanate or barium strontium titanate. When the barium compound and titanium compound aqueous solution are used in the barium titanate dispersion preparation step so as to satisfy the first condition, the precursor barium titanate dispersion is prepared in a state in which a certain amount of barium ions are present in the system, thereby producing a barium titanate slurry with little aggregation. Furthermore, by using such a barium titanate slurry with little aggregation as a precursor and carrying out the barium ion debarking process and the deagglomeration process to produce barium calcium titanate or barium strontium titanate, it is possible to obtain barium calcium titanate or barium strontium titanate with a high degree of particle size uniformity. Furthermore, by satisfying the second condition, the second process is carried out so that a certain amount of barium ions are present in the dispersion, and in this way, it is also possible to obtain barium calcium titanate or barium strontium titanate with a high degree of particle size uniformity.
[0020] (1) Barium titanate dispersion preparation step In the method for producing a perovskite compound of the present invention, in order to satisfy the first condition, the molar ratio of barium to titanium (Ba / Ti) may be 4.5 or more, preferably 5 or more, and more preferably 6 or more. Furthermore, in consideration of the production cost of the perovskite compound, the molar ratio of barium to titanium (Ba / Ti) is preferably 10 or less.
[0021] When the method for producing a perovskite compound of the present invention is carried out so as to satisfy the second condition, in the barium titanate dispersion preparation step, the ratio of the moles of barium element in the barium compound to the moles of titanium element in the titanium compound aqueous solution may be less than 5, but considering the efficiency of preparation of barium titanate, it is preferable to use the titanium compound aqueous solution and the barium compound so that the ratio is 0.5 or more.
[0022] The barium compound used in the barium titanate dispersion preparation step is not particularly limited, but examples thereof include barium hydroxide, barium oxalate, barium acetate, barium nitrate, barium nitrite, barium chloride, barium chlorate, barium perchlorate, barium bromide, barium bromate, barium iodide, barium hydrogen phosphate, barium nitride, barium oxide, barium peroxide, barium sulfide, barium azide, barium fluoride, barium formate, barium lactate, barium metaphosphate, barium methacrylate, barium rhodizonate, barium tartrate, barium sulfate, barium sulfite, barium trifluoromethanesulfonate, bis(acetylacetonato)diaquabarium(II), barium benzoate, barium 2-ethylhexanoate, barium octanoate, barium oleate, and barium citrate. Examples of suitable cation exchangers include barium hydroxide, barium hydride, barium thiocyanate, barium metatitanate, barium aluminate, barium chromate, barium ferrate, barium naphthenate, barium propionate, barium dipropionate, barium hexaborate, barium laurate, barium malonate, barium thiosulfate, barium trifluoroacetate, barium trimethylacetate, barium malate, barium succinate, barium valerate, barium camphorate, barium picrate, barium caproate, barium gluconate, barium benzenesulfonate, barium salicylate, barium mandelate, barium cinnamate, barium stearate, barium palmitate, barium myristate, barium laurate, and barium sulfamate. One or more of these compounds may be used. Among these, compounds that render aqueous solutions of barium hydroxide and barium oxide basic are preferred. More preferred is barium hydroxide.
[0023] Examples of the titanium compound aqueous solution used in the barium titanate dispersion preparation step include aqueous solutions of titanium tetrachloride and water-soluble titanium complexes, and one or more of these can be used. The ligand of the water-soluble titanium complex preferably contains a hydroxy acid (salt). The hydroxy acid may be an α-hydroxy acid. Examples of α-hydroxy acids include glycolic acid, citric acid, malic acid, tartaric acid, and lactic acid. Titanium complexes containing an ammonium salt of lactic acid as a ligand may also be used. For example, titanium bis(ammonium lactate) dihydroxide (TALH) may be mentioned. Among these, aqueous solutions of titanium tetrachloride and TALH are preferred. An aqueous solution of titanium tetrachloride is more preferred.
[0024] When mixing with the titanium compound aqueous solution in the barium titanate dispersion preparation step, the barium compound may be mixed as a solid, but in order to produce a sufficient amount of barium titanate, it is preferable to mix it after making it into a solution. The solvent used to prepare the barium compound solution may be either an organic solvent or an inorganic solvent, but examples include water and water-miscible organic solvents such as methanol and ethanol, and one or more of these can be used. Among these, it is preferable to use water or a mixture of a water-miscible organic solvent and water.
[0025] In the barium titanate dispersion preparation step, the barium compound and the aqueous titanium compound solution may be mixed together in one go, in separate portions, or sequentially. Alternatively, both the barium compound and the aqueous titanium compound solution may be added to a container, or one may be added to the other.
[0026] The amount of solvent used in the barium titanate dispersion preparation step is not particularly limited, but is preferably an amount that results in a solids concentration of 10 to 1,000 g / L in the resulting barium titanate dispersion. More preferably, it is 10 to 500 g / L, even more preferably, 10 to 250 g / L, and most preferably, 10 to 100 g / L. If the solids concentration is too low, the productivity of the perovskite compound will decrease, while if the solids concentration is too high, there is a risk of non-uniformity in the washing process in the barium ion removal treatment step. The amount of solvent used here refers to the total amount of water contained in the aqueous titanium compound solution and the solvent contained in the barium compound solution when the barium compound is mixed in solution.
[0027] In the barium titanate dispersion preparation step, the pH of the mixed solution of the barium compound and the aqueous titanium compound solution is preferably adjusted to 5 or higher. By mixing in such an alkaline range, a sufficient amount of barium titanate can be produced. The pH of the mixed solution of the barium compound and the aqueous titanium compound solution is more preferably 8 or higher, and even more preferably 10 or higher.
[0028] (2) Barium Ion Removal Treatment Step In the method for producing a perovskite compound of the present invention, to satisfy the second condition, the barium titanate concentration in the barium titanate dispersion may be 65 g / L or more, preferably 80 g / L or more, and more preferably 110 g / L or more.
[0029] When the method for producing a perovskite compound of the present invention is carried out so as to satisfy the first condition, the barium titanate concentration in the barium titanate dispersion used in the barium ion removal treatment step may be less than 65 g / L, but considering the efficiency of producing the perovskite compound, it is preferable to make it 10 g / L or more.
[0030] In the barium ion removal treatment step, the barium titanate dispersion obtained in the barium titanate dispersion preparation step may be washed to make the molar ratio of barium element to titanium element less than 1.00. The molar ratio of barium element to titanium element can be confirmed by X-ray fluorescence analysis (XRF).
[0031] The barium titanate washing treatment performed in the barium ion removal treatment step can efficiently elute barium ions from the barium titanate. The washing treatment may be any treatment capable of achieving a molar ratio of barium to titanium of less than 1.00, but is preferably performed by adding an acid while stirring the barium titanate slurry. The barium ion removal treatment is preferably performed by an acid washing treatment using an inorganic acid such as hydrochloric acid, sulfuric acid, nitric acid, or phosphoric acid, or an organic acid such as acetic acid, oxalic acid, or citric acid. While water washing can be used to achieve a molar ratio of barium to titanium of less than 1.00, this is not practical due to the large amount of water required. Using an acid to elute barium ions is quantitative and suitable for industrial production.
[0032] The method of debarium ion treatment in the above-mentioned debarium ion treatment step is not particularly limited as long as it can make the molar ratio of barium element to titanium element in barium titanate less than 1.00, but it is preferable to add an acid to barium titanate and perform the treatment so that the pH of the obtained slurry is 5 to 11. Furthermore, it is preferable to perform the treatment by appropriately adjusting the pH of the slurry within the above-mentioned pH range depending on the specific surface area of the barium titanate to be debarium ion treated in the debarium ion treatment step and the amount of barium element substituted with calcium element or strontium element. For example, 2 When barium titanate having a molecular weight of 10000 / g is treated to remove barium ions at pH 7, the molar ratio of barium element is about 0.60 to 0.70, and when treated at pH 11, the molar ratio is about 0.75 to 0.90.
[0033] It is preferable to carry out a water washing step before subjecting the barium titanate after the barium ion removal treatment in the barium ion removal treatment step to a heat treatment step, which makes it possible to remove the acid and the eluted barium element from the barium titanate, and to produce a perovskite-type compound having a large amount of solid solution of calcium and strontium and a small amount of impurities.
[0034] Regarding the washing treatment in the barium ion removal treatment step, in consideration of sufficient elution of barium element and production efficiency, washing is preferably carried out until the electrical conductivity of the washing water becomes 100 μS / cm or less, more preferably 50 μS / cm or less.
[0035] (3) Heat Treatment Step The heat treatment step involves mixing the barium titanate obtained in the barium ion removal treatment step with a calcium salt or a strontium salt, followed by heat treatment. The calcium salt or strontium salt to be mixed with the barium titanate is not particularly limited, and examples thereof include oxides, hydroxides, chlorides, carbonates, sulfates, nitrates, phosphates, and organic acid salts such as hydroiodic acid, acetates, oxalates, and citric acid of calcium and strontium, and one or more of these may be used.
[0036] When a calcium salt is used in the heat treatment step, the amount of calcium salt used is preferably such that the amount of calcium contained in the calcium salt is greater than 0 mol% and not more than 30 mol% relative to 100 mol% of titanium element contained in barium titanate. By using such a ratio, calcium dissolves in barium titanate, and a highly pure product can be synthesized that does not contain any crystalline phase other than barium calcium titanate. The amount of calcium salt used is more preferably such that the amount of calcium contained in the calcium salt is 0.5 to 20 mol% relative to 100 mol% of titanium element contained in barium titanate, and even more preferably such that the amount of calcium is 1 to 10 mol%. When a strontium salt is used in the heat treatment step, it is also preferably used so that the amount of strontium contained in the strontium salt is the same as that described above relative to 100 mol% of titanium element contained in barium titanate.
[0037] In the heat treatment step, in addition to the calcium salt or strontium salt, a barium salt may be mixed with the barium titanate. By mixing the barium salt, the behavior of the perovskite compound during the heat treatment can be controlled, and the particle size can be controlled. The amount of barium salt used can be appropriately set depending on the desired particle size, etc.
[0038] In the heat treatment step, the method for mixing barium titanate with a calcium salt or a strontium salt is not particularly limited as long as they are sufficiently mixed, but for example, a method may be used in which a calcium salt or a strontium salt is added to a barium titanate slurry and then the slurry is stirred with a stirrer, etc. The same method is used for mixing a barium salt.
[0039] In the heat treatment step, the temperature at which the mixture of barium titanate and calcium salt or strontium salt is heat treated is preferably 400 to 1200°C. More preferably, it is 450 to 1000°C, even more preferably 500 to 800°C, and particularly preferably 550 to 700°C. The heat treatment time is preferably 0.5 to 12 hours, more preferably 1 to 10 hours, and even more preferably 2 to 8 hours. The atmosphere in which the heat treatment is performed is not particularly limited, and may be air or an inert gas atmosphere such as nitrogen or argon.
[0040] The number of heat treatments in the heat treatment step is not particularly limited and may be one or more. Preferably, the barium titanate obtained in the barium ion removal treatment step is mixed with a calcium salt or a strontium salt, heated and dried to obtain a dry mixture, and then calcined. Drying the mixture of barium titanate and a calcium salt or a strontium salt before calcination suppresses compositional segregation, resulting in a precursor with a uniform distribution of calcium and strontium elements. Calcining this precursor results in a uniform solid solution of calcium and strontium elements in the perovskite-type compound, improving particle uniformity. While the method for drying the mixture is not particularly limited, a method using a box dryer, fluidized-bed dryer, flash dryer, or spray dryer is preferred. Hereinafter, the heat treatment step of mixing the barium titanate obtained in the barium ion removal treatment step with a calcium salt or a strontium salt and heating and drying to obtain a dry mixture is referred to as the drying step, and the step of calcining the dry mixture is referred to as the calcination step.
[0041] When the heat treatment step includes a drying step and a calcination step of calcining the dried mixture, the temperature and time for calcining the dried mixture are preferably the same as those for the heat treatment step. The mixture is preferably dried at 80 to 300°C, more preferably 90 to 110°C. The time for drying the mixture is preferably 0.5 to 24 hours, more preferably 2 to 6 hours, if a box dryer is used.
[0042] (4) Deagglomeration Step The method for producing a perovskite compound of the present invention further includes a deagglomeration step in which the perovskite compound obtained in the heat treatment step is heated in a solvent to deagglomerate the compound. This allows for the production of a perovskite compound with minimal interparticle connectivity. The heating temperature when the perovskite compound is heated in a solvent to deagglomerate in the deagglomeration step is not particularly limited as long as the particles of the perovskite compound are deagglomerated, but is preferably 30 to 500°C. Heating the perovskite compound in a solvent to such a temperature allows for sufficient deagglomeration of the agglomerated particles of the perovskite compound, resulting in a perovskite compound with minimal interparticle connectivity and a high proportion of nearly spherical particles. The temperature at which the perovskite compound is heated is preferably 30 to 500°C, but more preferably 60 to 300°C in order to more thoroughly deagglomerate the agglomerated particles of the perovskite compound. The temperature is more preferably 100 to 200°C, and particularly preferably 100 to 180°C.
[0043] The heating time for the perovskite compound in the above-mentioned deagglomeration step is not particularly limited, but is preferably 1 to 120 hours from the viewpoint of sufficiently deagglomerating the agglomerated particles of the perovskite compound. It is more preferably 2 to 72 hours, even more preferably 4 to 60 hours, and particularly preferably 10 to 40 hours. Depending on the desired properties, the heating time may be 10 to 30 hours in consideration of production efficiency. The heating atmosphere is not particularly limited, and may be air or an inert gas atmosphere such as nitrogen or argon.
[0044] The solvent used when heating the perovskite compound in the disintegration step may be either an organic solvent or an inorganic solvent, but examples thereof include water and water-miscible organic solvents such as methanol and ethanol, and one or more of these can be used. Among these, it is preferable to use water or a mixture of a water-miscible organic solvent and water.
[0045] The above-mentioned deagglomeration step may be carried out by adding an acid or a base, or a substance that acts as an acid or a base in the solvent, to the solvent. Adding these to the solvent allows for more efficient deagglomeration of the agglomerated particles. Examples of the acid include the same acids used in the debarium ion treatment in the above-mentioned debarium ion treatment step. Examples of the base include inorganic bases such as hydroxides of alkali metals or alkaline earth metals, such as lithium hydroxide, sodium hydroxide, potassium hydroxide, and barium hydroxide, and organic bases such as organic amines. Among these, barium hydroxide is preferably used because of its high effect of deagglomerating agglomerated particles of the perovskite compound. The acid or base, or the substance that acts as an acid or a base in the solvent, may each be used alone or in combination of two or more.
[0046] (5) Other Steps The method for producing a perovskite compound of the present invention may include other steps in addition to those described above. These other steps include dispersing or washing the perovskite compound obtained in the heat treatment or deagglomeration step, and drying the washed perovskite compound. The dispersion method used in the perovskite compound dispersion step is not particularly limited, but examples include a method using a media-based disperser such as a bead mill, or a media-less disperser such as an emulsifier or ultrasonic disperser. The washing method used in the washing step of the perovskite compound is not particularly limited, but water washing is preferred. The drying method used in the drying step of the washed perovskite compound is not particularly limited, but examples include a method using a box dryer, fluidized bed dryer, flash dryer, or spray dryer, and leaving the dried compound in an atmosphere of 80 to 300°C for 0.5 to 24 hours in the case of a box dryer.
[0047] The method for producing a perovskite compound of the present invention is a method capable of producing barium calcium titanate having highly uniform particle size. The barium calcium titanate, which is one type of perovskite compound of the present invention and is obtained by such a production method of the present invention, can be suitably used as an electronic material for multilayer ceramic capacitors and the like.
[0048] Specific examples are given below to explain the present invention in detail, but the present invention is not limited to these examples. Unless otherwise specified, "%" and "wt%" mean "weight % (mass %)." The methods for measuring each physical property are as follows.
[0049] <Composition Analysis> Composition analysis was performed using an X-ray fluorescence analyzer (ZSX Primus II, manufactured by Rigaku Corporation, calibration curve method) to determine the molar ratios of Ba / Ti, Ca / Ti, and (Ba+Ca) / Ti. <Specific Surface Area> The specific surface areas of the barium titanate powder and barium calcium titanate powder were measured by the BET single-point method using a fully automatic specific surface area measurement device (Macsorb HM model-1220, manufactured by Mountec Co., Ltd.) after degassing at 350°C for 15 minutes. <Calculation of CV Value and Circularity> Images of particles were obtained at 30,000 magnification using a scanning electron microscope (SU8020, manufactured by Hitachi High-Tech Corporation), and the data obtained by dividing the images into nine sections was loaded into image analysis software DeepCle (manufactured by Sakai Chemical Industry Co., Ltd.) and analyzed using the analysis model Ver. Using Ver. 3.18, the average particle size (circle-equivalent diameter) and standard deviation σ (circle-equivalent diameter) were measured, and the standard deviation was divided by the average particle size. The resulting value was multiplied by 100 to calculate the CV value: coefficient of variation (%). The closer the circularity is to 1, the closer it is to a circle. This is defined as 4π x (area) / (square of perimeter), and the particle area and perimeter were measured and calculated using the image analysis software DeepClé analysis model Ver. 3.18. <Point Analysis and EDS Mapping> Point analysis and EDS mapping were performed using an atomic resolution analytical electron microscope (JEOL Ltd., JEM-ARM200F). <Crystal Structure> The crystal structure was confirmed using a powder X-ray analyzer (Bruker, D8 ADVANCE, radiation source: CuKα). <Formation and Evaluation of a Film Simulating a Green Sheet> (Dispersion Treatment) 0.2 g of dispersant (NOF Corporation, SP-0201) was placed in a polypropylene container, followed by 4 g of barium calcium titanate powder and 20 g of ethanol to obtain a barium calcium titanate mixture. 25 g of zirconia beads (3 mm diameter) were then added to this mixture, and the mixture was dispersed using a planetary ball mill. The zirconia beads were then removed. (Preparation of Organic Vehicle) 1.2 g of ethyl cellulose (Kishida Chemical Co., Ltd.) and 48.8 g of terpineol (Nippon Terpene Chemical Co., Ltd.) were added to a glass beaker and heated to dissolve, obtaining an organic vehicle. (Formation of a Film Simulating a Green Sheet) 1.0 g of the dispersed mixture and 0.8 g of organic vehicle were mixed, and a small amount was dripped onto a glass plate.The mixture on the glass plate was then applied to a film using an applicator with a gap of 75 μm. This film was dried at 120°C for 10 minutes to obtain a film simulating a green sheet. The surface roughness of this film (arithmetic mean roughness: Ra, maximum height: Rz) was measured using a surface roughness meter. The surface roughness was measured using a SURFCOM 130A (manufactured by Tokyo Seimitsu Co., Ltd.).
[0050] Example 1 (Barium titanate dispersion preparation step) 1.3 L of pure water and 1,157 g of barium hydroxide octahydrate (manufactured by Sakai Chemical Industry Co., Ltd.) were placed in a 5 L reaction vessel and heated to dissolve the barium hydroxide octahydrate in water to prepare a barium hydroxide aqueous solution. 0.23 L of titanium tetrachloride solution (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd., concentration of 186 g / L in terms of Ti) was mixed with the barium hydroxide aqueous solution to obtain BaTiO 3A barium titanate precursor aqueous slurry with a concentration of 80 g / L was obtained. The Ba / Ti molar ratio at the end of mixing the barium hydroxide aqueous solution and the titanium tetrachloride solution was 4.0. (Barium Ion Detachment Process) While stirring the barium titanate precursor slurry with a stirrer, a 20% nitric acid aqueous solution was added dropwise to adjust the pH of the slurry to 11.0, and the pH was maintained for 1 hour. The slurry was then filtered and washed with water until the electrical conductivity of the filtrate reached 50 μS / cm or less, yielding a washed cake. Water was added to the cake to bring the liquid volume to 1 L, and after washing, a barium titanate bulk slurry was obtained. A portion of the obtained slurry was sampled and dried in a box dryer at 95°C. The Ba / Ti molar ratio was determined by XRF analysis and found to be 0.814. SEM observation results of this barium titanate precursor aqueous slurry are shown in Figure 1-1. FIG. 1-1 confirms that the obtained barium titanate precursor had no particle aggregation. (Heat Treatment Step (Drying Step)) After the water washing, 12 g of calcium acetate monohydrate (Kanto Chemical Co., Ltd.) and 27 g of barium hydroxide octahydrate (Sakai Chemical Industry Co., Ltd.) were added to the barium titanate bulk slurry, which was then stirred with a stirrer. The mixture was then spray-dried at 95°C and crushed in a mortar or other device to obtain a barium calcium titanate precursor powder. (Heat Treatment Step (Firing Step)) 20 g of the barium calcium titanate precursor powder was placed in an alumina crucible and heat-treated in an air furnace at 600°C for 2 hours to obtain a barium calcium titanate-bound product. (Disintegration Step) 15 g of the obtained barium calcium titanate-bound product was placed in an autoclave, and 7 g of pure water and 11 g of barium hydroxide octahydrate (Sakai Chemical Industry Co., Ltd.) were added, followed by hydrothermal treatment at 160°C for 24 hours. The contents of the autoclave were allowed to cool to room temperature, and the recovered slurry was filtered and washed with water until the electrical conductivity of the filtrate reached 50 μS / cm or less, after which it was dried for 6 hours in a box dryer at 95°C. The dried solidified material was crushed in a mortar to obtain barium calcium titanate powder. SEM observation results of the obtained barium calcium titanate are shown in Figure 1-2, HAADF-STEM images are shown in Figures 3 and 4, and EDS mapping results are shown in Figures 5 and 6. Figure 1-2 confirms that the obtained barium calcium titanate was spherical and had a uniform particle size.Point analysis at location 01 in the HAADF-STEM image in Figure 3 revealed that the proportions were 2.0 atomic % for Ca and 98.0 atomic % for Ba + Ti. Here, atomic % is synonymous with mol %. In Figure 4, barium atoms are shown in white, and titanium atoms are shown in gray. In Figure 5, which shows the results of EDS mapping, only Ba is shown in white, and in Figure 6, only Ca is shown in white. Comparing Figures 5 and 6, Ca is detected in Figure 6 at a position that overlaps with the Ba position in Figure 5. This confirmed that calcium was dissolved in the barium site.
[0051] Examples 2 to 7 Examples 2 to 7 were carried out in the same manner as Example 1, except that the types and amounts of the various components used in the reaction and the reaction conditions were changed as shown in Table 1. The results of XRD measurement of the barium calcium titanate obtained in Example 7 are shown in Figure 7. No phase was observed in the XRD measurement chart of Figure 7, confirming that a highly pure perovskite-type compound was obtained.
[0052] Comparative Example 1: 1.6 L of pure water and 868 g of barium hydroxide octahydrate (manufactured by Sakai Chemical Industry Co., Ltd.) were placed in a 5 L reaction vessel and heated to dissolve the barium hydroxide octahydrate in the water, thereby preparing an aqueous barium hydroxide solution. 0.17 L of titanium tetrachloride solution (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd., concentration: 186 g / L in terms of Ti) was mixed with the aqueous barium hydroxide solution to obtain BaTiO 3 A barium titanate precursor aqueous slurry with a concentration of 60 g / L was obtained. The Ba / Ti molar ratio at the end of mixing the barium hydroxide aqueous solution and the titanium tetrachloride solution was 4.0. SEM observation results of the obtained barium titanate precursor aqueous slurry are shown in Figure 2-1. In Figure 2-1, particle aggregation of the barium titanate precursor was confirmed in the area surrounded by the solid line. Subsequently, the same procedures as in Example 1 were carried out up to the deagglomeration step, except that each step was changed as shown in Table 1, to obtain a barium calcium titanate powder of Comparative Example 1. SEM observation results of the barium calcium titanate obtained in the deagglomeration step are shown in Figure 2-2. In Figure 2-2, coarse particles of barium calcium titanate were observed in the area surrounded by the solid line, confirming variation in particle size.
[0053] Comparative Examples 2 and 3 Comparative Examples 2 and 3 were carried out in the same manner as Comparative Example 1, except that the types and amounts of the components used in the reaction and the reaction conditions were changed as shown in Table 1.
[0054] Comparative Example 4 (Barium titanate dispersion preparation step) 2.1 L of pure water and 909 g of barium hydroxide octahydrate (manufactured by Sakai Chemical Industry Co., Ltd.) were placed in a 5 L reaction vessel and heated to dissolve the barium hydroxide octahydrate in water to prepare a barium hydroxide aqueous solution. 0.50 L of titanium hydroxide aqueous slurry (manufactured by Sakai Chemical Industry Co., Ltd., concentration 184 g / L in terms of Ti) was mixed with the barium hydroxide aqueous solution to obtain BaTiO 3A barium titanate aqueous slurry with a concentration of 159 g / L was obtained. The Ba / Ti molar ratio was 2.2 when the titanium hydroxide aqueous slurry was added to the barium hydroxide aqueous solution. The barium titanate aqueous slurry was placed in an autoclave and subjected to hydrothermal treatment at 100°C for 6 hours. The contents of the autoclave were allowed to cool to room temperature, yielding a barium titanate precursor slurry. (Barium Ion Desorption Treatment Step) While stirring the barium titanate precursor slurry with a stirrer, a 20% nitric acid aqueous solution was added dropwise to adjust the slurry pH to 7.0, and the pH was maintained for 1 hour. The mixture was then filtered and washed with water until the electrical conductivity of the filtrate reached 100 μS / cm or less, yielding a washed cake. Water was added to the cake to make the liquid volume 1 L, yielding a washed barium titanate precursor slurry. A portion of the resulting slurry was sampled and dried in a box dryer at 95°C. The Ba / Ti molar ratio was determined by XRF analysis and found to be 0.902. (Heat Treatment Step (Drying Step)) After the water washing, 11 g of calcium acetate monohydrate (manufactured by Kanto Chemical Co., Inc.) was added to the barium titanate precursor slurry, stirred with a stirrer, spray-dried at 95°C, and crushed in a mortar or the like to obtain a barium calcium titanate precursor powder. (Heat Treatment Step (Firing Step)) 10 g of the barium calcium titanate precursor powder was placed in an alumina crucible and heat-treated in an air-tight firing furnace at 600°C for 2 hours to obtain a barium calcium titanate-bound product. (Disintegration Step) 10 g of the resulting barium calcium titanate-bound product was placed in an autoclave, and 50 g of pure water and 29 g of barium hydroxide octahydrate (manufactured by Sakai Chemical Industry Co., Ltd.) were added, followed by hydrothermal treatment at 160°C for 24 hours. The contents of the autoclave were allowed to cool to room temperature, and the recovered slurry was filtered and washed with water until the electrical conductivity of the filtrate reached 50 μS / cm or less, after which it was dried for 6 hours in a box dryer at 95° C. The dried solidified material was crushed in a mortar to obtain a barium calcium titanate powder.
[0055] Comparative Example 5 Comparative Example 5 was carried out in the same manner as in Comparative Example 4, except that the types and amounts of the components used in the reaction and the reaction conditions were changed as shown in Table 1.
[0056]
[0057] Table 2 shows the results of various measurements on the barium calcium titanate (BCT) obtained in Examples 1 to 7 and Comparative Examples 1 to 5.
[0058]
[0059] As shown in Tables 1 and 2, barium calcium titanate with a CV value of 20% or less was obtained in all of Examples 1 to 7. On the other hand, the barium calcium titanate obtained in Comparative Examples 1 to 5 all had a CV value of greater than 20%. These results confirm that barium calcium titanate with a high degree of particle size uniformity can be obtained by using the method for producing a perovskite compound of the present invention.
Claims
1. The following general formula (1): (1-x) A x TiO 3 (1) A perovskite type compound represented by the formula: (wherein A represents Ca or Sr, and x is a number satisfying 0.00<x≦0.30), characterized in that a CV value represented by a ratio of a standard deviation of particle diameter to an average particle diameter (equivalent circle diameter) obtained by observation with a scanning electron microscope (standard deviation of particle diameter / average particle diameter×100) is 20% or less.
2. BET specific surface area is 5 to 70 m 2 2. The perovskite compound according to claim 1, wherein the Mo content is 1 / g.
3. A method for producing a perovskite compound, comprising: a barium titanate dispersion preparation step of mixing a barium compound with an aqueous titanium compound solution to obtain a barium titanate dispersion; a barium ion depletion step of washing the barium titanate dispersion obtained in the barium titanate dispersion preparation step to obtain barium titanate having a molar ratio of barium element to titanium element of less than 1.00; a heat treatment step of mixing the barium titanate obtained in the barium ion depletion step with a calcium salt or a strontium salt and heat treating the mixture; and a disintegration step of heating the compound obtained in the heat treatment step in a solvent to disintegrate the particles, wherein in the barium titanate dispersion preparation step, at least one of the following is performed: the barium compound and the aqueous titanium compound solution are used so that the molar ratio (Ba / Ti) of the barium element in the barium compound to the titanium element in the aqueous titanium compound solution is 4.5 or more, or the barium titanate concentration in the barium titanate dispersion used in the barium ion depletion step is 65 g / L or more.
Citation Information
Patent Citations
Fine powder of perovskite type compound and its production
JP1994305729A
Production of perovskite-type multiple oxide powder
JP1995277710A
Barium calcium titanate, production process thereof and capacitor
JP2006089368A
Production Of Barium Titanate Compounds
US20070202036A1
Method for producing perovskite compound, and perovskite compound
WO2021199702A1
Cited By
Inorganic particle material, method for producing same, and resin composition
WO2026185945A1