Resin composition, prepreg, resin film, metal-clad laminated plate, printed wiring board, and semiconductor package
The resin composition with a curable prepolymer of 50,000 or more molecular weight, containing vinylbenzyl and indene rings, addresses adhesion issues in stacked prepregs, enhancing tackiness and moldability, and achieving low dielectric properties for high-frequency applications in electronic devices.
Patent Information
- Application Number
- PCT/JP2024/018831
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
Resin compositions with vinylbenzyl compounds used in high-frequency applications tend to adhere strongly when stacked, making it difficult to peel off prepregs and reducing workability and formability of metal-clad laminates, leading to concerns about transmission loss in electronic devices.
A resin composition with a curable prepolymer containing vinylbenzyl groups and indene rings, having a weight average molecular weight of 50,000 or more, which improves tackiness and moldability, reducing adhesion and layer separation in cured products.
The resin composition enhances the tackiness of coated products and moldability of cured products, such as metal-clad laminates, while maintaining low dielectric constants and loss tangents, suitable for high-frequency applications, improving the manufacturing process and performance of electronic components.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin composition, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package
[0001] The present disclosure relates to a resin composition, a prepreg, a resin film, a metal-clad laminate, a printed wiring board, and a semiconductor package.
[0002] Metal-clad laminates, such as copper-clad laminates, prepregs that can be used with metal-clad laminates, and semiconductor packages that use metal-clad laminates are used in a variety of electronic devices, including mobile communication devices such as smartphones, their base station equipment, servers, routers, large servers, and other network infrastructure devices, as well as large computers, personal computers, and industrial computers. They are also used in electronic devices installed in home appliances, automobiles, and other devices. With the spread of 5G, there is a growing demand for electronic communication devices to process massive amounts of data at high speeds.
[0003] When electronic devices process huge amounts of data at high speed, they require circuit board materials with low transmission loss in the high-frequency range. While resins with low dielectric constants and low dielectric loss tangents are used as circuit board materials and provide circuit boards with low transmission loss, recent advances in communication technology have created a demand for the development of resins with even lower dielectric constants and dielectric loss tangents.
[0004] Patent Document 1 discloses a thermosetting resin composition containing a vinylbenzyl compound and a polycarbodiimide compound as a material for electronic components for use in high frequency bands, and proposes that the resulting electronic components have improved adhesion to metal materials while maintaining excellent dielectric properties.
[0005] Japanese Patent Application Laid-Open No. 2007-119531
[0006] The speed and capacity of signals used in mobile communication devices such as smartphones, their base station equipment, servers, routers and other network infrastructure equipment, and electronic devices such as large computers are increasing year by year. As a result, the printed wiring boards used in these electronic devices must be able to handle higher frequencies, and dielectric properties that can reduce transmission loss are required, resulting in a demand for board materials with low dielectric constants and low dielectric dissipation factors.
[0007] Patent Document 1 discloses a resin composition containing a vinylbenzyl compound and a polycarbodiimide compound, which has dielectric properties suitable for high-frequency band applications. However, further investigation by the present inventors revealed that when multiple prepregs or resin films formed using such a resin composition containing a vinylbenzyl compound are stacked, they tend to adhere to each other and become difficult to peel. This raises concerns about reduced workability in transporting prepregs and manufacturing metal-clad laminates. Furthermore, there is room for improvement in the formability of metal-clad laminates.
[0008] An object of the present disclosure is to provide a resin composition that improves the tackiness of a coated product and the moldability of a cured product, and a prepreg, a resin film, a metal-clad laminate, a printed wiring board, and a semiconductor package obtained using the resin composition.
[0009] The present disclosure includes the following embodiments. The present disclosure is not limited to the following embodiments. One embodiment relates to a resin composition comprising a curable prepolymer that contains a vinylbenzyl group and an indene ring and has a weight average molecular weight of 50,000 or more.
[0010] The present disclosure can provide a resin composition that improves the tackiness of a coated product and the moldability of a cured product, as well as a prepreg, a resin film, a metal-clad laminate, a printed wiring board, and a semiconductor package obtained using the resin composition.
[0011] Hereinafter, embodiments of the present disclosure will be described in detail, but the present invention is not limited to the following embodiments.
[0012] In the present disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit of a certain numerical range may be replaced with the upper or lower limit of another numerical range. Furthermore, the upper or lower limit of a numerical range described in the present disclosure may be replaced with a value shown in the examples. In the present disclosure, unless otherwise specified, each component may contain one or more corresponding substances. In the present disclosure, when a resin composition contains multiple substances corresponding to each component, the content of each component in the resin composition means the total amount of the multiple substances present in the resin composition, unless otherwise specified.
[0013] In this disclosure, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values measured by the following procedure. The weight average molecular weight and number average molecular weight are converted from a calibration curve using standard polystyrene by gel permeation chromatography (GPC). The calibration curve is approximated by a cubic equation using a set of five standard polystyrene samples (PStQuick MP-H, PStQuick B [product name, Tosoh Corporation]). The GPC conditions are shown below.
[0014] Apparatus: High-speed GPC apparatus "HLC-8320GPC" (Tosoh Corporation, trade name) Detector: Ultraviolet absorption detector "UV-8320" (Tosoh Corporation, trade name) Columns: Guard column; TSKgel guard column Super (HZ)-M+, column; TSKgel SuperMultipore HZ-M (2 columns), reference column; TSKgel Super H-RC (2 columns) (all Tosoh Corporation, trade names) Column size: 4.6 x 20 mm (guard column), 4.6 x 150 mm (column), 6.0 x 150 mm (reference column) Eluent: Tetrahydrofuran Sample concentration: 10 mg / 1 mL Injection volume: 20 μL or 2 μL Flow rate: 0.35 mL / min Measurement temperature: 40°C
[0015] "Resin composition" The resin composition of one embodiment contains a curable prepolymer that contains a vinylbenzyl group and an indene ring and has a weight-average molecular weight of 50,000 or more. Hereinafter, the curable prepolymer that contains a vinylbenzyl group and an indene ring and has a weight-average molecular weight of 50,000 or more may be simply referred to as a curable prepolymer.
[0016] The curable prepolymer is a prepolymer in which a portion of the vinylbenzyl group having a polymerizable reactive group remains without contributing to the polymerization reaction. Because the curable prepolymer has a vinylbenzyl group, a cured product can be obtained by accelerating curing using heat, pressure, a curing accelerator, or the like. In order to make the curable prepolymer moldable by coating it on a substrate or the like, it is preferable that the curable prepolymer itself is liquid, or that the curable prepolymer is dissolved or dispersed in a solvent to form a liquid composition.
[0017] The weight-average molecular weight (Mw) of the curable prepolymer is preferably 50,000 or more, more preferably 100,000 or more, 150,000 or more, or 300,000 or more. Within these ranges, the surface tackiness of a coated product of the resin composition can be more appropriately suppressed. For example, the tackiness of coated products such as prepregs and resin films can be further improved. When mixed with other components, the compatibility between the curable prepolymer and elastomers, etc. can be more favorably maintained. Furthermore, resin separation can be more effectively suppressed when a coated product of the resin composition is cured. For example, resin layer separation can be more effectively suppressed in cured products such as metal-clad laminates.
[0018] The weight-average molecular weight (Mw) of the curable prepolymer is not particularly limited, but may be, for example, 500,000 or less. From the viewpoint of suppressing gelation of the resin composition and coatability, the weight-average molecular weight (Mw) of the curable prepolymer may be 250,000 or less, 200,000 or less, or 150,000 or less. Furthermore, within these ranges, there is also the advantage that the solution viscosity of the synthesis system can be maintained at a good level when synthesizing the curable prepolymer.
[0019] For example, the weight average molecular weight (Mw) of the curable prepolymer may be 50,000 or more and 500,000 or less, 100,000 or more and 250,000 or less, or 150,000 or more and 200,000 or less. On the other hand, from the viewpoint of the tackiness of the coated product and the moldability of the cured product, the weight average molecular weight (Mw) of the curable prepolymer is preferably 150,000 or more and 500,000 or less, or 300,000 or more and 500,000 or less. The method for measuring the weight average molecular weight (Mw) of the curable prepolymer conforms to the method described above.
[0020] The curable prepolymer contains a vinylbenzyl group and an indene ring. Examples of the curable prepolymer include a prepolymer containing a structural unit having a vinylbenzyl group and a structural unit having an indene ring, a prepolymer containing a vinylbenzyl group and an indene ring as substituents in the skeleton of the prepolymer, a prepolymer containing a structural unit having a vinylbenzyl group and containing an indene ring as a substituent in the skeleton of the prepolymer, a prepolymer containing a structural unit having an indene ring and containing a vinylbenzyl group as a substituent in the skeleton of the prepolymer, a prepolymer containing a structural unit having an indene ring and containing a vinylbenzyl group as a substituent in the skeleton of the prepolymer, and a prepolymer containing a structural unit having a vinylbenzyl group and an indene ring.
[0021] The curable prepolymer is preferably a prepolymer containing a structural unit having a vinylbenzyl group and an indene ring, and more preferably a prepolymer containing a structural unit having an indene ring and a vinylbenzyl group directly bonded to a carbon atom of the indene ring.
[0022] In the curable prepolymer, the indene ring may be unsubstituted or may have a substituent. For example, the indene ring is represented by the following formula (1):
[0023]
[0024] In formula (1), R 1 and R 4 R are each independently a hydrogen atom, a halogen atom, a monovalent organic group, or a group having a bonding site with another structure. 1 and R 4The monovalent organic group represented by the formula (1) may be an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a thioalkoxy group having 1 to 5 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an arylalkyl group having 7 to 20 carbon atoms. The halogen atom may be a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom. In formula (1), R 1 and R 4 At least one of R may be a vinylbenzyl group. 1 and R 4 At least one of the R is a group having a bonding site with another structure. 1 and R 4 may be all the same, or some or all of them may be different. The benzene ring of the indene ring may be unsubstituted.
[0025] Furthermore, the R present in the curable prepolymer 1 and R 4 At least one of the groups may be an arylalkyl group other than a vinylbenzyl group, and the arylalkyl group may not have a polymerizable unsaturated bond.
[0026] The indene ring may be represented by the following formula (1a):
[0027] In formula (1a), R 1 and R 4 may each independently be one of those listed in formula (1) above, and R 2 and R 3 are each independently R in the above formula (1). 1 R 1 ~R 3 may be all the same, or may be partially or completely different. 4 may all be the same, or some or all may be different. The benzene ring of the indene ring may be unsubstituted.
[0028] In the curable prepolymer, the vinylbenzyl group may be unsubstituted or may have a substituent. For example, the vinylbenzyl group is represented by the following formula (2):
[0029]
[0030] In formula (2), R 5 is a hydrogen atom, a halogen atom, or a monovalent organic group. 5 The monovalent organic group represented by the formula (I) may be an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a thioalkoxy group having 1 to 5 carbon atoms, or an aryl group having 6 to 20 carbon atoms. The halogen atom may be a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom. 5 may all be the same, or some or all may be different. The vinylbenzyl group may be unsubstituted.
[0031] The curable prepolymer is represented by the formula (1), where R 1 At least one of R may be a vinylbenzyl group. 1 At least one of the groups may be a group containing a bonding site with another structure. 1 At least one of R is a vinylbenzyl group, and the remaining R 1 At least one of the groups may be a group containing a bonding site to another structure.
[0032] Furthermore, the R present in the curable prepolymer 1 At least one of the groups may be an arylalkyl group other than a vinylbenzyl group, and the arylalkyl group may not have a polymerizable unsaturated bond.
[0033] The curable prepolymer may comprise a structure having a methylphenyl group, an indenyl group bonded to the methyl group of the methylphenyl group, and a vinylbenzyl group further bonded to the indenyl group, or may comprise a structure having a methylphenyl group, an indenyl group bonded to the methyl group of the methylphenyl group at any one of the 1-, 2-, and 3-positions, and a vinylbenzyl group bonded to at least one of the remaining 1-, 2-, and 3-positions of the indenyl group.
[0034] The curable prepolymer may include a structure having a methylphenyl group, an indenyl group bonded to the methyl group of the methylphenyl group, and a vinylbenzyl group further bonded to the indenyl group, or a structure having a methylphenyl group, an indenyl group bonded to the methyl group of the methylphenyl group, and an arylalkyl group other than a vinylbenzyl group further bonded to the indenyl group, and the arylalkyl group may be one that does not have a polymerizable unsaturated bond. The curable prepolymer may include a structure having a methylphenyl group, an indenyl group bonded to the methyl group of the methylphenyl group at any one of the 1-, 2-, and 3-positions, and a vinylbenzyl group bonded to at least one of the remaining 1-, 2-, and 3-positions of the indenyl group, or a structure having a methylphenyl group, an indenyl group bonded to the methyl group of the methylphenyl group at any one of the 1-, 2-, and 3-positions, and an arylalkyl group other than a vinylbenzyl group bonded to at least one of the remaining 1-, 2-, and 3-positions of the indenyl group, wherein the arylalkyl group may not have a polymerizable unsaturated bond.
[0035] The 1st, 2nd and 3rd positions of the indenyl group and indene ring are as shown below.
[0036]
[0037] For example, the curable polymer may include a structural unit represented by formula (3):
[0038]
[0039] In formula (3), R 6 is an unsubstituted or substituted indenyl group. 5 may be those listed in formula (2). 5 may be partially or entirely hydrogen atoms. For example, the curable polymer may contain a structural unit represented by the following formula (4):
[0040]
[0041] In formula (4), R 1 and R 4 may each independently be as recited in formula (1), and R5 may be those listed in formula (2). 1 At least one of R may be an unsubstituted or substituted vinylbenzyl group. 1 At least one of R may be a group having a bonding site with another structure. 4 and R 5 may be partially or entirely hydrogen atoms.
[0042] Furthermore, the R present in the curable prepolymer 1 At least one of the groups may be an arylalkyl group other than a vinylbenzyl group, and the arylalkyl group may not have a polymerizable unsaturated bond.
[0043] The curable prepolymer may be a polymer of a monomer. Examples of the monomer include a monomer having one or more vinylbenzyl groups, a monomer having one or more indene rings, and a monomer having one or more vinylbenzyl groups and one or more indene rings. The polymerization may be terminated without being completed, but at a state where a certain amount of vinylbenzyl groups derived from the monomer remain. For example, to obtain a liquid curable prepolymer, the polymerization may be terminated at a state where the viscosity of the polymerization reaction system of the curable prepolymer reaches a certain level. An oligomer may be used together with or instead of the monomer.
[0044] The curable prepolymer may be, for example, a polymer containing structural units derived from a vinylbenzyl compound having a vinylbenzyl group and an indene ring in one molecule. This vinylbenzyl compound may be a monomer, an oligomer, or a combination thereof, but from the viewpoint of molecular design, a monomer is preferred. Hereinafter, a vinylbenzyl compound having a vinylbenzyl group and an indene ring may be simply referred to as a vinylbenzyl compound. The curable prepolymer may contain only structural units derived from the same vinylbenzyl compound, or may contain structural units derived from multiple types of vinylbenzyl compounds.
[0045] The vinylbenzyl compound may be a compound having one or more vinylbenzyl groups and one or more indene rings in one molecule, a compound having one or more vinylbenzyl groups and one indene ring in one molecule, or a compound having 1 to 3 vinylbenzyl groups and one indene ring in one molecule. The vinylbenzyl compound may be a compound in which a vinylbenzyl group is directly bonded to a carbon atom of an indene ring.
[0046] The vinylbenzyl compound may be a compound having one or more vinylbenzyl groups, one or more indene rings, and one or more arylalkyl groups other than vinylbenzyl groups in one molecule. It may also be a compound having one or more vinylbenzyl groups, one indene ring, and one or more arylalkyl groups other than vinylbenzyl groups in one molecule. The vinylbenzyl compound may be a compound in which a vinylbenzyl group and an arylalkyl group other than a vinylbenzyl group are directly bonded to a carbon atom of an indene ring. The arylalkyl group other than a vinylbenzyl group may not have a polymerizable unsaturated bond.
[0047] The curable prepolymer may be a polymer containing a structural unit derived from a compound having an indene ring and having 1 to 3 vinylbenzyl groups bonded to any one of the 1-, 2-, and 3-positions of the indene ring, or may be a polymer containing a structural unit derived from a compound having 2 to 3 vinylbenzyl groups bonded to the 1-, 2-, and 3-positions of the indene ring.
[0048] The curable prepolymer may also be a polymer containing a structural unit derived from a compound having an indene ring, one or two vinylbenzyl groups bonded to any one of the 1-, 2-, or 3-positions of the indene ring, and one or two arylalkyl groups other than vinylbenzyl groups bonded to any one of the 1-, 2-, or 3-positions of the indene ring. Furthermore, the curable prepolymer may be a polymer containing both a structural unit derived from a compound having an indene ring, one to three vinylbenzyl groups bonded to any one of the 1-, 2-, or 3-positions of the indene ring, and no arylalkyl groups other than vinylbenzyl groups, and a structural unit derived from a compound having an indene ring, one or two vinylbenzyl groups bonded to any one of the 1-, 2-, or 3-positions of the indene ring, and one or two arylalkyl groups other than vinylbenzyl groups bonded to any one of the 1-, 2-, or 3-positions of the indene ring.
[0049] In polymerization using such a monomer, if a curable prepolymer is obtained in a state where the polymerization is not completely completed, some of the vinylbenzyl groups of the monomer will contribute to the polymerization in the curable prepolymer and form the skeleton of the prepolymer, while other parts of the vinylbenzyl groups of the monomer will not contribute to the polymerization and will exist as vinylbenzyl groups in the curable prepolymer.
[0050] In the vinylbenzyl compound, the indene ring and the vinylbenzyl group may be unsubstituted or may have a substituent. The substituent on the indene ring may be R 1 and R 4 The substituent of the vinylbenzyl group may be any of those listed in the above formula (3) R 5 It may be one of those listed above.
[0051] The vinylbenzyl compound may be a compound represented by the following formula (5-1) or (5-2).
[0052]
[0053] In formula (5-1), n is an integer of 1 to 3. n is more preferably 2 or 3, and more preferably 2. Note that the resin composition containing a curable prepolymer may contain a curable prepolymer that is a copolymer of multiple types of monomers with different n's. In this case, n is preferably 1 to 3 on average, more preferably 2 to 3, and even more preferably 2.0 to 2.5. Note that in formula (5-1), the indene ring and the vinylbenzyl group may each have a substituent.
[0054] In formula (5-1), the vinylbenzyl group may be directly bonded to any of the carbon atoms at the 1-, 2-, and 3-positions of the indene ring, but is preferably bonded to the 1-position or a combination of the 1- and 3-positions. One or two vinylbenzyl groups may be bonded to each position. For example, the vinylbenzyl groups may be bonded to a combination of the 1-, 1'-, and 3-positions of the indene ring, or a combination of the 1- and 1'-positions of the indene ring.
[0055] In formula (5-1), the methyl group of the vinylbenzyl group may be in any of the o-, m-, and p-positions, but is preferably in the m- or p-position. When the polymer is obtained using two or more types of monomers, it may be a mixture of the o-, m-, and p-forms. In this case, a combination of the m- and p-forms is preferred, and the mass ratio of the m- to p-forms is preferably 40:60 to 60:40.
[0056] In formula (5-2), R 7 is a hydrogen atom or a saturated hydrocarbon group having 1 to 6 carbon atoms. 7 may be an alkyl group having 1 to 3 carbon atoms. Hereinafter, the following structural portion in formula (5-2) may be referred to as an "arylalkyl group".
[0057]
[0058] In formula (5-2), p is an integer of 1 to 3, q is 0, 1, or 2, and p + q is an integer of 1 to 3. The resin composition containing a curable prepolymer may contain a curable prepolymer that is a copolymer of multiple types of monomers with different p and q. In this case, p is preferably 1 to 3 on average, more preferably 2 to 3, and even more preferably 2.0 to 2.5. Furthermore, q is preferably 0.3 to 1 on average, and even more preferably 0.5 to 0.8. In formula (5-2), the indene ring, vinylbenzyl group, and arylalkyl group may each have a substituent.
[0059] In formula (5-2), the vinylbenzyl group and the arylalkyl group may be directly bonded to any one of the carbon atoms at the 1st, 2nd, and 3rd positions of the indene ring.
[0060] In formula (5-2), the methyl group of the vinylbenzyl group may be in any of the o-, m-, and p-positions, but is preferably in the m- or p-position. When the polymer is obtained using two or more types of monomers, it may be a mixture of the o-, m-, and p-forms. In this case, a combination of the m- and p-forms is preferred, and the mass ratio of the m- to p-forms is preferably 40:60 to 60:40.
[0061] The curable prepolymers exemplified above may be homopolymers or copolymers. The homopolymer may be a homopolymer of a unit having a vinylbenzyl group and an indene ring. The copolymer may be a copolymer containing two or more units having a vinylbenzyl group and an indene ring, a copolymer containing one or more units each containing a vinyl group and one or more units containing an indene ring, or a copolymer of these copolymers with other units. In order to achieve a lower dielectric constant and a lower dielectric dissipation factor, the curable prepolymer may contain no units other than the unit having a vinylbenzyl group and an indene ring, the unit having a vinylbenzyl group, and the unit having an indene ring. From this perspective, the total amount of the unit having a vinylbenzyl group and an indene ring, the unit having a vinylbenzyl group, and the unit having an indene ring in the curable prepolymer is preferably 50% by mass or more, more preferably 60% by mass or more, 80% by mass or more, or even 90% by mass or more, based on the total mass of the curable prepolymer. In particular, in the curable prepolymer, the total amount of units having a vinylbenzyl group and an indene ring is preferably 50 mass % or more, more preferably 60 mass % or more, 80 mass % or more, or even 90 mass % or more, relative to the total mass of the curable prepolymer.
[0062] The curable prepolymers exemplified above may have a substituent, but since the curable prepolymer is more preferably a hydrocarbon compound, the curable prepolymer does not need to have a polar group. Examples of polar groups include an ester bond (-CO-O-) and an ether bond (-C-O-). Furthermore, from the viewpoint of dielectric properties, the curable prepolymer does not need to contain a heteroatom. Examples of heteroatoms include an oxygen atom, a nitrogen atom, and a sulfur atom. In particular, it is preferable that the curable prepolymer does not contain an oxygen atom.
[0063] A method for synthesizing a curable prepolymer will be described below. The curable prepolymer can be obtained, for example, by polymerizing a compound containing a vinylbenzyl group and an indene ring. In another example, the curable prepolymer can be obtained by copolymerizing a compound having a vinylbenzyl group with a compound having an indene ring. In yet another example, the curable prepolymer can be obtained by introducing a vinylbenzyl group and an indene ring into a polymer skeleton. A method for polymerizing a compound containing a vinylbenzyl group and an indene ring will be described below. Note that the curable prepolymer is not limited to those synthesized by these synthesis methods.
[0064] First, an example of a method for synthesizing a vinylbenzyl compound will be described. Among vinylbenzyl compounds, a method for synthesizing a vinylbenzyl compound represented by the aforementioned formula (5-1) includes, for example, a method of reacting indene with a styrene having a halogenated methyl group in the presence of a basic compound. Examples of the styrene having a halogenated methyl group include o-chloromethylstyrene, m-chloromethylstyrene, and p-chloromethylstyrene, and these may be used alone or in a mixture of two or more. The ratio of the styrene having a halogenated methyl group to 1 mole of indene may be, for example, in the range of 1 to 3 moles, 2 to 3 moles, or 2.0 to 2.5 moles. Examples of the basic compound include alkali metal hydroxides and alkali metal alkoxides.
[0065] Furthermore, among vinylbenzyl compounds, a method for synthesizing the vinylbenzyl compound represented by the aforementioned formula (5-2) can be, for example, a method in which indene, a styrene having a halogenated methyl group, and an aryl compound having a halogenated methyl group (excluding styrene having a halogenated methyl group) are reacted in the presence of a basic compound. Examples of the styrene having a halogenated methyl group include those mentioned above, and these may be used alone or in a mixture of two or more. Examples of the aryl compound having a halogenated methyl group include α-chlorotoluene and α-chloro-p-xylene. The ratio of the styrene having a halogenated methyl group to 1 mole of indene may be, for example, in the range of 1 to 3 moles, 2 to 3 moles, or 2.0 to 2.5 moles. The ratio of the aryl compound having a halogenated methyl group to 1 mole of indene may be, for example, in the range of 0.3 to 1 mole, or 0.5 to 0.8 moles. The total number of moles of the styrene having a halogenated methyl group and the aryl compound having a halogenated methyl group per mole of indene may be in the range of 1.5 to 3 moles, or may be in the range of 2 to 3 moles, or may be in the range of 2.5 to 2.9 moles. Examples of the basic compound include those mentioned above.
[0066] A phase transfer catalyst may be used in the above reaction. Examples of the phase transfer catalyst include tetra-n-butylammonium bromide. The reaction may be carried out by solution polymerization. The reaction may be carried out, for example, under heating and stirring. A polymerization inhibitor may be added to the reaction system. The obtained product may be purified, if necessary, by known methods such as concentration, reprecipitation, and washing.
[0067] In the method for synthesizing a curable prepolymer, the vinylbenzyl compound may be used alone or in combination of two or more. For example, in the method for synthesizing the vinylbenzyl compound represented by the above formula (5-1) or (5-2), a compound in which a vinylbenzyl group is directly bonded to at least one carbon atom at the 1st, 2nd, and 3rd positions of an indene ring is synthesized, but the compound may also be provided as a mixture of two or more isomeric vinylbenzyl compounds having different bonding sites.
[0068] Next, a method for obtaining a curable prepolymer by polymerizing a vinylbenzyl compound will be described. The polymerization of the vinylbenzyl compound is preferably carried out by radical polymerization so as not to generate polar components in the reaction product. The radical polymerization can be carried out using a radical polymerization initiator. The polymerization can be carried out by solution polymerization, and the polymerization solvent is not particularly limited. For example, one or a combination of two or more organic solvents used in the resin composition described below may be used as the polymerization solvent.
[0069] The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator, but is preferably a thermal radical polymerization initiator. The radical polymerization initiator is not particularly limited, and examples thereof include an azo-based polymerization initiator and an organic peroxide-based polymerization initiator.
[0070] Examples of the azo polymerization initiator include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylpropanenitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylpropionate)dimethyl, 1,1'-azobis(methyl cyclohexylcarboxylate), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 4,4'-azobis(3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl 4-cyanopentanoate), and 1,1'-azobis(cyclohexane-1-carbonitrile).
[0071] Examples of the organic peroxide polymerization initiator include dicumyl peroxide, dibenzoyl peroxide, 2-butanone peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, bis(tert-butylperoxyisopropyl)benzene, and tert-butyl hydroperoxide.
[0072] In order to prevent the incorporation of polar components into the resin composition, it is advisable to reduce the generation of polar by-products in the polymerization system. From this perspective, it is advisable to use a compound with a small amount of oxygen atoms among radical polymerization initiators. As such a compound, an azo-based polymerization initiator is preferred. Among these, it is preferable that the azo-based polymerization initiator is a compound that does not contain any heteroatoms other than the two nitrogen atoms (N) of the azo group. For example, a compound represented by the following formula (6) can be mentioned.
[0073] R 11 -N=N-R 12 (6)
[0074] In formula (6), R 11 and R 12 are each independently a hydrogen atom or a monovalent functional group, and R 11 and R 12 At least one of R is a monovalent functional group. 11 and R 12 may be the same or different. The monovalent functional group is preferably a hydrocarbon group, and may be a saturated or unsaturated hydrocarbon group, or may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The monovalent functional group is preferably a saturated or unsaturated aliphatic hydrocarbon group, and is preferably an alkyl group.
[0075] The alkyl group may be either a chain alkyl group or a cyclic alkyl group. The chain alkyl group may be a straight-chain alkyl group or a branched alkyl group. The cyclic alkyl group may have a substituent bonded to a carbon atom on the ring.
[0076] The alkyl group may be, for example, an alkyl group having 1 to 10 carbon atoms, 3 to 8 carbon atoms, or 4 to 8 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, an n-hexyl group, an isohexyl group, a cyclohexyl group, a methylcyclohexyl group, a cyclohexylmethyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a nonyl group, a decyl group, a 1,1',3,3'-tetramethylbutyl group, and a 2,2',4,4'-tetramethylbutyl group.
[0077] Specific examples of the compound represented by formula (6) include 2,2'-azobis(2,4,4-trimethylpentane) and 2,2'-azobis(2,4-dimethylvaleronitrile).
[0078] The amount of the radical polymerization initiator used may be adjusted appropriately depending on the desired degree of polymerization of the curable prepolymer. Furthermore, the amount of the radical polymerization initiator used may be adjusted appropriately depending on the functionality of the vinylbenzyl group of the vinylbenzyl compound, etc. For example, the amount of the radical polymerization initiator used may be 0.01 to 5 parts by mass, 0.1 to 4 parts by mass, or 0.5 to 2 parts by mass relative to 100 parts by mass of the vinylbenzyl compound content of the polymerization system.
[0079] In the reaction of polymerizing a curable prepolymer from a vinylbenzyl compound, a polymerization inhibitor, a chain transfer agent, etc. may be used from the viewpoint of adjusting the degree of polymerization of the curable prepolymer and leaving an effective amount of unreacted vinylbenzyl groups in the curable prepolymer. Furthermore, while measuring the weight average molecular weight of the polymerization system, the polymerization may be terminated when a curable prepolymer with a certain degree of polymerization is obtained.
[0080] Optional components that may be included in the resin composition are described below. The resin composition may also include an elastomer as an optional component. Examples of the elastomer include diene-based elastomers, olefin-based elastomers, polysulfide-based elastomers, silicone-based elastomers, fluorine-based elastomers, urethane-based elastomers, and ether-based elastomers. More specifically, diene-based elastomers include styrene-butadiene rubber (SBR), butadiene rubber (BR), styrene-isoprene rubber, isoprene rubber (IR), chloroprene rubber (CR), and acrylonitrile-butadiene rubber (NBR). Examples of olefin-based elastomers include butyl rubber (IIR), ethylene-propylene rubber, ethylene-vinyl acetate rubber, chlorosulfonated polyethylene, and acrylic rubber. These elastomers may be either non-hydrogenated or hydrogenated. Among these, styrene-butadiene rubber (SBR) is preferred due to its low dielectric constant and excellent heat resistance.
[0081] Since styrene-butadiene rubber does not contain oxygen atoms in its molecule, the amount of polar groups can be reduced in a cured product obtained using a resin composition containing styrene-butadiene rubber, thereby further reducing the dielectric constant and dielectric loss tangent. Furthermore, since styrene-butadiene rubber has a benzene ring derived from styrene in its molecule, it has good compatibility with a curable prepolymer having a vinylbenzyl group in the resin composition, and the moldability of the resulting cured product can be further improved.
[0082] Examples of styrene-butadiene rubber include styrene-butadiene copolymers and styrene-butadiene-styrene copolymers. These may be non-hydrogenated or hydrogenated. In the case of hydrogenated products, the carbon-carbon double bonds of the butadiene may be partially or entirely saturated. Examples of hydrogenated products include styrene-ethylene-butylene-styrene copolymers and styrene-ethylene-butylene copolymers.
[0083] In the styrene-butadiene rubber or its hydrogenated product, the styrene-derived structural units are preferably 5 to 80 mass %, more preferably 10 to 75 mass %, even more preferably 15 to 60 mass %, and even more preferably 20 to 45 mass %, from the viewpoint of dielectric properties. In addition, within these ranges, the viscoelasticity of the styrene-butadiene rubber or its hydrogenated product becomes appropriate, and the adhesion of the resin composition to the substrate can be further improved.
[0084] From the viewpoints of solvent solubility, moldability, and flexibility, the weight average molecular weight (Mw) of the elastomer is preferably 50,000 to 500,000, more preferably 70,000 to 300,000, and even more preferably 100,000 to 200,000. From the viewpoints of solvent solubility, moldability, and flexibility, the number average molecular weight (Mn) of the elastomer is preferably 10,000 to 200,000, more preferably 30,000 to 150,000, and even more preferably 50,000 to 120,000. From the viewpoint of compatibility with the curable prepolymer, the Mw / Mn of the elastomer is preferably 1.0 to 5.0, more preferably 1.5 to 3.5, and even more preferably 2.0 to 3.0. The weight average molecular weight (Mw) and number average molecular weight (Mn) of the elastomer are measured according to the method described above.
[0085] The elastomer may be used alone or in combination of two or more types, and may be present in an amount of 1 to 80 parts by weight, 10 to 70 parts by weight, 20 to 60 parts by weight, or 30 to 40 parts by weight per 100 parts by weight of the curable prepolymer.
[0086] In a resin composition, the curable prepolymer itself provides excellent tackiness of the coating and excellent moldability of the cured product, so the content of the elastomer can be reduced, and it is even possible to eliminate the need for an elastomer in the resin composition. On the other hand, in a resin composition, the curable prepolymer does not have a polar group, so it tends to have good compatibility with the elastomer in the resin composition, and it is possible to increase the content of the elastomer. Furthermore, when the weight-average molecular weight (Mw) of the curable prepolymer is 50,000 or more, compatibility with the elastomer is even better, and the content of the elastomer can be further increased.
[0087] The resin composition may contain a filler as an optional component. Examples of the filler include inorganic fillers and organic fillers, and inorganic fillers are preferred from the viewpoint of dielectric properties. Examples of inorganic fillers include silica (SiO 2 ), alumina (Al 2 O 3 ), titanium oxide, barium titanate, strontium titanate, potassium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, aluminum borate, silicon carbide, mica, beryllia, clay, talc, etc.
[0088] The shape and size of the inorganic filler are not particularly limited. The average particle diameter of the inorganic filler may be, for example, 0.01 to 20 μm, 0.1 to 10 μm, or 1 to 5 μm. Here, the average particle diameter of the inorganic filler is the particle diameter at a point corresponding to an integrated value of 50% in a volume-based particle distribution measured by a laser diffraction scattering method.
[0089] The filler may be used alone or in combination of two or more. The filler may be used in an amount of 10 to 500 parts by mass, 50 to 400 parts by mass, 100 to 350 parts by mass, or 200 to 300 parts by mass per 100 parts by mass of the curable prepolymer. When the resin composition contains an elastomer, the inorganic filler may be used in an amount of 50 to 400 parts by mass, 100 to 350 parts by mass, or 200 to 300 parts by mass per 100 parts by mass of the combined amount of the curable prepolymer and the elastomer.
[0090] The resin composition may be a solvent-free resin composition containing a curable prepolymer, provided that the curable prepolymer is liquid. Alternatively, the resin composition may contain a curable prepolymer and a solvent. The solvent can adjust the viscosity of the resin composition and further improve the coatability. An organic solvent is preferred as the solvent.
[0091] Examples of organic solvents include alcohol-based solvents such as ethanol, propanol, butanol, methyl cellosolve, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based solvents such as tetrahydrofuran; aromatic hydrocarbon-based solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur-containing solvents such as dimethyl sulfoxide; and ester-based solvents such as γ-butyrolactone. The organic solvents may be used alone or in combination of two or more.
[0092] When the resin composition contains a solvent, the components other than the solvent are considered to be solids, and the solids content may be 10 to 80 mass%, 30 to 70 mass%, or 40 to 60 mass% relative to the total mass of the resin composition.
[0093] The resin composition may further contain additives other than the above components, as long as the effects of the present invention are not impaired. Examples of additives include curing agents, curing accelerators, flame retardants, antioxidants, heat stabilizers, antistatic agents, UV absorbers, pigments, colorants, lubricants, etc. The resin composition may also contain thermosetting resins and thermoplastic resins other than those described above. The resin composition may also contain a radical polymerization initiator or a by-product thereof derived from the polymerization of the prepolymer. The resin composition may also contain a radical polymerization initiator or the like as a curing accelerator.
[0094] The method for producing the resin composition is not particularly limited. The resin composition according to one embodiment is not limited by the production method, and its characteristics are as described in the present disclosure. In one example of a method for producing a resin composition, a curable prepolymer is mixed alone or in combination with optional components to obtain a resin composition. For example, the curable prepolymer is dissolved or dispersed in a solvent, and an elastomer, a filler, other additives, etc. are added as needed and mixed to obtain a resin composition. The conditions for mixing each component, such as the order of mixing, temperature, and time, are not particularly limited, and may be set appropriately depending on the type of raw material, production scale, production equipment, etc.
[0095] "Cured Product" According to one embodiment, a cured product of a resin composition can be provided. Details of the resin composition are as described above. Furthermore, since this cured product is provided using a resin composition containing a curable prepolymer, the tackiness of a coating of the resin composition can be improved and the occurrence of molding marks in the cured product can be reduced. Furthermore, when a cured product is provided using a resin composition containing a curable prepolymer and an elastomer, the weight-average molecular weight (Mw) of the curable prepolymer can be 50,000 or more, thereby improving the compatibility of the resin composition and reducing the occurrence of layer separation in the resulting cured product due to component imbalance.
[0096] The cured product of the resin composition preferably has a dielectric constant (Dk) of 4.0 or less, more preferably 3.5 or less, and even more preferably 3.2 or less at 25°C and 10 GHz. More specifically, the cured product of the resin composition may have a dielectric constant (Dk) of 3.20 or less, 3.15 or less, or 3.10 or less at 25°C and 10 GHz. The smaller the dielectric constant (Dk) of the cured product of the resin composition at 25°C and 10 GHz, the more preferable it is, and there is no particular restriction on the lower limit, but it may be, for example, 2.3 or more, or 2.4 or more, taking into consideration the balance with other physical properties.
[0097] The cured product of the resin composition preferably has a dielectric loss tangent (Df) of 0.0080 or less, more preferably 0.0012 or less, and even more preferably 0.0011 or less at 25°C and 10 GHz. The smaller the dielectric loss tangent (Df) of the cured product of the resin composition at 25°C and 10 GHz, the better. There is no particular restriction on the lower limit, but it may be, for example, 0.0001 or more, taking into consideration the balance with other physical properties.
[0098] Furthermore, when the resin composition does not contain a filler, the cured product of the resin composition preferably has a dielectric constant (Dk) of 3.0 or less, more preferably 2.7 or less, and even more preferably 2.5 or less at 25°C and 10 GHz. More specifically, the cured product of the resin composition may have a dielectric constant (Dk) of 2.70 or less, 2.65 or less, or 2.60 or less at 25°C and 10 GHz. Furthermore, when the resin composition does not contain a filler, the cured product of the resin composition preferably has a dielectric loss tangent (Df) of 0.0020 or less, more preferably 0.0014 or less, even more preferably 0.0012 or less, and even more preferably 0.0010 or less at 25°C and 10 GHz.
[0099] In the present disclosure, the dielectric constant (Dk) and dielectric loss tangent (Df) at 25°C and 10 GHz are measured in the 10 GHz band at 25°C in accordance with the SPDR method (split post dielectric resonator). A "PNA Network Analyzer N5227A" (trade name) from Agilent Technologies may be used as the measuring device. The sample used to measure the dielectric constant (Dk) and dielectric loss tangent (Df) of the cured product of the resin composition is a cured product obtained using the resin composition and molded into a 1 cm thick, 5 cm x 10 cm sample.
[0100] Furthermore, the sample used to measure the dielectric constant (Dk) and dielectric loss tangent (Df) of the cured resin composition was prepared by curing the resin composition to a C-stage state according to JIS K 6800 (1985).
[0101] "Prepreg" According to one embodiment, a prepreg containing the resin composition or a semi-cured product of the resin composition can be provided. Details of the resin composition are as described above.
[0102] The prepreg may contain a resin composition or a semi-cured product of the resin composition and a fiber substrate. In the prepreg, the curable prepolymer may be in an uncured state, or the curable prepolymer may be in a partially or entirely semi-cured state.
[0103] Prepregs can be obtained, for example, by applying a resin composition to a fiber substrate and drying it. Alternatively, prepregs can be obtained by impregnating a fiber substrate with a resin composition and then drying the fiber substrate impregnated with a curable prepolymer. Drying is preferably carried out at a temperature at which volatile components such as solvents that may be contained in the resin composition are removed or higher, and may be carried out within a temperature range in which the curable prepolymer contained in the resin composition is semi-cured depending on the application. Furthermore, drying is preferably adjusted so that the curable prepolymer contained in the resin composition is not completely cured. From this perspective, the drying temperature may be 80 to 200°C, and the drying time may be 1 to 30 minutes depending on the drying temperature, drying equipment, its scale, etc.
[0104] In the present disclosure, a semi-cured product of a curable prepolymer refers to a state in which some of the vinylbenzyl groups contained in the curable prepolymer contribute to the curing reaction, with the remaining vinylbenzyl groups remaining. A semi-cured product of a curable prepolymer having vinylbenzyl groups can be further subjected to a heat treatment or the like to be in a state in which the curing reaction can continue. In the present disclosure, one indicator of a semi-cured product is the B-stage state according to JIS K 6800 (1985).
[0105] The fiber substrate may be any of woven fabric, knitted fabric, and nonwoven fabric. The fiber substrate may be provided in the form of chopped strand mat, roving, etc. The fiber material may be any of inorganic fiber and organic fiber. Examples of inorganic fiber include glass fiber and carbon fiber. Examples of glass fiber include E-glass, NE-glass, D-glass, S-glass, Q-glass, etc. Examples of organic fiber include polyimide, polyester, tetrafluoroethylene, etc. The fiber substrate may be a single fiber of these, or a blend of two or more types of fibers. From the viewpoint of dielectric properties and heat resistance, the fiber substrate is preferably an inorganic fiber, and more preferably a glass fiber.
[0106] The fiber substrate may be selected appropriately depending on the application of the prepreg, but a sheet-like fiber substrate is preferred. Examples of the sheet-like fiber substrate include various sheet-like fiber substrates used in known laminates for electrical insulating materials. The thickness of the sheet-like fiber substrate is not particularly limited, but is preferably 0.02 to 0.5 mm, for example. Here, the thickness is measured at five points at equal distances across the entire surface of the sheet-like fiber substrate, and the arithmetic average value of the five measurements is used.
[0107] In the prepreg, the total mass of the curable prepolymer and elastomer may be 20 to 90 mass % or 30 to 80 mass % based on the total mass of the curable prepolymer, elastomer, and fibrous substrate. However, the mass of the elastomer may be 0 mass %. Within these ranges, the fibrous substrate in the prepreg can be more easily impregnated with resin. Furthermore, the process of assembling the prepreg into a molded product and curing it can be more easily performed.
[0108] "Resin Film" According to one embodiment, a resin film containing the resin composition or a semi-cured product of the resin composition can be provided. Details of the resin composition are as described above.
[0109] The term "resin film" refers to a resin composition formed into a film. In the resin film, the curable prepolymer may be in an uncured state, or the curable prepolymer may be partially or entirely semi-cured. A cured product can be obtained by curing the resin film by heat treatment or the like.
[0110] The resin film can be obtained, for example, by applying a resin composition to a substrate and drying it. Drying can be performed in the same manner as in the prepreg manufacturing method described above. After drying the resin film on the substrate, a product can be provided as a combination of the resin film and the substrate. For example, this method can provide a resin film as an insulating layer or the like in a printed wiring board. In another method, after drying the resin film on the substrate, the resin film can be peeled off from the substrate and provided as a product.
[0111] The substrate may be either an inorganic substrate or an organic substrate, and examples thereof include glass substrates, metal substrates such as metal foils and metal plates, plastic substrates such as plastic plates and plastic films, and paper substrates, as well as the fiber substrates described above for the prepreg. A substrate having a release layer formed on its surface may be used so that the resin film can be peeled off from the substrate.
[0112] The relative dielectric constant (Dk) and dielectric dissipation factor (Df) of the prepreg and resin film are not particularly limited, but it is preferable that they are each independently within the numerical range of the relative dielectric constant (Dk) and dielectric dissipation factor (Df) of the cured product of the resin composition described above.
[0113] "Metal-clad laminate" According to one embodiment, a metal-clad laminate having a cured resin composition and a metal foil can be provided. Details of the resin composition are as described above.
[0114] The metal-clad laminate preferably has a cured resin layer containing a cured resin and a metal foil formed on at least one side of the cured resin layer. The cured resin layer contains a cured product of a resin composition, but may be a cured product of the prepreg or resin film described above. In a more useful application, a metal foil is formed on at least one side of the cured prepreg, and more preferably, a metal foil is formed on both sides of the cured prepreg. The cured resin layer may be one in which a metal foil is formed on at least one side of a single sheet-like prepreg, or two or more sheet-like prepregs are laminated together, and a metal foil is formed on at least one side of the outermost surface of the laminate. In a more useful application, the metal-clad laminate is one in which two or more sheet-like prepregs are laminated together, and a metal foil is formed on both sides of the laminate.
[0115] Metal-clad laminates can be produced, for example, by placing metal foil on one or both sides of a sheet-like prepreg and then heat-pressure molding it. This allows the curing reaction of the sheet-like prepreg to proceed, resulting in a cured prepreg. When heat-pressure molding, only one prepreg may be used, or two or more prepregs may be laminated together. The heat-pressure conditions are not particularly limited, but can be, for example, a temperature of 100 to 300°C, a time of 10 to 300 minutes, and a pressure of 1.5 to 5 MPa. Furthermore, after heat-pressure, reheating may be performed to further promote curing of the prepreg. In this case, the reheating temperature may be 100 to 300°C. Examples of heat-pressure methods that can be used include an autoclave molding machine, a multi-stage press, a multi-stage vacuum press, and a continuous molding machine.
[0116] The metal for the metal foil is not particularly limited, and examples thereof include copper, nickel, aluminum, gold, silver, platinum, molybdenum, ruthenium, tungsten, iron, titanium, chromium, and alloys containing two or more of these metal elements. Industrially, the metals copper, nickel, and aluminum are preferred. By using copper as the metal foil, a copper-clad laminate can be provided.
[0117] The dielectric properties of the cured resin of the metal-clad laminate with the metal foil removed (also simply referred to as the relative dielectric constant of the metal-clad laminate or the dielectric loss tangent of the metal-clad laminate) are preferably as follows:
[0118] The dielectric constant (Dk) of the metal-clad laminate is preferably 4.0 or less, more preferably 3.5 or less, and even more preferably 3.2 or less at 25°C and 10 GHz. More specifically, the dielectric constant (Dk) of the metal-clad laminate may be 3.20 or less, 3.15 or less, or 3.10 or less at 25°C and 10 GHz. The smaller the dielectric constant (Dk) of the metal-clad laminate is at 25°C and 10 GHz, the more preferable it is. There is no particular restriction on the lower limit, but it may be, for example, 2.3 or more, or 2.4 or more, taking into consideration the balance with other physical properties.
[0119] The dielectric loss tangent (Df) of the metal-clad laminate is preferably 0.0080 or less, more preferably 0.0012 or less, and even more preferably 0.0011 or less at 25° C. and 10 GHz. The smaller the dielectric loss tangent (Df) of the metal-clad laminate is at 25° C. and 10 GHz, the better. There is no particular restriction on the lower limit, but it may be, for example, 0.0001 or more in consideration of the balance with other physical properties.
[0120] The method for measuring the dielectric constant (Dk) and dielectric loss tangent (Df) of a metal-clad laminate is as described above for the cured product of the resin composition. The sample used for measuring the dielectric constant (Dk) and dielectric loss tangent (Df) of a metal-clad laminate is prepared by immersing the metal-clad laminate in an etching solution to remove the metal foil from the cured resin, and then cutting out a 0.2 mm thick, 5 cm x 10 cm evaluation board from the specimen from which the metal foil has been removed. In the case of a copper-clad laminate, a 10% by mass solution of ammonium persulfate is used as the etching solution.
[0121] "Printed Wiring Board" According to one embodiment, a printed wiring board having a cured product of the resin composition can be provided. Details of the resin composition are as described above.
[0122] In the printed wiring board, the cured product of the resin composition can be produced using a resin composition, a prepreg, a resin film, a metal-clad laminate, or a combination thereof. For example, a printed wiring board can be provided by producing a printed wiring board substrate using a cured prepreg. In yet another example, a printed wiring board can be provided by using a metal-clad laminate as the printed wiring board substrate. Details of the prepreg, resin film, and metal-clad laminate are as described above.
[0123] The printed wiring board may be either a single-layer printed wiring board or a multi-layer printed wiring board.
[0124] "Semiconductor Package" According to one embodiment, a semiconductor package having a printed wiring board and a semiconductor element can be provided. Details of the printed wiring board are as described above. The semiconductor package can be manufactured, for example, by mounting a semiconductor element, a memory, etc. on the printed wiring board by a known method.
[0125] Examples of embodiments are listed below. The present invention is not limited to the following embodiments: <1> A resin composition containing a curable prepolymer that contains a vinylbenzyl group and an indene ring and has a weight average molecular weight of 50,000 or more.
[0126] <2> The resin composition according to <1>, wherein the curable prepolymer has a weight average molecular weight of 150,000 or more.
[0127] <3> The resin composition according to <1> or <2>, wherein the curable prepolymer contains a structural unit having an indene ring and a vinylbenzyl group directly bonded to a carbon atom of the indene ring.
[0128] <4> The resin composition according to any one of <1> to <3>, wherein the curable prepolymer contains a structural unit derived from a vinylbenzyl compound having 1 to 3 vinylbenzyl groups and one indene ring in one molecule.
[0129] <5> The resin composition according to any one of <1> to <4>, further comprising a filler.
[0130] <6> A prepreg containing the resin composition according to any one of <1> to <5> above or a semi-cured product of the resin composition.
[0131] <7> A resin film containing the resin composition according to any one of <1> to <5> above or a semi-cured product of the resin composition.
[0132] <8> A metal-clad laminate comprising a cured product of the resin composition according to any one of <1> to <5> above and a metal foil.
[0133] <9> A printed wiring board having a cured product of the resin composition according to any one of <1> to <5> above.
[0134] <10> A semiconductor package comprising the printed wiring board according to <9> above and a semiconductor element.
[0135] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. Tables 1 to 6 show the compositions of resin compositions and the evaluation results.
[0136] "Method for measuring weight-average molecular weight (Mw)" The weight-average molecular weight was determined by gel permeation chromatography (GPC) using a calibration curve obtained using standard polystyrene. The calibration curve was approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Types: A-2500, A-5000, F-20, F-80) (product name, Tosoh Corporation). The GPC measurement conditions are shown below.
[0137] Apparatus: High-speed GPC apparatus HLC-8320GPC (Tosoh Corporation, trade name) Detector: Ultraviolet absorption detector UV-8320 (Tosoh Corporation, trade name) Columns: Guard column; TSKgel guard column Super (HZ)-M+, column; TSKgel SuperMultipore HZ-M (2 columns), reference column; TSKgel Super H-RC (2 columns) (all Tosoh Corporation, trade names) Column size: 4.6 x 20 mm (guard column), 4.6 x 150 mm (column), 6.0 x 150 mm (reference column) Eluent: Tetrahydrofuran Sample concentration: 10 mg / 1 mL Injection volume: 20 μL or 2 μL Flow rate: 0.35 mL / min Measurement temperature: 40°C
[0138] "Preparation of Vinylbenzyl Monomer (1)" A 500 mL reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet was charged with 35.6 parts by mass of indene, 101.2 parts by mass of the following chloromethylstyrene, 7.1 parts by mass of tetra-n-butylammonium bromide (manufactured by Kanto Chemical Co., Inc.) as a phase transfer catalyst, 0.1 parts by mass of phenothiazine as a polymerization inhibitor, and 77.6 parts by mass of toluene as a solvent, and the mixture was heated and stirred at 40°C while blowing in nitrogen at a flow rate of 50 ml / min.
[0139] Chloromethylstyrene "CMS-P": AGC Seimi Chemical Co., Ltd., mixture of m- and p-isomers, m-isomer content 50% by mass, p-isomer content 50% by mass.
[0140] Next, 46.5 parts by mass of an aqueous solution of the following basic compound was added dropwise over 20 minutes, and the mixture was stirred at 60°C for another 9 hours. Nitrogen was continuously blown in during the reaction. The mixture was cooled to room temperature (approximately 25°C) and neutralized with a 10% aqueous hydrochloric acid solution. The mixture was then washed twice with pure water, and the toluene was distilled off under reduced pressure. The resulting viscous liquid was washed with methanol and then vacuum-dried to obtain vinylbenzyl monomer (1).
[0141] Aqueous solution of basic compound: an aqueous solution of sodium hydroxide with a concentration of 48% by mass, manufactured by Kanto Chemical Co., Inc.
[0142] The obtained vinylbenzyl monomer (1) is 1H-NMR analysis confirmed that the vinylbenzyl monomer (1) had a structure having a vinylbenzyl group directly bonded to the carbon atom at the 1-position, 3-position, or a combination thereof of the indene. Furthermore, gel permeation chromatography (GPC) analysis confirmed that the vinylbenzyl monomer (1) was a mixture of a monomer having two vinylbenzyl groups and a monomer having three vinylbenzyl groups. When the vinylbenzyl monomer had three vinylbenzyl groups, it was confirmed that the monomer had two vinylbenzyl groups directly bonded to the carbon atom at the 1-position and one vinylbenzyl group directly bonded to the carbon atom at the 3-position of the indene ring. The weight-average molecular weight (Mw) of the vinylbenzyl monomer (1) was 500. The weight-average molecular weight (Mw) was measured by the method described above.
[0143] "Production of Prepolymer (1)" The vinylbenzyl monomer (1) obtained above was mixed with toluene to a solids content of 60% by mass. 4000 g of this vinylbenzyl monomer (1) with a solids content of 60% by mass and 24 g of the following azo-based polymerization initiator were placed in a 5 L separable flask and stirred at 200 rpm for 1 minute. The mixture was then heated to 110°C ± 10°C while flowing nitrogen at 400 ml / min.
[0144] When the Mw of the produced curable prepolymer (1) reached the desired value between 5,000 and 500,000, heating was stopped and the solution was cooled to obtain a solution of curable prepolymer (1) having each Mw shown in the table. The weight average molecular weight (Mw) was measured by the method described above.
[0145] Azo-based polymerization initiator: 2,2'-azobis(2,4,4-trimethylpentane) ("VR-110" (trade name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (10-hour half-life temperature: 110°C).
[0146] "Preparation of Vinylbenzyl Monomer (2)" A 500 mL reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet was charged with 35.6 parts by mass of indene, 101.2 parts by mass of the above chloromethylstyrene, 24.1 parts by mass of α-chloro-p-xylene, 9.1 parts by mass of tetra-n-butylammonium bromide (manufactured by Kanto Chemical Co., Inc.) as a phase transfer catalyst, 0.1 part by mass of phenothiazine as a polymerization inhibitor, and 91.6 parts by mass of toluene as a solvent, and the mixture was heated and stirred at 40°C while blowing in nitrogen at a flow rate of 50 ml / min.
[0147] Next, 122.9 parts by mass of the aqueous solution of the basic compound was added dropwise over 20 minutes, and the mixture was stirred at 60°C for another 9 hours. Nitrogen was continuously blown in during the reaction. The mixture was cooled to room temperature (approximately 25°C) and neutralized with a 10% aqueous hydrochloric acid solution. The mixture was then washed twice with pure water, and the toluene was distilled off under reduced pressure. The resulting viscous liquid was washed with methanol and then vacuum-dried to obtain vinylbenzyl monomer (2).
[0148] The obtained vinylbenzyl monomer (2) is 1 H-NMR analysis revealed that a reaction had occurred in which a vinylbenzyl group or a methylbenzyl group was bonded to at least one of the 1- to 3-positions of the indene ring. Furthermore, gel permeation chromatography (GPC) analysis confirmed that vinylbenzyl monomer (2) was a mixture of a vinylbenzyl monomer having one substituent selected from the group consisting of vinylbenzyl and methylbenzyl groups (monosubstituted monomer), a vinylbenzyl monomer having two substituents (disubstituted monomer), and a vinylbenzyl monomer having three substituents (trisubstituted monomer). The weight-average molecular weight (Mw) of vinylbenzyl monomer (2) was 323. The weight-average molecular weight (Mw) was measured by the method described above.
[0149] "Production of Prepolymer (2)" The vinylbenzyl monomer (2) obtained above was mixed with toluene to a solids content of 60% by mass. 4000 g of this vinylbenzyl monomer (2) with a solids content of 60% by mass and 24 g of the above azo-based polymerization initiator were placed in a 5 L separable flask and stirred at 200 rpm for 1 minute. The mixture was then heated to 110°C ± 10°C while flowing nitrogen at 400 ml / min.
[0150] When the Mw of the produced curable prepolymer (2) reached the desired value between 5,000 and 500,000, heating was stopped and the solution was cooled to obtain a solution of curable prepolymer (2) having the Mw shown in the table. The weight average molecular weight (Mw) was measured by the method described above.
[0151] "Preparation of Resin Composition" Each component shown in the table was blended with toluene in the amounts shown in the table, and the blended resin compositions of the examples and comparative examples each having a solids concentration of approximately 60% by mass were prepared by stirring and mixing at 25°C. In the table, the blend amount of each component is expressed in parts by mass, and in the case of a solution, this means parts by mass converted into solids.
[0152] The components used are as follows. Vinylbenzyl monomer (1): The product manufactured as described above was used. Curable prepolymer (1): The product manufactured as described above was used. Curable prepolymer (2): The product manufactured as described above was used. Elastomer 1: Styrene-ethylene-butylene-styrene copolymer (SEBS), styrene content: 20% by mass, trade name "MD-1648", Kraton Corporation. Elastomer 2: Styrene-ethylene-butylene copolymer (SEB), styrene content: 34% by mass, trade name "MD-6951", Kraton Corporation. Silica filler: Average particle size 2 μm.
[0153] "Preparation of Prepreg" The obtained resin composition was applied to a 0.5 mm thick glass cloth (manufactured by Nitto Boseki Co., Ltd.) by impregnation, and the cloth was dried by heating at 130°C for 4 minutes to obtain a prepreg having a solid content derived from the resin composition of 70 mass%.
[0154] "Preparation of copper-clad laminate" An 18 μm thick electrolytic copper foil ("3EC-M3-VLP-18" (trade name) manufactured by Mitsui Mining & Smelting Co., Ltd.) was laminated on both sides of the obtained prepreg so that the matte surface faced the prepreg, and heated and pressed at 230° C. for 80 minutes under vacuum pressing conditions of 3 MPa to prepare a copper-clad laminate.
[0155] "Evaluation and measurement methods" Evaluation and measurement were carried out as follows, and the results are shown in the table.
[0156] (Tackiness of prepreg) The resin composition was impregnated and coated onto a glass cloth having a thickness of 30 μm, and dried at 130° C. for 10 minutes to obtain a prepreg. At this time, the film thickness of the dried prepreg was set to 50 μm. After drying, the surface of the prepreg was touched with a hand in an uncured state, and the presence or absence of tackiness was evaluated sensorily. The evaluation criteria are as follows. The criteria for no tackiness were equivalent to the prepreg of Example 1. A: No tackiness. B: Tackiness present.
[0157] (Compatibility of Resin Composition) The resin composition was placed in a transparent screw tube and allowed to stand for 1 hour, and the presence or absence of phase separation of the resin composition was visually observed. The evaluation criteria are as follows. The resin composition was also dropped into an aluminum cup and dried and cured in a dryer at 170°C for 30 minutes. The cured resin was visually observed to see if it had separated into patches. In Examples and Comparative Examples in which phase separation of the resin composition was not observed, the resin did not separate into patches during application. A: Phase separation of the resin composition was not observed. B: Phase separation of the resin composition was observed.
[0158] (Moldability of Copper-Clad Laminate) The copper-clad laminate produced as described above was cut into 250 mm square pieces, and then the edges were cut off by about 1 cm. The copper foil on the surface of the copper-clad laminate was then etched to obtain an evaluation board. The edges and surfaces of the evaluation board were visually inspected for the presence or absence of separation of the resin or silica filler. The surface of the evaluation board was also visually inspected for the presence or absence of streaks. The evaluation criteria were as follows: A: No streaks were observed on the surface of the evaluation board, and no separation of the resin or silica filler was observed. B: Streaks were observed on the surface of the evaluation board, but no separation of the resin or silica filler was observed. C: Separation of the evaluation board was observed.
[0159] (Dielectric Properties of Cured Resin Composition) The dielectric constant (Dk) and dielectric dissipation factor (Df) of the cured resin composition were measured at 25 ° C. in the 10 GHz band in accordance with the SPDR method (split post dielectric resonator). The measurement device used was Agilent Technologies' "PNA Network Analyzer N5227A" (trade name). The sample to be measured for the dielectric constant (Dk) and dielectric dissipation factor (Df) of the cured resin composition was a resin composition cured to a C-stage state according to JIS K 6800 (1985). Specifically, the solvent of the resin composition was dried at 130 ° C. for 10 minutes, and the resulting resin powder was placed in a PTFE mold and press-molded. The pressing conditions were the same as those in "Preparation of Copper-Clad Laminates," and a sample 1 cm thick and 5 cm x 6 cm in size was prepared.
[0160]
[0161]
[0162]
[0163]
[0164]
[0165]
[0166] As shown in the table, it can be seen that the tackiness of the prepreg and the formability of the copper-clad laminate are improved by using a resin composition containing a curable prepolymer having a weight average molecular weight (Mw) of 50,000 or more.
[0167] Resin compositions according to some embodiments of the present disclosure can be used as substrate materials for metal-clad laminates such as copper-clad laminates and printed wiring boards in electronic devices where higher signal speeds and larger capacity are expected, such as mobile communication devices typified by smartphones, their base station equipment, servers, routers, and other network infrastructure devices, and large-scale computers.
[0168] This disclosure relates to the subject matter described in Japanese Patent Application No. 2023-085360, filed May 24, 2023, the entire disclosure of which is incorporated herein by reference. It should be noted that, in addition to what has already been described, various modifications and variations may be made to the above-described embodiments without departing from the novel and advantageous features of the present disclosure. Accordingly, all such modifications and variations are intended to be included within the scope of the appended claims.
Claims
1. A resin composition comprising a curable prepolymer having a vinylbenzyl group and an indene ring and a weight average molecular weight of 50,000 or more.
2. The resin composition according to claim 1, wherein the curable prepolymer has a weight average molecular weight of 150,000 or more.
3. The resin composition according to claim 1, wherein the curable prepolymer comprises a structural unit having an indene ring and a vinylbenzyl group bonded directly to a carbon atom of the indene ring.
4. The resin composition according to claim 1, wherein the curable prepolymer contains structural units derived from a vinylbenzyl compound having 1 to 3 vinylbenzyl groups and one indene ring in one molecule.
5. The resin composition according to claim 1, further comprising a filler.
6. A prepreg comprising the resin composition according to any one of claims 1 to 5 or a semi-cured product of said resin composition.
7. A resin film comprising the resin composition according to any one of claims 1 to 5 or a semi-cured product of said resin composition.
8. A metal-clad laminate comprising a cured product of the resin composition according to any one of claims 1 to 5 and a metal foil.
9. A printed wiring board having a cured product of the resin composition according to any one of claims 1 to 5.
10. A semiconductor package comprising the printed wiring board according to claim 9 and a semiconductor element.
Citation Information
Patent Citations
Production method of indene-styrene graft polymer, and molding material, film or additive and optical part using polymer which is obtained by this production method
JP2002003545A
Curable vinylbenzyl compound and method for producing the same
JP2003277440A
Adhesive composition and adhesive sheet
JP2011190336A
Cited By
Resin composition, prepreg, resin film, metal-clad laminated plate, printed wiring board, and semiconductor package
WO2025089252A1
Curable resin material, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package
WO2026058835A1
Resin, resin production method, curable resin material, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package
WO2026126848A1
Aralkyl-modified resin, curable resin material, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package
WO2026126849A1
Curable resin composition, curable composition for metal-clad laminates, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package