A thermal insulation and integrated technology, applied in the direction of covering/lining, construction, chemical instruments and methods, etc., can solve the problems of rough operation, unsafe construction, labor and labor, etc., and reduce the internal space temperature and production cost Reduce and save the effect of stone resources
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2015-05-06
- Estimated Expiration
- Not applicable · inactive patent
Smart Images
Figure 1
Abstract
Description
technical field
[0001] The invention belongs to the technical field of thermal insulation materials for building walls, and relates to an exterior wall panel profile integrated with reflective heat insulation and decorative surfaces. Background technique
[0002] Building thermal insulation and energy saving is one of the key points of my country's energy conservation work. With the further standardization of civil building energy-saving design "standards" and the implementation of the State Council's "Civil Building Energy Conservation Regulations", more and more new building materials and external wall thermal insulation systems have been proposed. Higher requirements require not only light weight, thermal insulation properties, but also outstanding compression, tensile, and anti-aging properties; reliable waterproof and impermeable properties, as well as fireproof, acid and alkali resistance, and anti-aging properties. Pollution performance must also meet the requirements...
Examples
Embodiment 1
[0027] The weight ratio of each component raw material of the facing layer is: 60 parts of waste rock debris, 5 parts of hollow glass microspheres, 1 part of vitrified microspheres, 1 part of rare earth metal oxide, 1 part of rutile, water-based 15 parts of emulsion, 3 parts of inorganic binder, 0.3 part of wood fiber, 0.3 part of polypropylene short fiber, 0.02 part of film-forming aid, 2 parts of water.
Embodiment 2
[0029] The weight ratio of each component raw material of the facing layer is: 65 parts of waste rock debris, 8 parts of hollow glass microspheres, 2.5 parts of vitrified microspheres, 2.5 parts of rare earth metal oxides, 2.5 parts of rutile, water-based 16.5 parts of emulsion, 3.5 parts of inorganic binder, 0.35 parts of wood fiber, 0.35 part of polypropylene short fiber, 0.025 part of film-forming aid, and 3 parts of water.
Embodiment 3
[0031] The weight ratio of each component raw material of the facing layer is: 70 parts of waste rock debris, 11 parts of hollow glass microspheres, 3.5 parts of vitrified microspheres, 3.5 parts of rare earth metal oxides, and 3.5 parts of rutile , 18.5 parts of water-based emulsion, 4.5 parts of inorganic binder, 0.45 parts of wood fiber, 0.45 part of polypropylene short fiber, 0.028 part of film-forming aid, and 4 parts of water.