Two-stage flotation process for low-grade mixed potassium salt

A potassium mixed salt, low-grade technology, applied in the field of potassium salt flotation, can solve the problem that the processing capacity cannot meet the ore output of potash mixed salt ore in salt fields, turn into langbeinite and anhydrous langbeinite, and potassium mixed salt flotation Solve problems such as separation difficulties, achieve the effect of improving process adaptability and reliability, good product quality, and improving K+ recovery rate

CN104193425AActive Publication Date: 2014-12-10CHANGSHA DESIGN & RES INST OF CHEM IND MIN
5 Cites 13 Cited by

Patent Information

Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Publication Date
2014-12-10

Smart Images

  • Figure 1
    Figure 1
Patent Text Reader

Abstract

The invention discloses a two-stage flotation process for low-grade mixed potassium salt. The process comprises the following steps: (1) grinding low-grade mixed potassium salt until content of the salt with size fraction of -0.15mm is no less than 64.90% by mass; (2) transferring ore pulp obtained from the step (1) to a flotation machine for the first stage of flotation; (3) adding an anionic collector to coarse ore pulp obtained from the step (2) for the second stage of flotation; (4) totally combining potassium chloride concentrate obtained from the step (2) with the second stage of flotation concentrate obtained from the step (3), adding fresh water at a mass ratio of the concentrate to the fresh water of 1: (0.65-0.80), stirring at normal temperature and conducting a conversion reaction fore 1-2h, filtering and drying to obtain a finished potassium sulfate fertilizer product. The process disclosed by the invention has such advantages as simple process, low energy consumption, easy implementation of operation and high K<+> recovery rate, and is suitable for recovering a potassium resource from some low-grade mixed potassium salt complex in potassium mineral composition through flotation.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention belongs to the field of potassium salt flotation, and relates to a process for preparing potassium and magnesium fertilizers by using low-grade potassium mixed salt flotation, in particular to a process for preparing potassium and magnesium fertilizers by using low-grade potassium mixed salts to flotation potassium salt minerals in stages Two-stage flotation process. Background technique

[0002] Potassium-containing minerals mainly include potassium halite, carnallite, langbeinite, kaleolite, polyhalite, etc., and the potassium mixed salt mines obtained by drying the existing sulfate-type salt lake brine generally contain lentilite Magnesite (K 2 SO 4 · MgSO 4 ·6H 2 O), potassium chloride, Epsom salts (MgSO 4 ·7H 2 O) and sodium chloride, while potassium chloride and epsom salt will be partially converted into kainite (KCl MgSO 4 2.75H 2 O), if the temperature is higher again, kobeinite may also be converted into kobeinite (K 2 ...

Examples

Embodiment 1

[0021] This embodiment includes the following steps:

[0022] (1) will be composed as K + 4.23%, Na + 22.08%, Mg 2+ 3.57%, SO 4 2- 14.32%, Cl - 37.71% low-grade potash mixed salt raw ore, ground to -0.15mm particle size accounted for 64.90% of the mass content, to obtain pulp;

[0023] (2) Transfer the ore slurry obtained in step (1) to a flotation machine for one-stage flotation. The target minerals of the one-stage flotation are potassium chloride and kainite. The process flow is one rough and one fine. Collector CB-805 [3-hexadecyloxypropylamine hydrochloride, the molecular formula is C 16 h 33 —O—(CH 2 ) 3 NH 2 ·HCl] for pulping, the agent dosage is 120g / t raw ore, and the flotation time is 8min to obtain potassium chloride roughing concentrate (including kainite) and roughing pulp, and the obtained potassium chloride roughing concentrate (including potassium magnesia) and then selected, selected without adding drugs, flotation time 6min, to obtain potassiu...

Embodiment 2

[0029] This embodiment includes the following steps:

[0030] (1) will be composed as K + 4.23%, Na + 22.08%, Mg 2+ 3.57%, SO 4 2- 14.32%, Cl - The mass content of 37.71% low-grade potassium mixed salt grinding to -0.15mm particle size accounted for 65.87%, and the ore pulp was obtained;

[0031] (2) Transfer the ore slurry obtained in step (1) to a flotation machine for one-stage flotation. The target minerals of the one-stage flotation are potassium chloride and kainite. The process flow is one rough and one fine. Collector CB-805 [3-hexadecyloxypropylamine hydrochloride, the molecular formula is C 16 h 33 —O—(CH 2 ) 3 NH 2 ·HCl] for pulping, the agent dosage is 140g / t raw ore, and the flotation time is 7min to obtain potassium chloride roughing concentrate (including kainite) and roughing pulp, and the obtained potassium chloride roughing concentrate (including potassium magnesia) and then selected, selected without adding drugs, flotation time 5min, to obta...

Embodiment 3

[0037] This embodiment includes the following steps:

[0038] (1) will be composed as K + 4.23%, Na + 22.08%, Mg 2+ 3.57%, SO 4 2- 14.32%, Cl - 37.71% of the low-grade potassium mixed-salt raw ore was ground to -0.15mm particle size, accounting for 67.44%, and the pulp was obtained;

[0039] (2) Transfer the ore slurry obtained in step (1) to a flotation machine for one-stage flotation. The target minerals of the one-stage flotation are potassium chloride and kainite. The process flow is one rough and one fine. Collector CB-805 [3-hexadecyloxypropylamine hydrochloride, the molecular formula is C 16 h 33 —O—(CH 2 ) 3 NH 2 ·HCl] for pulping, the agent dosage is 160g / t raw ore, and the flotation time is 6min to obtain potassium chloride roughing concentrate (including kainite) and roughing pulp, and the obtained potassium chloride roughing concentrate (including potassium gallinite) and then selected, selected without adding drugs, flotation time 4min, to obtain p...