Cutting tool

The cutting tool's multi-layer coating structure with specific residual stress and thickness ranges enhances wear and fracture resistance, addressing the limitations of conventional tools in light interrupted turning of black-skinned alloy steel, resulting in extended tool life.

WO2024261951A1PCT designated stage expired Publication Date: 2024-12-26SUMITOMO ELECTRIC HARDMETAL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/023096
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-22
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Conventional cutting tools used in light interrupted turning of black-skinned alloy steel face challenges with abrasion resistance, fracture resistance, and wear resistance, leading to reduced tool life due to insufficient residual stress and chipping resistance in the coating layers.

Method used

A cutting tool design featuring a base material coated with a multi-layer structure: a first layer of titanium carbonitride, a second layer of aluminum oxide, and a third layer of titanium carbonitride, where the residual stresses in each layer satisfy the relationship X < Y < Z, with specific stress and thickness ranges to enhance wear and fracture resistance.

Benefits of technology

The multi-layer coating structure significantly improves the tool's wear resistance and fracture resistance, extending the tool life during light interrupted turning of black-skinned alloy steel by balancing residual stresses and layer thicknesses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023023096_26122024_PF_FP_ABST
    Figure JP2023023096_26122024_PF_FP_ABST
Patent Text Reader

Abstract

This cutting tool is provided with a base material, and a coating film that is disposed on the base material, wherein the coating film includes a first layer that is positioned on the base material, a second layer that is positioned on the first layer, and a third layer that is positioned on the second layer, the first layer is composed of titanium carbonitride, the second layer is composed of aluminum oxide, the third layer is composed of titanium carbonitride, and the residual stress X of the first layer, the residual stress Y of the second layer, and the residual stress Z of the third layer satisfy the relationship set forth in formula 1.
Need to check novelty before this filing date? Find Prior Art

Description

cutting tools

[0001] The present disclosure relates to cutting tools.

[0002] Conventionally, cutting tools including a substrate and a coating disposed on the substrate have been used in cutting processes (Patent Documents 1 to 6).

[0003] JP 2020-037150 A JP 2020-116645 A International Publication No. 2009 / 112116 International Publication No. 2022 / 244241 International Publication No. 2022 / 244242 International Publication No. 2022 / 244243

[0004] A cutting tool according to the present disclosure is a cutting tool including a substrate and a coating disposed on the substrate, wherein the coating includes a first layer located on the substrate, a second layer located on the first layer, and a third layer located on the second layer, wherein the first layer is made of titanium carbonitride, the second layer is made of aluminum oxide, and the third layer is made of titanium carbonitride, and the residual stress X of the first layer, the residual stress Y of the second layer, and the residual stress Z of the third layer satisfy the relationship of Equation 1: X<Y<Z Equation 1

[0005] Fig. 1 is a schematic cross-sectional view illustrating one embodiment of a cutting tool according to the present disclosure. Fig. 2 is a schematic cross-sectional view of an example of a CVD (Chemical Vapor Deposition) apparatus used in manufacturing the cutting tool according to the present disclosure.

[0006] [Problem to be Solved by the Present Disclosure] In recent years, there has been an increasing demand for improved tool life, particularly in light intermittent turning of black alloy steel. Key factors for further improving tool life in light intermittent turning of black alloy steel include "wear resistance" and "fracture resistance." From the perspective of improving wear resistance, a cutting tool has been used in light intermittent turning of black alloy steel, which includes a substrate and a coating disposed on the substrate. The coating includes a first layer located on the substrate, a second layer located on the first layer, and a third layer located on the second layer, the first layer being made of titanium carbonitride, the second layer being made of aluminum oxide, and the third layer being made of titanium carbonitride. However, in such coatings, the third layer is easily destroyed by blasting, making it difficult to introduce sufficient residual stress into the first layer, resulting in insufficient "fracture resistance." Furthermore, wear may easily occur due to minute damage caused by insufficient "fracture resistance" (i.e., insufficient "wear resistance"). Therefore, there is a need for a tool that combines excellent "wear resistance" and excellent "fracture resistance" to extend tool life, particularly in lightly interrupted turning of black alloy steel.

[0007] Therefore, an object of the present disclosure is to provide a cutting tool that has a long tool life, particularly in lightly interrupted turning of black alloy steel.

[0008] Effect of the Present Disclosure According to the present disclosure, it is possible to provide a cutting tool having a long tool life, particularly in light interrupted turning of black alloy steel.

[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. (1) A cutting tool of the present disclosure is a cutting tool including a substrate and a coating disposed on the substrate, wherein the coating includes a first layer located on the substrate, a second layer located on the first layer, and a third layer located on the second layer, wherein the first layer is made of titanium carbonitride, the second layer is made of aluminum oxide, and the third layer is made of titanium carbonitride, and the residual stress X of the first layer, the residual stress Y of the second layer, and the residual stress Z of the third layer satisfy the relationship of Equation 1: X<Y<Z Equation 1

[0010] According to the present disclosure, a cutting tool having a long tool life can be provided, particularly in light interrupted turning of black alloy steel.

[0011] (2) In the above (1), the residual stress X of the first layer is preferably −1.0 GPa or more and −0.3 GPa or less, thereby providing a cutting tool having a longer tool life, particularly in light intermittent turning of black alloy steel.

[0012] (3) In the above (1) or (2), the residual stress Y of the second layer is preferably −0.5 GPa or more and 0.1 GPa or less, thereby providing a cutting tool having a longer tool life, particularly in light intermittent turning of black alloy steel.

[0013] (4) In any of the above (1) to (3), the residual stress Z of the third layer is preferably −0.3 GPa or more and 0.4 GPa or less, thereby providing a cutting tool having a longer tool life, particularly in light intermittent turning of black alloy steel.

[0014] (5) In any of the above (1) to (4), the thickness of the first layer is preferably 3 μm or more and 15 μm or less, thereby providing a cutting tool having a longer tool life, particularly in light intermittent turning of black alloy steel.

[0015] (6) In any of the above (1) to (5), the thickness of the second layer is preferably 3 μm or more and 15 μm or less, thereby providing a cutting tool having a longer tool life, particularly in light interrupted turning of black alloy steel.

[0016] (7) In any of the above (1) to (6), the thickness of the third layer is preferably 2 μm or more and 4 μm or less, thereby providing a cutting tool having a longer tool life, particularly in light intermittent turning of black alloy steel.

[0017] [Details of the embodiment of the present disclosure] A specific example of a cutting tool according to one embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference symbols represent the same or corresponding parts. Furthermore, dimensional relationships such as length, width, thickness, and depth have been changed as appropriate for clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.

[0018] In this specification, the expression "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and a unit is specified only for B, the unit of A and the unit of B are the same.

[0019] [Embodiment 1: Cutting Tool] A cutting tool according to one embodiment of the present disclosure will be described with reference to Figure 1. One embodiment of the present disclosure (hereinafter also referred to as "this embodiment") is a cutting tool 10 including a substrate 1 and a coating 2 disposed on the substrate 1, wherein the coating 2 includes a first layer 3 located on the substrate 1, a second layer 4 located on the first layer 3, and a third layer 5 located on the second layer 4, wherein the first layer 3 is made of titanium carbonitride, the second layer 4 is made of aluminum oxide, and the third layer 5 is made of titanium carbonitride, and the residual stress X of the first layer 3, the residual stress Y of the second layer 4, and the residual stress Z of the third layer 5 satisfy the relationship of Equation 1: X<Y<Z Equation 1

[0020] According to the present disclosure, it is possible to provide a cutting tool having a long tool life, particularly in light interrupted turning of black alloy steel. The reason for this is presumably as follows.

[0021] The residual stress X of the first layer 3, the residual stress Y of the second layer 4, and the residual stress Z of the third layer 5 satisfy the relationship of Equation 1: X<Y<Z Equation 1 As a result, the residual stress on the substrate 1 side of the coating 2 becomes relatively low, which can improve fracture resistance. Furthermore, the residual stress on the surface side of the coating 2 becomes relatively high, which reduces film breakdown due to stress introduction, making it easier to suppress the occurrence of film structure shedding, which can improve wear resistance.

[0022] That is, according to the present disclosure, since the cutting tool 1 can have both excellent "wear resistance" and excellent "fracture resistance," it is possible to provide a cutting tool having a long tool life, particularly in light intermittent turning of black alloy steel.

[0023] 1 , a cutting tool 10 according to an embodiment of the present disclosure includes a substrate 1 and a coating 2 disposed on the substrate 1. The coating 2 preferably covers the entire surface of the substrate 1, but it does not depart from the scope of this embodiment even if a portion of the substrate 1 is not coated with the coating 2 or if the coating 2 has a partially different configuration. In cases where a portion of the substrate 1 is not coated with the coating 2, the coating 2 is preferably disposed so as to cover the surface of at least a portion of the substrate 1 that is involved in cutting. In this specification, the portion of the substrate 1 that is involved in cutting refers to a region of the substrate 1 that is surrounded by the cutting edge ridge and an imaginary surface that is, for example, 5 mm, 3 mm, 2 mm, 1 mm, or 0.5 mm away from the cutting edge ridge toward the substrate 1 along a perpendicular to a tangent to the cutting edge ridge, depending on the size and shape of the substrate 1.

[0024] The cutting tool 10 of this embodiment can be suitably used as a cutting tool 10 such as a drill, an end mill, an indexable cutting tip for a drill, an indexable cutting tip for an end mill, an indexable cutting tip for a milling process, an indexable cutting tip for a turning process, a metal saw, a gear cutting tool, a reamer, a tap, etc.

[0025] <<Substrate>> Any conventionally known substrate 1 of this type can be used as the substrate 1. For example, the substrate 1 is preferably any one of cemented carbide (WC-based cemented carbide, cemented carbide containing WC and Co, cemented carbide containing carbonitrides of Ti, Ta, Nb, etc.), cermet (mainly composed of TiC, TiN, TiCN, etc.), high-speed steel, ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, etc.), cubic boron nitride sintered body, and diamond sintered body.

[0026] It is particularly preferable to select a WC-based cemented carbide or a cermet (particularly a TiCN-based cermet) from among these various substrates 1. These substrates 1 have an excellent balance between hardness and strength, particularly at high temperatures, and therefore, when used as the substrate 1 of a cutting tool 10, can contribute to extending the life of the cutting tool 10.

[0027] <Coating> The coating 2 includes a first layer 3 located on the substrate 1, a second layer 4 located on the first layer 3, and a third layer 5 located on the second layer 4. By covering the substrate 1, the coating 2 improves various properties of the cutting tool 10, such as wear resistance and chipping resistance, and has the effect of extending the life of the cutting tool 10. Note that the coating 2 may include "other layers" described below in addition to the first layer 3, second layer 4, and third layer 5, to the extent that the effects of the present disclosure are not impaired.

[0028] The thickness of the coating 2 is preferably 6 μm or more and 30 μm or less. If the thickness of the coating 2 is less than 6 μm, the coating 2 is too thin, which tends to shorten the life of the cutting tool 10. On the other hand, if the thickness of the coating 2 exceeds 30 μm, chipping of the coating 2 tends to occur in the early stages of cutting, which tends to shorten the life of the cutting tool 10. The thickness of the coating 3 can be measured by observing the cross section of the coating 2 using a scanning electron microscope (SEM). Specifically, the observation magnification of the cross section sample is set to 5,000 to 10,000 times, and the observation area is set to 100 to 500 μm. 2 The thickness width is measured at three points in one visual field, and the average value is taken as the "thickness." The same applies to the thickness of each layer described below unless otherwise specified.

[0029] <First Layer> <Composition of First Layer> The first layer 3 is made of titanium carbonitride. Here, "made of titanium carbonitride" means that the first layer 3 may contain inevitable impurities in addition to titanium carbonitride, as long as the effects of the present disclosure are achieved. Examples of the inevitable impurities include chlorine atoms (Cl). The total content of the inevitable impurities in the first layer 3 is preferably greater than 0 mass% and less than 3 mass%.

[0030] The fact that the first layer 3 is made of titanium carbonitride is measured by X-ray diffraction (XRD) and energy dispersive X-ray analysis (EDX). The content of inevitable impurities in the first layer 3 is measured by secondary ion mass spectrometry (SIMS). It has been confirmed that, as long as measurements are performed using the same cutting tool 10, there is no variation in the measurement results even if the measurement location is arbitrarily selected.

[0031] <Structure of First Layer> The thickness of the first layer 3 is preferably 3 μm or more and 15 μm or less. This allows for both better wear resistance and better fracture resistance, making it possible to provide a cutting tool with a longer tool life, particularly in light intermittent turning of black alloy steel. The lower limit of the thickness of the first layer 3 is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 7 μm or more. The upper limit of the thickness of the first layer 3 is preferably 15 μm or less, more preferably 13 μm or less, and even more preferably 11 μm or less. The thickness of the first layer 3 is more preferably 5 μm or more and 13 μm or less, and even more preferably 7 μm or more and 11 μm or less.

[0032] <Residual Stress of First Layer> The residual stress X of the first layer 3 is preferably -1.0 GPa or more and -0.3 GPa or less. This makes it easier to suppress the spread of damage when minute fractures occur, thereby providing a cutting tool with a longer tool life, particularly in light intermittent turning of black alloy steel. The lower limit of the residual stress X of the first layer 3 is preferably -1.0 GPa or more, more preferably -0.9 GPa or more, and even more preferably -0.8 GPa or more. The upper limit of the residual stress X of the first layer 3 is preferably -0.3 GPa or less, more preferably -0.4 GPa or less, and even more preferably -0.5 GPa or less. The residual stress X of the first layer 3 is more preferably -0.9 GPa or more and -0.4 GPa or less, and even more preferably -0.8 GPa or more and -0.5 GPa or less.

[0033] The residual stress X of the first layer 3 can be determined by measuring the first layer 3 using an X-ray residual stress measurement device with the sin2ψ method (see pages 54-66 of "X-Ray Stress Measurement Method" (Published by the Japan Society for Materials Science, Yokendo Co., Ltd., 1981)). The temperature during the measurement is room temperature (20°C). It has also been confirmed that, as long as the measurement is performed using the same cutting tool 10, there is no variation in the measurement results even if the measurement location is arbitrarily selected.

[0034] <Second Layer> <Composition of Second Layer> The second layer 4 is made of aluminum oxide. Here, "made of aluminum oxide" means that the second layer 4 may contain inevitable impurities in addition to aluminum oxide, as long as the effects of the present disclosure are achieved. Examples of the inevitable impurities include chlorine atoms (Cl). The total content of the inevitable impurities in the second layer 4 is preferably greater than 0% by mass and less than 3% by mass.

[0035] The fact that the second layer 4 is made of aluminum oxide is measured by X-ray diffraction (XRD) and energy dispersive X-ray analysis (EDX). The content of inevitable impurities in the second layer 4 is measured by secondary ion mass spectrometry (SIMS). It has been confirmed that, as long as measurements are performed using the same cutting tool 10, there is no variation in the measurement results even if the measurement location is arbitrarily selected.

[0036] <Structure of Second Layer> The thickness of the second layer 4 is preferably 3 μm or more and 15 μm or less. This makes it possible to achieve both better wear resistance and better fracture resistance, thereby providing a cutting tool with a longer tool life, especially in light intermittent turning of black alloy steel. The lower limit of the thickness of the second layer 4 is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 7 μm or more. The upper limit of the thickness of the second layer 4 is preferably 15 μm or less, more preferably 13 μm or less, and even more preferably 11 μm or less. The thickness of the second layer 4 is more preferably 5 μm or more and 13 μm or less, and even more preferably 7 μm or more and 11 μm or less.

[0037] <Residual Stress of Second Layer> The residual stress Y of the second layer 4 is preferably -0.5 GPa or more and 0.1 GPa or less. This allows for the introduction of a moderate residual stress, which makes the alumina structure less susceptible to fracture and improves chipping resistance, thereby providing a cutting tool with a longer tool life, especially in light intermittent turning of black alloy steel. The lower limit of the residual stress Y of the second layer 4 is preferably -0.5 GPa or more, more preferably -0.4 GPa or more, and even more preferably -0.3 GPa or more. The upper limit of the residual stress Y of the second layer 4 is preferably 0.1 GPa or less, more preferably 0 GPa or less, and even more preferably -0.1 GPa or less. The residual stress Y of the second layer 4 is preferably -0.4 GPa or more and 0 GPa or less, and even more preferably -0.3 GPa or more and -0.1 GPa or less.

[0038] The residual stress Y in the second layer 4 can be determined by a method similar to the method for measuring the residual stress X in the first layer 3, except that the measurement is performed on the second layer 4. It has been confirmed that, as long as the measurement is performed using the same cutting tool 10, there is no variation in the measurement results even if the measurement location is arbitrarily selected.

[0039] <Third Layer> <Composition of Third Layer> The third layer 5 is made of titanium carbonitride. Here, "made of titanium carbonitride" means that the third layer 5 may contain inevitable impurities in addition to titanium carbonitride, as long as the effects of the present disclosure are exhibited. Examples of the inevitable impurities include chlorine atoms (Cl). The total content of the inevitable impurities in the third layer 5 is preferably greater than 0 mass% and less than 3 mass%.

[0040] The third layer 5 is determined to be made of titanium carbonitride by X-ray diffraction (XRD) and energy dispersive X-ray analysis (EDX). The content of inevitable impurities in the third layer 5 is measured by secondary ion mass spectrometry (SIMS). It has been confirmed that, as long as measurements are performed using the same cutting tool 10, there is no variation in the measurement results even if the measurement location is arbitrarily selected.

[0041] <Structure of Third Layer> The thickness of the third layer 5 is preferably 2 μm or more and 4 μm or less. This allows for both better fracture resistance and better wear resistance, making it possible to provide a cutting tool with a longer tool life, especially in light intermittent turning of black alloy steel. The lower limit of the thickness of the third layer 5 is preferably 2 μm or more, and more preferably 2.5 μm or more. The upper limit of the thickness of the third layer 5 is preferably 4 μm or less, and more preferably 3.5 μm or less. The thickness of the third layer 5 is more preferably 2.5 μm or more and 3.5 μm or less.

[0042] <Residual Stress of Third Layer> The residual stress Z of the third layer 5 is preferably -0.3 GPa or more and 0.4 GPa or less. This makes it easier to suppress flank wear in the early stages of cutting, thereby providing a cutting tool with a longer tool life, especially in light intermittent turning of black alloy steel. The lower limit of the residual stress Z of the third layer 5 is preferably -0.3 GPa or more, more preferably -0.2 GPa or more, and even more preferably -0.1 GPa or more. The upper limit of the residual stress Z of the third layer 5 is preferably 0.4 GPa or less, more preferably 0.3 GPa or less, and even more preferably 0.2 GPa or less. The residual stress Z of the third layer 5 is more preferably -0.2 GPa or more and 0.3 GPa or less, and even more preferably -0.1 GPa or more and 0.2 GPa or less.

[0043] The residual stress Z of the third layer 5 can be determined by a method similar to the method for measuring the residual stress X of the first layer 3, except that the measurement is performed on the third layer 5. It has been confirmed that, as long as the measurement is performed using the same cutting tool 10, there is no variation in the measurement results even if the measurement location is arbitrarily selected.

[0044] <Relationship Between First Layer, Second Layer, and Third Layer> The residual stress X of the first layer 3, the residual stress Y of the second layer 4, and the residual stress Z of the third layer 5 satisfy the relationship of Equation 1: X<Y<Z Equation 1 This allows the cutting tool 10 to have both excellent wear resistance and excellent fracture resistance, and therefore allows it to exhibit a long tool life, especially in light intermittent turning of black alloy steel.

[0045] Y-X is preferably 0.1 or greater and 0.6 or less. This makes it more difficult for chipping to occur from the first layer 3 to the second layer 4, thereby providing the cutting tool with better fracture resistance. Y-X is more preferably 0.15 or greater and 0.55 or less, and even more preferably 0.2 or greater and 0.5 or less.

[0046] Y-Z is preferably -0.6 or more and -0.1 or less. This makes it more difficult for chipping to occur from the second layer 4 to the third layer 5, thereby providing the cutting tool 10 with better fracture resistance. Y-Z is more preferably -0.55 or more and -0.15 or less, and even more preferably -0.50 or more and -0.20 or less.

[0047] <Other Layers> Examples of the other layers include an underlayer (not shown), an intermediate layer (not shown), and a surface layer (not shown). The underlayer is a layer disposed between the substrate 1 and the first layer 3. The surface layer is a layer located on the surface of the coating 2. The intermediate layer is a layer disposed between the first layer 3 and the second layer 4, between the second layer 4 and the third layer 5, or both. The intermediate layer is a thin adhesive layer such as TiCNO. Therefore, the intermediate layer does not affect the stress distribution.

[0048] [Embodiment 2: Method for manufacturing a cutting tool] A method for manufacturing a cutting tool of this embodiment will be described with reference to Fig. 2. Fig. 2 is a schematic cross-sectional view of an example of a CVD apparatus used in manufacturing the cutting tool of this embodiment.

[0049] The method for manufacturing a cutting tool of this embodiment is the same as the method for manufacturing a cutting tool as described in embodiment 1, and includes a first step of preparing a substrate, a second step of forming a coating on the substrate, and a third step of blasting the coating to obtain a cutting tool, and the second step includes, in this order, a second step A of forming a first layer by a CVD method, a second step B of forming a second layer by a CVD method, and a third step C of forming a third layer by a CVD method. Details of each step are described below.

[0050] First Step In the first step, a substrate is prepared. The substrate described in the first embodiment can be used.

[0051] For example, when a cemented carbide is used as the substrate, a commercially available substrate may be used, or it may be manufactured by a general powder metallurgy method. When manufactured by a general powder metallurgy method, for example, WC powder and Co powder are mixed using a ball mill or the like to obtain a mixed powder. The mixed powder is then dried and molded into a predetermined shape to obtain a compact. The compact is then sintered to obtain a WC-Co cemented carbide (sintered body). Next, the sintered body is subjected to a predetermined cutting edge processing such as honing, thereby producing a substrate made of a WC-Co cemented carbide. Any substrate other than those described above can also be prepared as long as it is a conventionally known substrate of this type.

[0052] <<Second Step>> In the second step, a coating is formed on the substrate to obtain a cutting tool. The coating is formed using, for example, a CVD apparatus as shown in FIG. 2 . The CVD apparatus 30 includes a plurality of substrate setting jigs 31 for holding the substrate 1 and a heat-resistant alloy steel reaction vessel 32 that encases the substrate setting jigs 31. A temperature control device 33 is provided around the reaction vessel 32 to control the temperature inside the reaction vessel 32. The reaction vessel 32 is provided with a gas introduction pipe 35 having a gas introduction port 34. The gas introduction pipe 35 extends vertically within the internal space of the reaction vessel 32 in which the substrate setting jigs 31 are placed, and is rotatable about the vertical axis. The gas introduction pipe 35 is also provided with a plurality of injection holes (through holes 36) for injecting gas into the reaction vessel 32. Using this CVD apparatus 30, the first, second, and third layers that constitute the coating can be formed as follows.

[0053] The second step includes, in this order, a step 2A of forming a first layer by a CVD method, a step 2B of forming a second layer by a CVD method, and a step 2C of forming a third layer by a CVD method. When the coating film includes the "other layer" described in embodiment 1, the "other layer" can be formed by a conventionally known method.

[0054] <Step 2A: Step of forming first layer by CVD method> In step 2A, the first layer is formed by CVD method. More specifically, first, the substrate 1 is placed in a substrate setting jig 31, and while the temperature and pressure in a reaction vessel 32 are controlled within predetermined ranges, a source gas for the first layer is introduced into the reaction vessel 32 from a gas introduction pipe 35. In this way, the first layer is formed on the substrate 1.

[0055] The source gas for the first layer is TiCl 4 , C.H. 3 C.N., C.O., N. 2 , HCl, and H 2 A mixture of the following gases is used.

[0056] TiCl in mixed gas 4 The content of CH in the mixed gas is preferably 8.0% by volume or more and 9.0% by volume or less. 3 The CN content in the mixed gas is preferably 0.2% by volume or more and 1.0% by volume or less. The CO content in the mixed gas is preferably 1.3% by volume or more and 2.0% by volume or less. 2 The content of HCl in the mixed gas is preferably 8.0% by volume or more and 12.0% by volume or less. The content of HCl in the mixed gas is preferably 1.0% by volume or more and 3.0% by volume or less.

[0057] The temperature inside the reaction vessel 32 is preferably controlled to be 800° C. or higher and 850° C. or lower, and the pressure inside the reaction vessel 32 is preferably controlled to be 100 hPa or higher and 120 hPa or lower. When introducing gas, it is preferable to rotate the gas introduction pipe 35.

[0058] In the above manufacturing method, the state of the first layer can be changed by controlling the conditions of the CVD method, for example, by adjusting the film formation time, the thickness of the first layer can be controlled.

[0059] <Step 2B: Step of forming second layer by CVD method> In step 2B, the second layer is formed by CVD method. More specifically, the first cutting tool precursor having the first layer formed on the substrate is placed in substrate setting jig 31, and while the temperature and pressure in reaction vessel 32 are controlled within predetermined ranges, a source gas for the second layer is introduced into reaction vessel 32 through gas inlet pipe 35. In this way, the second layer is formed on the first layer.

[0060] The source gas for the second layer is AlCl 3 , CO 2 , H 2 S, and H 2 A mixture of the following gases is used.

[0061] AlCl in mixed gas 3 The content of CO in the mixed gas is preferably 2.0% by volume or more and 2.5% by volume or less. 2 The content of H in the mixed gas is preferably 2.5% by volume or more and 3.5% by volume or less. 2 The S content is preferably 0.5% by volume or more and 1.0% by volume or less.

[0062] The temperature inside the reaction vessel 32 is preferably controlled to be 980° C. or higher and 1015° C. or lower, and the pressure inside the reaction vessel 32 is preferably controlled to be 60 hPa or higher and 75 hPa or lower. When introducing gas, it is preferable to rotate the gas introduction pipe 35.

[0063] In the above manufacturing method, the state of the second layer can be changed by controlling the conditions of the CVD method, for example, by adjusting the film formation time, the thickness of the second layer can be controlled.

[0064] <Step 2C: Step of Forming Third Layer by CVD> In Step 2C, the third layer is formed by CVD. More specifically, first, a second cutting tool precursor having a first layer formed on a substrate and a second layer formed on the first layer is placed in a substrate setting jig 31. While controlling the temperature and pressure in a reaction vessel 32 within predetermined ranges, a source gas for the third layer is introduced into the reaction vessel 32 through a gas inlet pipe 35. This forms the third layer on the second layer.

[0065] The source gas for the third layer is TiCl 4 , C.H. 3 C.N., C.O., N. 2 , HCl, and H 2 A mixture of the following gases is used.

[0066] TiCl in mixed gas 4 The content of CH in the mixed gas is preferably 8.0% by volume or more and 9.0% by volume or less. 3 The CN content in the mixed gas is preferably 0.2% by volume or more and 0.8% by volume or less. The CO content in the mixed gas is preferably 1.3% by volume or more and 2.0% by volume or less. 2 The content of HCl in the mixed gas is preferably 8.0% by volume or more and 12.0% by volume or less. The content of HCl in the mixed gas is preferably 1.0% by volume or more and 3.0% by volume or less.

[0067] The temperature inside the reaction vessel 32 is preferably controlled to be 950° C. or higher and 1000° C. or lower, and the pressure inside the reaction vessel 32 is preferably controlled to be 80 hPa or higher and 100 hPa or lower. When introducing gas, it is preferable to rotate the gas introduction pipe 35.

[0068] In the above manufacturing method, the state of the third layer can be changed by controlling the conditions of the CVD method, for example, by adjusting the film formation time, the thickness of the third layer can be controlled.

[0069] <Step 3: Blasting the Coating to Obtain a Cutting Tool> In step 3, the coating is blasted to obtain a cutting tool. Here, "blasting" refers to a process in which a large number of small spheres (media) made of steel or non-ferrous metal (e.g., ceramics) are collided (projected) at high speed against the surface of the coating, such as the rake face, to change various properties of the surface, such as residual stress.

[0070] The types of media include, for example, ceramics, zirconia, alumina, and the like.

[0071] The average particle size of the media is 100 μm or more and 200 μm or less.

[0072] The density of the projected media is 100 g / min or more and 350 g / min or less, and preferably 150 g / min or more and 250 g / min or less.

[0073] The distance between the projection unit that projects the media and the surface of the coating (hereinafter also referred to as "projection distance") is 35 mm or more and 60 mm or less, and preferably 35 mm or more and 50 mm or less.

[0074] The projection angle of the media is 75° to the surface of the coating.

[0075] The pressure applied to the media during projection (hereinafter also referred to as "projection pressure") is preferably 0.10 MPa or more and 0.50 MPa or less, and more preferably 0.15 MPa or more and 0.45 MPa or less.

[0076] The blasting time is preferably 20 seconds or more and 30 seconds or less.

[0077] The above-mentioned conditions for the blasting treatment can be adjusted appropriately in accordance with the structure of the coating.

[0078] <Other Steps> In the manufacturing method according to this embodiment, in addition to the steps described above, additional steps may be carried out as appropriate within a range that does not impair the effects of this embodiment.

[0079] <Features of the Cutting Tool Manufacturing Method of the Present Embodiment> A cutting tool obtained by the above manufacturing method can be manufactured that includes a substrate and a coating disposed on the substrate, wherein the coating includes a first layer located on the substrate, a second layer located on the first layer, and a third layer located on the second layer, the first layer being made of titanium carbonitride, the second layer being made of aluminum oxide, and the third layer being made of titanium carbonitride, and wherein the residual stress X of the first layer, the residual stress Y of the second layer, and the residual stress Z of the third layer satisfy the relationship of Equation 1: X<Y<Z Equation 1 The reason for this is presumed to be as follows.

[0080] The cutting tool manufacturing method of this embodiment is particularly characterized in that, after forming a third layer located on the second layer in step 2C, the third step is performed by using coarse media with an average particle size of 100 to 200 μm, setting the media concentration to 100 g / min or more and 350 g / min or less, setting the media projection angle to 75° relative to the coating surface, and setting the projection distance to 35 mm or more and 60 mm or less. Projecting the coarse media at a projection angle of 75° facilitates the introduction of stress into the substrate side of the coating. Furthermore, because the media concentration is low, it is easy to increase the media projection speed, further facilitating the introduction of stress into the substrate side of the coating. Furthermore, the long projection distance makes it possible to differentiate the stress between the third layer and the second layer. As a result of the above, the residual stress X of the first layer, the residual stress Y of the second layer, and the residual stress Z of the third layer can satisfy the relationship of Equation 1 above. This was newly discovered by the inventors after extensive research.

[0081] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.

[0082] <<Preparation of Cutting Tools>> Cutting tools according to Samples 1 to 31 and 101 to 104 were prepared as follows.

[0083] <Step 1> As a substrate, a cemented carbide indexable cutting tip (shape: SEET13T3AGSN-G, manufactured by Sumitomo Electric Hardmetal Corporation) having a composition consisting of TaC (2.0 mass%), Co (11.0 mass%) and WC (balance) (including unavoidable impurities) was prepared.

[0084] <Step 2> A first layer was formed on the substrate by CVD under the following conditions so that the composition of the first layer was as shown in Tables 3 and 4 (Step 2A). The deposition time was adjusted appropriately so that the first layer had a thickness as shown in Tables 3 and 4. (Conditions for Step 2A) TiCl in the mixed gas 4 Content of CH in mixed gas: 8.0 to 9.0% by volume 3 CN content: 0.2 to 1.0% by volume CO content in the mixed gas: 1.3 to 2.0% by volume N content in the mixed gas2 Content of HCl in the mixed gas: 1.0 to 3.0 vol% Content of H in the mixed gas: 8.0 to 12.0 vol% 2 Content: Remaining Temperature: 800-850°C Pressure: 100-120hPa

[0085] Next, a second layer was formed on the first layer by CVD under the following conditions so that the composition of the second layer would be as shown in Tables 3 and 4 (Step 2B). The deposition time was adjusted appropriately so that the second layer would have the thickness shown in Tables 3 and 4. (Conditions for Step 2B) AlCl in the mixed gas 3 Content of CO in the mixed gas: 2.0 to 2.5% by volume 2 Content of: 2.5 to 3.5% by volume H in the mixed gas 2 S content: 0.5 to 1.0% by volume H in the mixed gas 2 Content: Remaining Temperature: 980-1015°C Pressure: 60-75hPa

[0086] Next, a third layer was formed on the second layer by CVD under the following conditions so that the composition of the third layer would be as shown in Tables 3 and 4 (Step 2C). The deposition time was adjusted appropriately so that the third layer would have the thickness shown in Tables 3 and 4. (Conditions for Step 2C) TiCl in the mixed gas 4 Content of CH in mixed gas: 8.0 to 9.0% by volume 3 CN content: 0.2 to 0.8% by volume CO content in the mixed gas: 1.3 to 2.0% by volume N content in the mixed gas 2 Content of HCl in the mixed gas: 1.0 to 3.0 vol% Content of H in the mixed gas: 8.0 to 12.0 vol% 2 Content: Remaining Temperature: 950-1000°C Pressure: 80-100hPa

[0087] <Third Step> A blasting treatment was performed on the surface of the cutting tool on which the first layer, the second layer, and the third layer were formed (in other words, the cutting tool on which the coating was formed) under the conditions shown in Tables 1 and 2.

[0088] By the above procedure, cutting tools according to Samples 1 to 31 and 101 to 104 were produced.

[0089]

[0090]

[0091]

[0092]

[0093] <Evaluation of Cutting Tool Characteristics> <Composition of First Layer> For each sample cutting tool, the composition of the first layer was determined by the method described in Embodiment 1. The results obtained are shown in the "Composition" column of the "First Layer" column in Tables 3 and 4. When "TiCN" is listed in the "Composition" column of the "First Layer" column in Tables 3 and 4, it means that the first layer is made of titanium carbonitride.

[0094] <Residual stress X of first layer> For each cutting tool sample, the residual stress X of the first layer was determined by the method described in embodiment 1. The results are shown in the "X [GPa]" column of Tables 3 and 4.

[0095] <Composition of Second Layer> The composition of the second layer of each cutting tool sample was determined by the method described in Embodiment 1. The results are shown in the "Composition" column of the "Second Layer" column in Tables 3 and 4. In Tables 3 and 4, the "Composition" column of the "Second Layer" column indicates "Al 2 O 3 " means that the second layer consists of aluminum oxide.

[0096] <Residual stress Y of second layer> For each cutting tool sample, the residual stress Y of the second layer was determined by the method described in embodiment 1. The obtained results are shown in the "Y [GPa]" column of Tables 3 and 4.

[0097] <Composition of Third Layer> For each sample cutting tool, the composition of the third layer was determined by the method described in Embodiment 1. The results obtained are shown in the "Composition" column of the "Third Layer" column in Tables 3 and 4. When "TiCN" is listed in the "Composition" column of the "Third Layer" column in Tables 3 and 4, it means that the third layer is made of titanium carbonitride.

[0098] <Residual stress Z of third layer> For each sample cutting tool, the residual stress Z of the third layer was determined by the method described in embodiment 1. The obtained results are shown in the "Z [GPa]" column of Tables 3 and 4.

[0099] <Coating Thickness> The coating thickness of each sample cutting tool was determined by the method described in Embodiment 1. The results obtained are shown in the "Thickness [μm]" column of the "Coating" column in Tables 3 and 4.

[0100] <Cutting Test> Cutting tests were performed using the cutting tools of each sample under the following cutting conditions. The tool life was measured as the time when the flank wear amount Vb [mm] exceeded 0.3 mm due to the combination of wear and minor chipping, causing damage to progress. The results are shown in the "Tool Life [min]" column of Tables 3 and 4. (Cutting Conditions) Workpiece: SCM440 (grooved round bar) Processing: External turning of grooved round bar Cutting speed: 250 m / min Feed rate: 0.3 mm / rev Depth of cut: 2.0 mm Cutting fluid: Water-soluble cutting oil The above cutting conditions correspond to the cutting conditions for lightly interrupted turning of black alloy steel.

[0101] The cutting tools of Samples 1 to 31 correspond to Examples. The cutting tools of Samples 101 to 104 correspond to Comparative Examples. The results in Tables 3 and 4 show that the cutting tools of Samples 1 to 31 have a longer tool life than the cutting tools of Samples 101 to 104, even in light interrupted turning of black alloy steel.

[0102] From the above, it was found that the cutting tools according to Samples 1 to 31 have a long tool life even in light intermittent turning of black alloy steel.

[0103] Although the embodiments and examples of the present disclosure have been described above, it is originally intended that the configurations of the above-described embodiments and examples may be appropriately combined or modified in various ways.

[0104] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the embodiments and examples described above, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.

[0105] REFERENCE SIGNS LIST 1 substrate, 2 coating, 3 first layer, 4 second layer, 5 third layer, 10 cutting tool, 30 CVD apparatus, 31 substrate setting jig, 32 reaction vessel, 33 temperature control device, 34 gas inlet, 35 gas inlet pipe, 36 through hole

Claims

1. A cutting tool comprising a substrate and a coating disposed on the substrate, the coating including a first layer located on the substrate, a second layer located on the first layer, and a third layer located on the second layer, the first layer being made of titanium carbonitride, the second layer being made of aluminum oxide, and the third layer being made of titanium carbonitride, and a residual stress X of the first layer, a residual stress Y of the second layer, and a residual stress Z of the third layer satisfy the relationship of formula 1. X<Y<Z Formula 1 2. The cutting tool according to claim 1, wherein the residual stress X of the first layer is not less than -1.0 GPa and not more than -0.3 GPa.

3. A cutting tool according to claim 1 or 2, wherein the residual stress Y of the second layer is -0.5 GPa or more and 0.1 GPa or less.

4. A cutting tool according to any one of claims 1 to 3, wherein the residual stress Z of the third layer is -0.3 GPa or more and 0.4 GPa or less.

5. A cutting tool according to any one of claims 1 to 4, wherein the thickness of the first layer is 3 μm or more and 15 μm or less.

6. A cutting tool according to any one of claims 1 to 5, wherein the second layer has a thickness of 3 μm or more and 15 μm or less.

7. A cutting tool according to any one of claims 1 to 6, wherein the thickness of the third layer is 2 μm or more and 4 μm or less.

Citation Information

Patent Citations

  • Coated cutting tool

    JP2020037150A

  • Coated cutting tool

    JP2020116645A

  • Covered cermet cutting tool and its manufacture

    JP1993177413A

  • Surface-coated cutting tool

    JP2008168365A

  • Coated tool and cutting tool provided with same

    WO2019181786A1