Composite copper current collector and preparation method therefor and use thereof

By preparing the second copper layer on the surface of the first copper layer of the polymer substrate layer, and combining the design of the anti-adhesion functional layer and the protective layer, the adhesion problem of composite copper current collector during the winding process is solved, which significantly improves the Its performance and stability have promoted its application in the battery field.

WO2024234308A1PCT designated stage expired Publication Date: 2024-11-21JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD

Patent Information

Application Number
PCT/CN2023/094576
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Traditional composite copper current collectors are prone to adhesion and surface tearing during the winding process, resulting in microscopic defects and affecting their performance and application.

Method used

The second copper layer is prepared on the surface of the first copper layer of the polymer substrate layer, and the design of the anti-adhesion functional layer and the protective layer can reduce the adhesion and defect rate, and use magnetron sputtering and electroplating to improve the design of the anti-adhesion functional layer and the protective layer. Properties of composite copper current collectors.

Benefits of technology

It significantly reduces the defect rate and square resistance of the composite copper current collector, improves the adhesion between the polymer substrate layer and the first copper layer, enhances the performance and stability of the composite copper current collector, and promotes its battery field Promote and apply.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023094576_21112024_PF_FP_ABST
    Figure CN2023094576_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a composite copper current collector, comprising a polymer base material layer (1). At least one side of the polymer base material layer (1) is provided with a first copper layer (2), the side of the first copper layer (2) distant from the polymer base material layer (1) is provided with a second copper layer (3), and the defect rate of the second copper layer (3) is less than or equal to 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Composite copper current collector and its preparation method and application Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a composite copper current collector and a preparation method and application thereof. Background Art

[0002] The preparation process of a polymer film-based composite copper current collector is typically divided into two steps: first, a layer of copper is deposited on the polymer film to produce a semi-finished composite copper current collector with a certain degree of conductivity; then, the semi-finished composite copper current collector is further processed to increase the thickness of the conductive copper layer, thereby producing a composite copper current collector with good conductivity. Compared with traditional copper current collectors, polymer film-based composite copper current collectors have the advantages of low cost, light weight, and excellent internal insulation. These characteristics enable the use of composite copper current collectors in batteries to reduce battery costs and improve battery energy density and safety.

[0003] Traditional composite copper current collectors deposit a copper layer on a polymer film to produce a semi-finished composite copper current collector. However, during the winding process, the surfaces of the semi-finished composite copper current collector come into contact with each other and adhere to each other. This can cause the adhered surfaces to tear during the unwinding process (electroplating), causing the microscopic copper layer to fall off and creating microscopic defects in the copper layer. During the electroplating process, copper cannot be deposited near the defect points due to the lack of conductivity, resulting in microscopic defects in the prepared composite copper current collector, which affects the performance and application of the composite copper current collector.

[0004] Summary of the Invention

[0005] In view of the above problems, the present application provides a composite copper current collector and a preparation method and application thereof, so as to reduce the defect rate of the composite copper current collector, thereby promoting the promotion and application of the composite copper current collector.

[0006] A first aspect of the present application provides a composite copper current collector, comprising a polymer substrate layer, wherein a first copper layer is provided on at least one side of the polymer substrate layer, a second copper layer is provided on a side of the first copper layer away from the polymer substrate layer, and a defect rate of the second copper layer is less than or equal to 5%.

[0007] In some embodiments, the defect rate of the second copper layer is less than or equal to 2%, and can be optionally 0-0.5%.

[0008] In some embodiments, the bonding force between the polymer substrate layer and the first copper layer is greater than or equal to 0.9 N / cm, and can be optionally 0.9 N / cm-10 N / cm.

[0009] In some embodiments, the sheet resistance of the composite copper current collector is less than or equal to 29 mΩ, and may be less than or equal to 24 mΩ.

[0010] In some embodiments, the thickness of the second copper layer is 500 nm-2000 nm, and optionally 700 nm-1200 nm.

[0011] In some embodiments, the thickness of the first copper layer is greater than or equal to 50 nm, and can be optionally 50 nm-500 nm.

[0012] In some embodiments, the polymer substrate layer has a thickness of 1.5 μm to 10 μm.

[0013] In some embodiments, the polymer substrate layer includes one or more of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene, and polyimide.

[0014] In some embodiments, the composite copper current collector further includes a protective layer, and the protective layer is located on a surface of the second copper layer away from the first copper layer.

[0015] In some embodiments, the thickness of the protective layer is 10 nm-100 nm, and can be optionally 30 nm-60 nm.

[0016] In some embodiments, the protective layer includes one or more of chromium oxide, copper chromium oxide, copper-organic acid complex, copper-imidazole complex, polysiloxane, nickel, chromium, nickel-chromium alloy, nickel oxide, graphite, carbon black, acetylene black, Ketjen black, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers and graphene.

[0017] The second aspect of the present application provides a method for preparing the composite copper current collector described in the first aspect of the present application, comprising the following steps:

[0018] preparing the first copper layer on at least one side of the polymer substrate layer;

[0019] preparing an anti-adhesive functional layer on a side of the first copper layer away from the polymer substrate layer, wherein the anti-adhesive functional layer comprises one or more of a metal and a metal oxide;

[0020] removing the anti-adhesion functional layer;

[0021] The second copper layer is prepared on the surface of the first copper layer from which the anti-adhesion functional layer is removed.

[0022] In some embodiments, the thickness of the anti-adhesion functional layer is greater than or equal to 5 nm, and can be optionally 10 nm-50 nm.

[0023] In some embodiments, the metal includes one or more of aluminum, magnesium, titanium, zinc, and nickel.

[0024] In some embodiments, the metal oxide includes one or more of aluminum oxide, magnesium oxide, copper oxide, cuprous oxide, nickel oxide, zinc oxide, and aluminum-doped zinc oxide.

[0025] In some embodiments, in the step of preparing the anti-adhesive functional layer on the side of the first copper layer away from the polymer substrate layer, the anti-adhesive functional layer is prepared by magnetron sputtering.

[0026] In some embodiments, the target material for magnetron sputtering includes one or more of the metal and the metal oxide.

[0027] In some embodiments, the source gas for magnetron sputtering includes argon.

[0028] In some embodiments, the gas source for magnetron sputtering includes argon gas, and the flow rate of the argon gas is less than or equal to 500 mL / min.

[0029] In some embodiments, the source gas for magnetron sputtering includes oxygen.

[0030] In some embodiments, the gas source for magnetron sputtering includes oxygen, and the flow rate of oxygen is less than or equal to 100 mL / min.

[0031] In some embodiments, the pressure in the magnetron sputtering chamber is less than or equal to 0.6 Pa.

[0032] In some embodiments, the power density of magnetron sputtering is 10 W / cm 2 -150W / cm 2 .

[0033] In some embodiments, the magnetron sputtering time is greater than or equal to 5 seconds.

[0034] In some embodiments, in the step of removing the anti-adhesive functional layer, an acid solution is used to dissolve and remove the anti-adhesive functional layer.

[0035] In some embodiments, the acid solution includes one of hydrochloric acid, sulfuric acid, nitric acid, a mixture of sulfuric acid and hydrochloric acid, and a mixture of sulfuric acid and nitric acid.

[0036] In some embodiments, the pH of the acid solution is less than or equal to 2.

[0037] In some embodiments, the dissolution time is greater than or equal to 10 s.

[0038] In some embodiments, in the step of preparing the first copper layer on at least one side of the polymer substrate layer, the first copper layer is prepared on at least one side of the polymer substrate layer by physical vapor deposition.

[0039] In some embodiments, in the step of removing the surface of the first copper layer of the anti-adhesion functional layer to prepare the second copper layer, the second copper layer is prepared by electroplating.

[0040] In some embodiments, the electroplating solution used to prepare the second copper layer by the electroplating method includes 100g / L-180g / L copper sulfate, 60g / L-120g / L sulfuric acid, 40g / L-100mg / L hydrochloric acid and electroplating solution additives.

[0041] In some embodiments, the electroplating bath additives include 1 mg / L-50 mg / L leveler, 100 mg / L-700 mg / L suppressor, and 0.5 mg / L-10 mg / L brightener.

[0042] In some embodiments, the leveler includes an organic amine compound, the inhibitor includes a polyethylene glycol compound, and the brightener includes an organic sulfur compound.

[0043] In some embodiments, the process conditions for preparing the second copper layer by electroplating include: the temperature of the electroplating solution is 20°C-40°C, the average cathode current density is 1A / dm 2 -5A / dm 2 , the electroplating time is 2min-15min.

[0044] The third aspect of the present application provides a negative electrode plate, comprising the composite copper current collector described in the first aspect of the present application or the composite copper current collector prepared by the preparation method described in the second aspect of the present application.

[0045] The fourth aspect of the present application provides a battery, comprising the negative electrode sheet described in the third aspect of the present application.

[0046] The fifth aspect of the present application provides an electrical device comprising the battery described in the fourth aspect of the present application.

[0047] The details of one or more embodiments of the present application are set forth in the description below. Other features, objects, and advantages of the present application will become apparent from the description and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] FIG1 is a schematic diagram of a composite copper current collector according to one embodiment of the present application.

[0049] FIG2 is a schematic diagram of a composite copper current collector according to another embodiment of the present application.

[0050] FIG3 is a field emission electron micrograph of the composite copper current collector prepared in Example 1 of the present application.

[0051] FIG4 is a field emission electron micrograph of the composite copper current collector prepared in Comparative Example 1 of the present application.

[0052] Description of reference numerals:

[0053] 1-polymer substrate layer; 2-first copper layer; 3-second copper layer; 4-protective layer. DETAILED DESCRIPTION

[0054] The following will clearly and completely describe the technical solutions of this application in conjunction with specific embodiments. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "one or more" used herein includes any and all combinations of one or more related listed items. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly defined. In this application, the technical features described in an open manner include closed technical solutions consisting of the listed features, and also include open technical solutions containing the listed features.

[0056] In this application, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.

[0057] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0058] In this application, terms such as "first aspect," "second aspect," and "third aspect" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor as implicitly indicating the importance or quantity of the technical features indicated. Furthermore, terms such as "first," "second," and "third," etc., are intended only to provide a non-exhaustive enumeration and description and should not constitute a closed-ended limitation on quantity.

[0059] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0060] In the present application, unless otherwise specified, the thickness of the first copper layer, the thickness of the second copper layer, the thickness of the anti-adhesive functional layer, and the thickness of the protective layer all refer to their thicknesses on one side of the polymer substrate layer.

[0061] Conventional semi-finished composite copper current collectors experience microscopic defects due to adhesion between their surfaces. This is because the copper grains deposited on the polymer film are in a metastable state, allowing them to fuse, leading to adhesion and microscopic defects. This application provides a composite copper current collector, its preparation method, and its application to address these issues.

[0062] In a first aspect, the present application provides a composite copper current collector comprising a polymer substrate layer, wherein a first copper layer is provided on at least one side of the polymer substrate layer, and a second copper layer is provided on a side of the first copper layer away from the polymer substrate layer, wherein the defect rate of the second copper layer is less than or equal to 5%.

[0063] In the above-described embodiment, a second copper layer is provided on the surface of the first copper layer, which can significantly reduce the defect rate of the second copper layer compared to the defect rate of the copper layer in a conventional composite copper current collector, thereby improving the performance and stability of the composite copper current collector and promoting the promotion and application of the composite copper current collector. Specifically, the defect rate of the second copper layer includes, but is not limited to, 0, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%.

[0064] In some embodiments, with reference to FIG1 , the composite copper current collector includes a polymer substrate layer 1 , wherein a first copper layer 2 is provided on both side surfaces of the polymer substrate layer 1 in a thickness direction thereof, and a second copper layer 3 is provided on a surface of the first copper layer 2 away from the polymer substrate layer 1 .

[0065] In some embodiments, with reference to FIG2 , the composite copper current collector includes a polymer substrate layer 1 , a first copper layer 2 is provided on one surface of the polymer substrate layer 1 in a thickness direction thereof, and a second copper layer 3 is provided on the surface of the first copper layer 2 away from the polymer substrate layer 1 .

[0066] In some embodiments, the defect rate of the second copper layer is less than or equal to 2%. This defect rate is significantly lower than the defect rate of the copper layer in conventional composite copper current collectors, thereby further improving the performance and stability of the composite copper current collector and promoting the promotion and application of the composite copper current collector. Furthermore, the defect rate of the second copper layer is 0-0.5%.

[0067] In some embodiments, the bonding force between the polymer substrate layer and the first copper layer is greater than or equal to 0.9 N / cm. Compared with the bonding force between the polymer substrate layer and the first copper layer in a conventional composite copper current collector, the bonding force between the polymer substrate layer and the first copper layer is significantly higher, thereby further improving the performance and stability of the composite copper current collector and promoting the promotion and application of the composite copper current collector. In some optional embodiments, the bonding force between the polymer substrate layer and the first copper layer is 0.9 N / cm-10 N / cm. It is understood that the bonding force between the polymer substrate layer and the first copper layer includes but is not limited to: 1.5 N / cm, 1.8 N / cm, 2 N / cm, 2.5 N / cm, 3 N / cm, 3.5 N / cm, 4 N / cm, 4.5 N / cm, 5 N / cm, 6 N / cm, 7 N / cm, 8 N / cm, 9 N / cm, 10 N / cm, 11 N / cm, 12 N / cm, 15 N / cm.

[0068] In some embodiments, the square resistance of the composite copper current collector is less than or equal to 29 mΩ. Compared with the square resistance of conventional composite copper current collectors, the square resistance of the composite copper current collector is significantly reduced, thereby further improving the performance and stability of the composite copper current collector and promoting the promotion and application of the composite copper current collector. Furthermore, the square resistance of the composite copper current collector is less than or equal to 24 mΩ. It is understood that the square resistance of the composite copper current collector includes but is not limited to: 10 mΩ, 13 mΩ, 16 mΩ, 19 mΩ, 22 mΩ, 24 mΩ, 26 mΩ, and 29 mΩ.

[0069] In some embodiments, the thickness of the second copper layer is 500 nm to 2000 nm. It should be noted that to balance the conductivity of the composite copper current collector and the requirement that the composite copper current collector be as thin as possible, the thickness of the second copper layer is controlled to be within the above range. Furthermore, the thickness of the second copper layer can be selected to be 700 nm to 1200 nm. It is understood that the thickness of the second copper layer includes, but is not limited to, 500 nm, 700 nm, 1000 nm, 1200 nm, 1400 nm, 1600 nm, 1800 nm, and 2000 nm.

[0070] In some embodiments, the thickness of the first copper layer is greater than or equal to 50 nm. It should be noted that controlling the thickness of the first copper layer to be within the above range improves the conductivity of the polymer substrate layer containing the first copper layer, and facilitates the attachment of the second copper layer to the first copper layer during the preparation of the second copper layer. Furthermore, the thickness of the first copper layer is 50 nm-500 nm. It is understood that the thickness of the above-mentioned first copper layer includes but is not limited to: 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm.

[0071] In some embodiments, the thickness of the polymer substrate layer is 1.5 μm-10 μm. Controlling the thickness of the polymer substrate layer within the above range takes into account its preparation process and cost, and can meet the application requirements of the composite copper current collector. It is understood that the thickness of the polymer substrate layer includes but is not limited to: 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm.

[0072] In some embodiments, the polymer substrate layer includes one or more of polyethylene terephthalate (PET), polypropylene (PP), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene, polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polystyrene (PS) and polyimide (PI).

[0073] In some embodiments, the composite copper current collector further includes a protective layer located on a surface of the second copper layer away from the first copper layer. It is understood that the protective layer located on the surface of the second copper layer can prevent the second copper layer from being chemically corroded or physically damaged.

[0074] Exemplarily, in conjunction with FIG. 1 and FIG. 2 , a protective layer 4 is provided on a surface of the second copper layer 3 that is away from the first copper layer 2 .

[0075] In some embodiments, the thickness of the protective layer is 10 nm to 100 nm. Controlling the thickness of the protective layer within the above range can further improve the protective effect of the protective layer on the second copper layer. When the thickness of the protective layer is too thin, its protective effect on the second copper layer is not obvious; when the thickness of the protective layer is too thick, it will affect the conductivity of the composite copper current collector. Furthermore, the thickness of the protective layer is 30 nm to 60 nm. It is understood that the thickness of the protective layer includes but is not limited to: 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, and 100 nm.

[0076] In some embodiments, the protective layer includes one or more of chromium oxide, copper chromium oxide, copper-organic acid complex, copper-imidazole complex, polysiloxane, nickel, chromium, nickel-chromium alloy, nickel oxide, graphite, carbon black, acetylene black, Ketjen black, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers and graphene.

[0077] In a second aspect, the present application provides a method for preparing the composite copper current collector described in the first aspect of the present application, comprising the following steps:

[0078] forming a first copper layer on at least one side of the polymer substrate layer;

[0079] preparing an anti-adhesive functional layer on a side of the first copper layer away from the polymer substrate layer, wherein the anti-adhesive functional layer comprises one or more of a metal and a metal oxide;

[0080] Removing the anti-adhesion functional layer;

[0081] A second copper layer is prepared on the surface of the first copper layer from which the anti-adhesion functional layer is removed.

[0082] The metal and metal oxide contained in the anti-adhesion functional layer are relatively stable or exist in an amorphous state, effectively inhibiting adhesion between the first copper layers. Removing the anti-adhesion functional layer from the first copper layer before forming the second copper layer prevents the introduction of impurities that could affect the purity of the second copper layer. Furthermore, the above-mentioned preparation method is simple to operate and suitable for large-scale promotion.

[0083] In some embodiments, the thickness of anti-bonding functional layer is greater than or equal to 5nm.Control the thickness of anti-bonding functional layer to be above-mentioned scope, further suppresses mutual bonding between the first copper layer.When the thickness of above-mentioned anti-bonding functional layer is too thin, the uniformity of anti-bonding functional layer is difficult to control, and can not have good protection effect to the first copper layer.It is understandable that, from the angle of cost, anti-bonding functional layer should not be too thick, and therefore, the thickness of anti-bonding functional layer can be selected as 10nm-50nm.Specifically, the thickness of anti-bonding functional layer includes but is not limited to: 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm.

[0084] In some embodiments, the metal includes one or more of aluminum, magnesium, titanium, zinc, and nickel. The internal crystals of these metal materials are relatively stable or exist in an amorphous state, and are easily soluble in acid, making them easy to remove, thereby avoiding the introduction of impurities that may affect the purity of the prepared second copper layer.

[0085] In some embodiments, the metal oxide includes one or more of aluminum oxide, magnesium oxide, copper oxide, cuprous oxide, nickel oxide, zinc oxide, and aluminum-doped zinc oxide. The internal crystals of these metal oxide materials are relatively stable or exist in an amorphous state, and are easily soluble in acid, making them easy to remove, thereby avoiding the introduction of impurities that may affect the purity of the prepared second copper layer.

[0086] In some embodiments, in the step of preparing the anti-adhesive functional layer on the side of the first copper layer away from the polymer substrate layer, the anti-adhesive functional layer is prepared by magnetron sputtering, thereby making it easier to prepare the anti-adhesive functional layer.

[0087] In some specific embodiments, the target material for magnetron sputtering includes one or more of metals and metal oxides. The purity of the target material is ≥99.9%. Controlling the purity of the target material improves the quality of the prepared anti-sticking functional layer.

[0088] In some specific embodiments, the gas source for magnetron sputtering includes argon. Thus, the quality of the prepared anti-adhesive functional layer is further improved. Alternatively, when the target material for magnetron sputtering is a metal, argon is used as the gas source for magnetron sputtering, and the prepared anti-adhesive functional layer is the metal. Alternatively, when the target material for magnetron sputtering is a metal oxide, argon is used as the gas source for magnetron sputtering, and the prepared anti-adhesive functional layer is the metal oxide.

[0089] In some specific embodiments, the flow rate of argon gas is less than or equal to 500 mL / min. This further improves the quality of the prepared anti-adhesive functional layer. It is understood that the flow rate of argon gas includes, but is not limited to, 50 mL / min, 100 mL / min, 150 mL / min, 200 mL / min, 250 mL / min, 300 mL / min, 400 mL / min, and 500 mL / min.

[0090] In some specific embodiments, the source gas for magnetron sputtering also includes oxygen. This further improves the quality of the anti-adhesion functional layer. Alternatively, when the target material for magnetron sputtering is a metal, the source gas uses argon and oxygen, and the anti-adhesion functional layer prepared is an oxide of the metal.

[0091] In some specific embodiments, the flow rate of oxygen is less than or equal to 100 mL / min. Thus, the quality of the prepared anti-adhesive functional layer is further improved. It is understood that the flow rate of oxygen includes but is not limited to: 10 mL / min, 20 mL / min, 30 mL / min, 40 mL / min, 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min, and 100 mL / min.

[0092] In some specific embodiments, the pressure within the magnetron sputtering chamber is less than or equal to 0.6 Pa. Controlling the pressure within the chamber further improves the quality of the anti-adhesive functional layer. When the pressure within the chamber is too high, the quality of the anti-adhesive functional layer is poor. It is understood that the pressure within the magnetron sputtering chamber includes, but is not limited to, 0.1 Pa, 0.2 Pa, 0.3 Pa, 0.4 Pa, 0.5 Pa, and 0.6 Pa.

[0093] In some specific embodiments, the power density of magnetron sputtering is 10 W / cm 2 -150W / cm 2. Controlling the power density of magnetron sputtering to the above range further improves the quality of the anti-adhesive functional layer and the deposition efficiency. When the power density is too low, the deposition efficiency of the anti-adhesive functional layer is low; when the power density is too high, the prepared anti-adhesive functional layer is prone to defects. Optionally, under this power density condition, the power supply of the magnetron sputtering is a DC power supply. It is understood that the power density of magnetron sputtering includes but is not limited to: 10W / cm 2 、30W / cm 2 , 50W / cm 2 、80W / cm 2 , 100W / cm 2 , 120W / cm 2 、150W / cm 2 .

[0094] In some specific embodiments, the time of magnetron sputtering is greater than or equal to 5s. The time of controlling magnetron sputtering is above-mentioned scope, can further improve the anti-bonding effect of anti-bonding functional layer. When the time of magnetron sputtering is too short, the anti-bonding functional layer of preparation is too thin and uneven, and its anti-bonding effect is poor. It is understandable that the time of magnetron sputtering includes but is not limited to: 5s, 8s, 10s, 12s, 15s, 18s, 20s, 22s, 25s.

[0095] In some embodiments, during the step of removing the anti-adhesive functional layer, an acid solution is used to dissolve and remove the anti-adhesive functional layer. This allows for simpler removal of the anti-adhesive functional layer, thereby preventing impurities from being introduced during the subsequent preparation of the second copper layer and affecting the purity of the second copper layer.

[0096] In some embodiments, the acid solution comprises one of hydrochloric acid, sulfuric acid, nitric acid, a mixture of sulfuric acid and hydrochloric acid, and a mixture of sulfuric acid and nitric acid. This allows for simple removal of the anti-adhesive functional layer, preventing the introduction of impurities during the subsequent preparation of the second copper layer that could affect the purity of the second copper layer. It should be noted that in the mixture of sulfuric acid and hydrochloric acid, the sulfuric acid and hydrochloric acid can be mixed in any ratio; and in the mixture of sulfuric acid and nitric acid, the sulfuric acid and nitric acid can be mixed in any ratio.

[0097] In some embodiments, the pH of the acid solution is less than or equal to 2. Controlling the pH of the acid solution within the above range can further improve the dissolution efficiency of the anti-adhesive functional layer. When the pH is too high, the acidity of the acid solution is weak, resulting in a slow dissolution rate of the anti-adhesive functional layer and low dissolution efficiency. It is understood that the pH of the acid solution includes, but is not limited to, 0.5, 0.7, 1, 1.2, 1.4, 1.6, 1.8, and 2.

[0098] In some embodiments, the dissolution time is greater than or equal to 10s. Controlling the dissolution time to be within the above range can further improve the dissolution efficiency of the anti-adhesive functional layer. When the dissolution time is too short, the anti-adhesive functional layer is not sufficiently dissolved, and the anti-adhesive functional layer has residues, which will affect the purity of the prepared second copper layer. It is understandable that the dissolution time includes but is not limited to: 10s, 12s, 15s, 18s, 20s, 22s, 25s, 28s, 30s, 32s, 35s.

[0099] In some embodiments, the step of forming the first copper layer on at least one side of the polymer substrate layer is performed by physical vapor deposition, specifically, the physical vapor deposition method includes one or more of magnetron sputtering and vacuum evaporation.

[0100] In some embodiments, in the step of forming the first copper layer on at least one side of the polymer substrate layer, the first copper layer is formed by magnetron sputtering.

[0101] In some specific embodiments, the process conditions for preparing the first copper layer by magnetron sputtering include: the metal target is a copper metal target. Optionally, the purity of the copper metal target is ≥ 99.9%. Controlling the purity of the copper metal target improves the quality of the prepared first copper layer.

[0102] In some specific embodiments, the process conditions for preparing the first copper layer by magnetron sputtering include: the gas source is argon gas, and the argon gas flow rate is less than or equal to 500 mL / min. Controlling the flow rate of argon gas further improves the quality of the prepared first copper layer. When the argon gas flow rate is too high, the pressure in the cabin increases, and the quality of the prepared first copper layer is poor. It is understood that the flow rate of argon gas includes but is not limited to: 50 mL / min, 100 mL / min, 150 mL / min, 200 mL / min, 250 mL / min, 300 mL / min, 400 mL / min, 500 mL / min.

[0103] In some specific embodiments, the process conditions for preparing the first copper layer using magnetron sputtering include: the pressure in the chamber is less than or equal to 0.6 Pa. Controlling the pressure in the chamber further improves the quality of the prepared first copper layer. When the pressure in the chamber is too high, the quality of the prepared first copper layer is poor. It is understood that the pressure in the chamber for magnetron sputtering includes, but is not limited to, 0.1 Pa, 0.2 Pa, 0.3 Pa, 0.4 Pa, 0.5 Pa, and 0.6 Pa.

[0104] In some specific embodiments, the process conditions for preparing the first copper layer by magnetron sputtering include: the power supply is a DC power supply, the power density is 10W / cm 2 -150W / cm 2Controlling the power density further improves the quality of the first copper layer. When the power density is too low, the deposition efficiency of the first copper layer is poor; when the power density is too high, defects are easily generated in the first copper layer. It is understood that the power density of magnetron sputtering includes but is not limited to: 10W / cm 2 、30W / cm 2 , 50W / cm 2 、80W / cm 2 , 100W / cm 2 , 120W / cm 2 、150W / cm 2 .

[0105] In some specific embodiments, the process conditions for preparing the first copper layer using a magnetron sputtering method include: a magnetron sputtering time of greater than or equal to 10 seconds. Controlling the magnetron sputtering time further improves the quality of the prepared first copper layer and the quality of the prepared second copper layer. When the magnetron sputtering time is too short, the thickness of the prepared first copper layer is too thin, resulting in poor conductivity of the first copper layer, which affects the subsequent preparation of the second copper layer. It is understood that the magnetron sputtering time includes but is not limited to: 10 seconds, 12 seconds, 15 seconds, 18 seconds, 20 seconds, 22 seconds, 25 seconds, 28 seconds, and 30 seconds.

[0106] In some embodiments, in the step of preparing the second copper layer by removing the surface of the first copper layer of the anti-adhesive functional layer, the second copper layer is prepared by electroplating, thereby making it easier to prepare the second copper layer and improving the preparation efficiency of the second copper layer.

[0107] In some embodiments, the electroplating solution used to prepare the second copper layer by electroplating includes 100 g / L-180 g / L copper sulfate, 60 g / L-120 g / L sulfuric acid, 40 g / L-100 mg / L hydrochloric acid, and electroplating solution additives.

[0108] In some embodiments, the electroplating solution additives include a leveler, a suppressor, and a brightener. Optionally, the concentrations of the leveler, suppressor, and brightener in the electroplating solution are 1 mg / L-50 mg / L, 100 mg / L-700 mg / L, and 0.5 mg / L-10 mg / L, respectively.

[0109] In some embodiments, the leveler comprises an organic amine compound, the inhibitor comprises a polyethylene glycol compound, and the brightener comprises an organic sulfur compound. Alternatively, the organic amine compound comprises one or more of 2-mercaptopyridine and Janus Green. The organic sulfur compound comprises one or more of sodium polydisulfide propanesulfonate (SPS) and sodium 3-mercapto-1-propanesulfonate (MPS).

[0110] In some embodiments, the process conditions for preparing the second copper layer by electroplating include: the temperature of the electroplating solution is 20°C-40°C, the average cathode current density is 1A / dm 2 -5A / dm 2 , the electroplating time is 2min-15min.

[0111] In some embodiments, the method for preparing a composite copper current collector further includes: preparing a protective layer on a surface of the second copper layer away from the first copper layer.

[0112] In some embodiments, the method for preparing the protective layer includes one or more of a coating method, a physical vapor deposition method, and a chemical vapor deposition method. Optionally, the coating method includes at least one of a dip coating method, a die coating method, a blade coating method, and an extrusion coating method; the physical vapor deposition method includes at least one of a vacuum evaporation method and a magnetron sputtering method; and the chemical vapor deposition method includes at least one of an atmospheric pressure chemical vapor deposition method and a plasma-enhanced chemical vapor deposition method.

[0113] In a third aspect, the present application provides a negative electrode plate, which includes the composite copper current collector described in the first aspect of the present application or the composite copper current collector prepared by the preparation method described in the second aspect of the present application.

[0114] The negative electrode sheet includes a composite copper current collector and a negative electrode active material layer. The negative electrode active material layer is disposed on at least one surface of the composite copper current collector. The negative electrode active material layer includes a negative electrode active material for batteries known in the art. For example, the negative electrode active material may include, but is not limited to, one or more of graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The present application does not particularly limit the preparation method of the negative electrode sheet. For example, the negative electrode sheet can be prepared by coating a negative electrode active slurry on at least one surface of the composite copper current collector. The negative electrode active slurry may include a negative electrode active material, a conductive agent, a binder, and a solvent.

[0115] In a fourth aspect, the present application provides a battery comprising the negative electrode sheet described in the third aspect of the present application.

[0116] Typically, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the charge and discharge process of the battery, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. The above-mentioned batteries may include but are not limited to lithium-ion secondary batteries, lithium-ion polymer secondary batteries, or lithium metal secondary batteries.

[0117] In a fifth aspect, the present application provides an electrical device comprising the battery described in the fourth aspect of the present application.

[0118] The above-mentioned battery can be used as a power source or energy storage unit in electrical devices, including but not limited to: electric vehicles, smart home appliances, computers, tablets, mobile phones, digital cameras, energy storage systems, etc.

[0119] The present application is further described in detail below with reference to specific embodiments and comparative examples.

[0120] Example 1

[0121] The preparation method of the composite copper current collector comprises the following steps:

[0122] S1. A 4.5 μm-thick biaxially oriented PET film was placed in a magnetron sputtering machine containing two independent sputtering chambers for the first magnetron sputtering process to form a first copper layer on both surfaces of the PET film in the thickness direction. The specific process parameters of the first magnetron sputtering process were as follows: a copper metal target with a purity of 99.99%, argon gas as the gas source, an argon gas flow rate of 500 mL / min, a chamber pressure of 0.2 Pa, and a DC power output power density of 100 W / cm 2 , the sputtering time is 20s;

[0123] S2. The product obtained in step S1 is placed in a second sputtering chamber, and an anti-adhesive functional layer is prepared on the surface of the first copper layer using a second magnetron sputtering process. The material of the anti-adhesive functional layer is aluminum oxide. The specific process parameters of the second magnetron sputtering process are as follows: the target material used is an aluminum metal target with a purity of 99.99%, the gas source is argon and oxygen, the argon flow rate is 500 mL / min, the oxygen flow rate is 100 mL / min, the pressure in the chamber is 0.6 Pa, and the power density of the DC power supply output is 10 W / cm 2 , the magnetron sputtering time is 5s;

[0124] S3. The anti-adhesive functional layer was dissolved in a hydrochloric acid solution for 10 seconds to remove the anti-adhesive functional layer. The pH of the hydrochloric acid solution was 2. After the anti-adhesive functional layer was completely dissolved, it was washed in a pure water tank for 30 seconds.

[0125] S4. A second copper layer is prepared on the product obtained in step S3 by electroplating, the second copper layer being located on the surface of the first copper layer; the components of the electroplating solution are a mixed aqueous solution of 100 g / L copper sulfate, 80 g / L sulfuric acid, 60 mg / L hydrochloric acid, 8 mg / L sodium polydisulfide bis(propanesulfonate), 10 mg / L 2-mercaptopyridine, and 100 mg / L PEG6000; the temperature of the electroplating solution is 25°C, and the average cathode current density is 2 A / dm 2 , the electroplating time is 6min;

[0126] S5. Prepare a protective layer on the surface of the second copper layer; after the electroplating is completed, place the plated film in a pure water cleaning tank for cleaning. After cleaning, soak it in a 5g / L chromic anhydride aqueous solution (25°C) for 30s, and then rinse it with pure water. After cleaning, place it in a 70°C oven for drying to obtain a finished composite copper current collector.

[0127] Example 2

[0128] The process is basically the same as Example 1, except that in step S2, the flow rate of argon gas is 300 mL / min.

[0129] Example 3

[0130] The process is basically the same as Example 1, except that in step S2, the flow rate of argon gas is 50 mL / min.

[0131] Example 4

[0132] The process is basically the same as Example 1, except that in step S2, the flow rate of argon gas is 550 mL / min.

[0133] Example 5

[0134] It is basically the same as Example 1, except that in step S2, the pressure inside the cabin is 0.2 Pa.

[0135] Example 6

[0136] It is basically the same as Example 1, except that in step S2, the pressure inside the cabin is 0.8 Pa.

[0137] Example 7

[0138] The process is basically the same as that of Example 1, except that in step S2, the magnetron sputtering time is 20 seconds.

[0139] Example 8

[0140] The process is basically the same as that of Example 1, except that in step S2, the magnetron sputtering time is 3 seconds.

[0141] Example 9

[0142] The same as Example 1, except that: in step S2, the power density of the DC power supply output is 80W / cm 2 .

[0143] Example 10

[0144] The same as Example 1, except that: in step S2, the power density of the DC power supply output is 150W / cm 2 .

[0145] Example 11

[0146] The same as Example 1, except that in step S2, the power density of the DC power supply output is 170W / cm 2 .

[0147] Example 12

[0148] The same as Example 1, except that: in step S2, the power density of the DC power supply output is 5W / cm 2 .

[0149] Example 13

[0150] The method is basically the same as Example 1, except that in step S2, the flow rate of argon is 501 mL / min, the flow rate of oxygen is 301 mL / min, the pressure in the cabin is 0.7 Pa, and the power density of the DC power supply is 9 W / cm 2 , the magnetron sputtering time is 4s.

[0151] Example 14

[0152] The method is basically the same as Example 1, except that: in step S3, the anti-adhesive functional layer is dissolved in a hydrochloric acid solution for 30 seconds.

[0153] Example 15

[0154] The method is basically the same as Example 1, except that: in step S3, the anti-adhesive functional layer is dissolved in a hydrochloric acid solution for 2 seconds.

[0155] Example 16

[0156] The method is basically the same as Example 1, except that in step S3, the pH value of the hydrochloric acid solution is 1.

[0157] Example 17

[0158] The method is basically the same as Example 1, except that in step S3, the pH value of the hydrochloric acid solution is 3.

[0159] Example 18

[0160] The method is basically the same as Example 1, except that in step S2, the target material used is a zinc metal target material, and the material of the anti-adhesion functional layer is zinc oxide.

[0161] Example 19

[0162] The method is basically the same as Example 1, except that in step S2, the target material used is a copper metal target material, and the material of the anti-adhesion functional layer is copper oxide.

[0163] Example 20

[0164] The method is basically the same as Example 1, except that in step S2, the target material used is a magnesium metal target material, and the material of the anti-adhesion functional layer is magnesium oxide.

[0165] Example 21

[0166] It is basically the same as Example 1, except that: in step S2, the target material used is an aluminum oxide target material, the gas source does not contain oxygen, and the material of the anti-adhesion functional layer is aluminum oxide.

[0167] Example 22

[0168] The method is basically the same as Example 1, except that: in step S2, the gas source does not contain oxygen, and the material of the anti-adhesion functional layer is aluminum.

[0169] Example 23

[0170] It is basically the same as Example 1, except that: in step S2, the target material used is a titanium target material, the gas source does not contain oxygen, and the material of the anti-adhesion functional layer is titanium.

[0171] Example 24

[0172] The method is basically the same as Example 1, except that: in step S1, the polymer substrate layer is a biaxially oriented PP film with a thickness of 4.5 μm.

[0173] Example 25

[0174] The method is basically the same as Example 1, except that: in step S1, the polymer substrate layer is a biaxially oriented PPS film with a thickness of 4.5 μm.

[0175] Example 26

[0176] The method is basically the same as Example 1, except that: in step S2, the magnetron sputtering time is 2.5 s, so that the thickness of the prepared anti-sticking functional layer is 5 nm.

[0177] Example 27

[0178] The method is basically the same as Example 1, except that: in step S2, the magnetron sputtering time is 50 s, so that the thickness of the prepared anti-sticking functional layer is 50 nm.

[0179] Example 28

[0180] The method is basically the same as Example 1, except that step S5 is not performed, that is, no protective layer is prepared on the second copper layer.

[0181] Example 29

[0182] The method is basically the same as Example 1, except that in step S1, the first copper layer is only prepared on one surface of the PET film in the thickness direction.

[0183] Comparative Example 1

[0184] The method is basically the same as Example 1, except that: Step S2 and Step S3 are omitted; in Step S4, a second copper layer is prepared on the product obtained in Step S1 by electroplating, and the second copper layer is located on the surface of the first copper layer.

[0185] Comparative Example 2

[0186] It is basically the same as Example 28, except that: step S2 and step S3 are omitted; in step S4, a second copper layer is prepared on the product obtained in step S1 by electroplating, and the second copper layer is located on the surface of the first copper layer.

[0187] Performance Testing

[0188] The finished or semi-finished composite copper current collectors prepared in each embodiment and each comparative example were tested using the following test methods:

[0189] (1) Defect rate test method: Place a composite copper current collector sample with an area of ​​A0 in a surface quality detection system (micro-visual charge coupled device CCD), scan the sample surface, and then convert the optical signal into an electrical signal and transmit it to a computer. The defect area of ​​the sample is counted and recorded as A1. The defect rate is (A0 / A1)×100%.

[0190] (2) Square resistance test method: Place a flat composite copper current collector sample on a sample table and use a four-probe square resistance meter to test the square resistance of the sample.

[0191] (3) Test method for the adhesion between the polymer substrate layer and the first copper layer: a layer of Permacel P-94 double-sided tape was adhered to a 1 mm thick aluminum foil, a composite copper current collector sample was adhered on top of the double-sided tape, and a layer of ethylene acrylic acid copolymer film (DuPont Nurcel0903, thickness of 50 μm) was covered on the sample, and then the first copper layer was placed on a 1.3 × 10 5 N / m 2 , hot press at 120℃ for 10s, cool to room temperature, and cut into 150mm×15mm strips. Finally, fix the ethylene acrylic acid copolymer film of the sample strip to the upper fixture of the tensile machine, and fix the rest of the film to the lower fixture. After fixing, the two are fixed at 180 o The layers were peeled off at an angle of 100 mm / min and a speed of 100 mm / min, and the peeling force was tested to obtain the bonding force between the polymer substrate layer and the first copper layer.

[0192] (4) Surface morphology testing method: The surface morphology of the composite copper current collector was observed using a field emission electron microscope (Zeiss Gemini Sigma300VP SEM).

[0193] (5) Test method for the thickness of the anti-adhesive functional layer: The product obtained in step S2 is prepared according to the requirements of focused ion beam microscopy (FIB-SEM) sample preparation, and then the sample is placed in a FIB-SEM (Zeiss Gemini2 Crossbeam). The sample surface is bombarded with an ion beam to prepare a cross-sectional sample. The surface position of the prepared cross-sectional sample is then magnified and observed, and the thickness of the anti-adhesive functional layer is measured using the measurement software provided with the electron microscope.

[0194] Table 1 Product parameters and performance test results

[0195] Observe Table 1, Example 1 is processed with step S2 and step S3 relative to Comparative Example 1. It can be seen from Example 1 and Comparative Example 1 that: compared with the composite copper current collector prepared in Comparative Example 1, the composite copper current collector prepared in Example 1 of the present application has no defects, and the performance such as square resistance and adhesion is significantly improved, and the performance of the composite copper current collector prepared by long-term operation is relatively stable. In addition, in conjunction with Figures 3-4, the surface morphology of the composite copper current collector prepared in Example 1 is defect-free, which is significantly improved relative to the composite copper current collector prepared in Comparative Example 1. Compared with Comparative Example 2, Example 28 is processed with step S2 and step S3, and the defect rate of the second copper layer and the square resistance of the composite copper current collector of Example 28 are significantly reduced, the adhesion between the polymer substrate layer and the first copper layer is significantly improved, and the performance of the composite copper current collector prepared by long-term operation is relatively stable. In summary, the present application reduces the defect rate of the second copper layer and the square resistance of the composite copper current collector by setting a second copper layer on the surface of the first copper layer, while improving the adhesion between the polymer substrate layer and the first copper layer.

[0196] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0197] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.

Claims

1. A composite copper current collector, comprising a polymer substrate layer, wherein a first copper layer is disposed on at least one side of the polymer substrate layer, a second copper layer is disposed on a side of the first copper layer away from the polymer substrate layer, and a defect rate of the second copper layer is less than or equal to 5%.

2. The composite copper current collector according to claim 1, wherein: The defect rate of the second copper layer is less than or equal to 2%, and can be optionally 0-0.5%.

3. The composite copper current collector according to claim 1 or 2, wherein: The bonding force between the polymer substrate layer and the first copper layer is greater than or equal to 0.9 N / cm, and can be optionally 0.9 N / cm-10 N / cm.

4. The composite copper current collector according to any one of claims 1 to 3, wherein: The square resistance of the composite copper current collector is less than or equal to 29 mΩ, and can be less than or equal to 24 mΩ.

5. The composite copper current collector according to any one of claims 1 to 4, wherein: The composite copper current collector has one or more of the following characteristics: (1a) the thickness of the second copper layer is 500nm-2000nm, and can be optionally 700nm-1200nm; (1b) the thickness of the first copper layer is greater than or equal to 50 nm, and can be selected from 50 nm to 500 nm; (1c) The thickness of the polymer substrate layer is 1.5 μm to 10 μm.

6. The composite copper current collector according to any one of claims 1 to 5, wherein: The polymer substrate layer includes one or more of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyimide.

7. The composite copper current collector according to any one of claims 1 to 6, wherein: The composite copper current collector further comprises a protective layer, wherein the protective layer is located on a surface of the second copper layer on a side away from the first copper layer; Optionally, the thickness of the protective layer is 10nm-100nm, and further optionally 30nm-60nm; Optionally, the protective layer includes one or more of chromium oxide, copper chromium oxide, copper-organic acid complex, copper-imidazole complex, polysiloxane, nickel, chromium, nickel-chromium alloy, nickel oxide, graphite, carbon black, acetylene black, Ketjen black, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers and graphene.

8. The method for preparing the composite copper current collector according to any one of claims 1 to 7, comprising the following steps: preparing the first copper layer on at least one side of the polymer substrate layer; Prepare an anti-adhesive functional layer on a side of the first copper layer away from the polymer substrate layer, wherein the anti-adhesive functional layer comprises one or more of a metal and a metal oxide; removing the anti-adhesive functional layer; The second copper layer is prepared on the surface of the first copper layer from which the anti-adhesion functional layer is removed.

9. The preparation method according to claim 8, wherein: The thickness of the anti-adhesive functional layer is greater than or equal to 5 nm, and can be selected from 10 nm to 50 nm; Optionally, the metal includes one or more of aluminum, magnesium, titanium, zinc and nickel; Optionally, the metal oxide includes one or more of aluminum oxide, magnesium oxide, copper oxide, cuprous oxide, nickel oxide, zinc oxide and aluminum-doped zinc oxide.

10. The preparation method according to claim 8 or 9, wherein: In the step of preparing the anti-adhesive functional layer on the side of the first copper layer away from the polymer substrate layer, the anti-adhesive functional layer is prepared by magnetron sputtering.

11. The preparation method according to claim 10, wherein: The process conditions of the magnetron sputtering method include one or more of the following conditions: (2a) The target material for magnetron sputtering includes one or more of the metal and the metal oxide; (2b) The gas source for magnetron sputtering includes argon gas; (2c) The gas source for magnetron sputtering includes argon gas, and the flow rate of the argon gas is less than or equal to 500 mL / min; (2d) The gas source for magnetron sputtering includes oxygen; (2e) The gas source for magnetron sputtering includes oxygen, and the flow rate of the oxygen is less than or equal to 100 mL / min; (2f) The pressure in the magnetron sputtering chamber is less than or equal to 0.6 Pa; (2g) The power density of magnetron sputtering is 10W / cm 2 -150W / cm 2 ; (2h) The magnetron sputtering time is greater than or equal to 5s.

12. The preparation method according to any one of claims 8 to 11, wherein: In the step of removing the anti-adhesive functional layer, an acid solution is used to dissolve and remove the anti-adhesive functional layer; Optionally, the acid solution includes one of hydrochloric acid, sulfuric acid, nitric acid, a mixture of sulfuric acid and hydrochloric acid, and a mixture of sulfuric acid and nitric acid; Optionally, the pH of the acid solution is less than or equal to 2; Optionally, the dissolution time is greater than or equal to 10 s.

13. The preparation method according to any one of claims 8 to 12, wherein: In the step of preparing the first copper layer on at least one side of the polymer substrate layer, the first copper layer is prepared on at least one side of the polymer substrate layer by using a physical vapor deposition method.

14. The preparation method according to any one of claims 8 to 13, wherein: In the step of removing the surface of the first copper layer of the anti-adhesive functional layer to prepare the second copper layer, the second copper layer is prepared by electroplating; Optionally, the electroplating solution used to prepare the second copper layer by the electroplating method includes 100g / L-180g / L copper sulfate, 60g / L-120g / L sulfuric acid, 40g / L-100mg / L hydrochloric acid and electroplating solution additives; further optionally, the electroplating The liquid additives include 1mg / L-50mg / L leveler, 100mg / L-700mg / L inhibitor and 0.5mg / L-10mg / L brightener; more optionally, the leveler includes an organic amine compound, the inhibitor includes a polyethylene glycol compound, and the brightener includes an organic sulfur compound; Optionally, the process conditions for preparing the second copper layer by electroplating include: the temperature of the electroplating solution is 20°C-40°C, the average cathode current density is 1A / dm 2 -5A / dm 2 , the electroplating time is 2min-15min.

15. A negative electrode plate, comprising the composite copper current collector according to any one of claims 1 to 7 or the composite copper current collector prepared by the preparation method according to any one of claims 8 to 14.

16. A battery comprising the negative electrode sheet according to claim 15.

17. An electrical device comprising the battery according to claim 16.

Citation Information

Patent Citations

  • Bipolar current collector, preparation method thereof and battery

    CN114430044A

  • Negative current collector for lithium ion battery and preparation method of negative current collector

    CN115911402A

  • Copper-plated film for battery

    CN212404283U

  • Copper foil for lithium secondary battery collector, and display method thereof, negative electrode for lithium secondary battery using copper foil, and lithium secondary battery

    JP2013187114A

Cited By

  • Composite copper current collector and preparation method and application thereof

    CN120834213A

  • Composite current collector and preparation method thereof, lithium metal battery and electric equipment

    CN120933382A