A pultruded composite board

By using a three-layer structure of pultruded composite panels and combined with ultrasonic oscillation treatment, the problem of traditional building materials that are prone to water absorption, rot and rust is solved, and efficient building construction and protection effects are achieved.

CN108859304BActive Publication Date: 2024-10-11SHANDONG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN201810806366.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-07-20
Publication Date
2024-10-11
Estimated Expiration
2038-07-20

AI Technical Summary

Technical Problem

Wooden or steel panels in the traditional construction field are prone to absorbing water, rotting or rusting. The metal panel frame has a good affinity with cement, which makes demoulding difficult and may cause quality accidents and low construction efficiency.

Method used

A pultruded composite panel with a three-layer structure, including a high-modulus unidirectional fiber rigid layer in the core, a tough splitting-resistant layer of mixed fibers in the middle, and a high-strength impact-resistant layer of mixed fibers on the surface, using lamination arrangement and pultrusion process It is molded in one piece and uses ultrasonic oscillation treatment during fiber impregnation in resin to improve mechanical properties.

Benefits of technology

The composite panel has good resistance to deformation, splitting and impact, and is suitable for building reinforcement, secondary processing of thermoplastic profiles and traffic protection. It has low affinity with cement and is easy to dismantle after construction, avoiding the defects of traditional materials. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108859304B_ABST
    Figure CN108859304B_ABST
Patent Text Reader

Abstract

The present invention relates to a pultruded composite sheet, which belongs to the technical field of carbon fiber sheet preparation. The composite sheet of the present invention is composed of a three-layer structure, including: a pultruded rigid layer of the core, a middle mixed fiber fabric toughness and splitting resistance layer, and a surface mixed fiber fabric high-strength impact-resistant layer. The three-layer structure adopts a stacking arrangement and is integrally formed by a pultrusion process. The composite sheet has the ability to resist deformation due to the middle rigid core layer, and the middle splitting resistance layer and the surface impact resistance layer have both high toughness and impact resistance. It can be widely used in various building wall reinforcements, secondary processing of thermoplastic profiles, transportation, protection and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber plate preparation, and in particular to a carbon fiber composite plate with a multi-layer functional structure and comprehensive properties such as splitting resistance, high rigidity and impact resistance. Background Art

[0002] With the gradual expansion of the civilian market for composite materials, the composite materials of various infrastructures have gradually become a hot spot for research and application. In addition to the pultruded composite sucker rod preparation that is widely used in the oil field and the pultruded composite mandrel products that are widely used in the power field, the composite material sheets in the basic construction field are also mainly pultruded. This molding process is fast and simple for processing composite materials, with high production efficiency, good uniformity of molded products and high density. However, the wooden or steel sheets used in the traditional construction field are easy to absorb water, rot or rust. At the same time, the sheet frame of metal materials must solve the problem of demoulding difficulties caused by good affinity with cement during construction, which not only leads to low construction efficiency, but also is likely to cause quality accidents. In order to avoid many problems in the field of basic building materials, it is particularly necessary to study a composite material sheet prepared by pultrusion with multiple mechanical properties. Summary of the invention

[0003] In view of the problems existing in the above-mentioned prior art, the present invention aims to provide a pultruded composite board. The composite board of the present invention is composed of a three-layer structure, including: a pultruded rigid layer in the core, a middle mixed fiber fabric toughness and splitting resistant layer and a surface mixed fiber fabric high-strength impact-resistant layer. The three-layer structure adopts a stacking arrangement and is integrally formed by a pultrusion process. The composite board has the ability to resist deformation due to the middle rigid core layer, and the middle splitting resistant layer and the surface impact-resistant layer have both high toughness and impact resistance. It can be widely used in various building wall reinforcements, secondary processing of thermoplastic profiles, transportation, protection and other fields.

[0004] One of the purposes of the present invention is to provide a pultruded composite board.

[0005] A second object of the present invention is to provide a pultruded composite sheet with adjustable shape.

[0006] A third object of the present invention is to provide a pultruded composite sheet and an application of a pultruded composite sheet with adjustable shape.

[0007] To achieve the above-mentioned purpose, the present invention discloses the following technical solutions:

[0008] Firstly, the present invention discloses a pultruded composite board, which consists of a three-layer structure, including: a core rigid layer, an intermediate splitting-resistant layer, and a surface impact-resistant layer. The composite board is integrally formed by a pultrusion process, wherein the core rigid layer is formed by pultrusion of a high-modulus unidirectional fiber array impregnated with resin glue; while the rigid core layer is pultruded, prepreg fabric layers formed by mixed fiber multidimensional fabric impregnated with resin are synchronously laminated and pultruded on the upper and lower surfaces of the rigid core layer to form the intermediate splitting-resistant layer; a prepreg fabric layer formed by mixed fiber multidimensional fabric impregnated with resin is synchronously pultruded on the outermost surface of the board to form the surface impact-resistant layer.

[0009] In the rigid layer of the core, the high modulus unidirectional fibers are selected from one or more of carbon fibers, PBO fibers, and aramid fibers.

[0010] In the rigid layer of the core, the carbon fiber therein can be selected from any one or more of M40, M40J, M55, M60, and M60J, and the mixing ratio of the carbon fiber can be flexibly adjusted according to the use requirements.

[0011] In the rigid layer of the core, the resin glue is selected from thermosetting or thermoplastic resin emulsion.

[0012] Preferably, the thermosetting resin is any one of epoxy resin, phenolic resin, unsaturated polyester resin, urea-formaldehyde resin, thermosetting polyurethane resin, silicone resin, furan resin and the like.

[0013] Preferably, the thermoplastic resin is any emulsion of polyurethane, polyethylene, polypropylene, polyether ketone, polyether ether ketone, polyphenylene sulfide, polyamide, and polyimide.

[0014] Preferably, the resin content in the rigid layer of the core is within the range of 30-60% and can be flexibly adjusted according to needs.

[0015] Preferably, the width of the rigid layer of the core is within the range of 50-300 mm and can be flexibly adjusted according to needs.

[0016] In the middle splitting resistant layer, the mixed fiber multi-dimensional fabric is a two-dimensional woven structure or a three-dimensional fabric structure formed by weaving fibers.

[0017] Preferably, the two-dimensional woven structure can be any one of plain weave, twill weave and satin weave.

[0018] Preferably, the three-dimensional woven structure can be any one of three-dimensional four-directional, three-dimensional five-directional, three-dimensional six-directional and three-dimensional seven-directional.

[0019] In the middle splitting-resistant layer, the fibers therein are selected from any one or more combinations of aramid fibers, UHMWPE fibers, and PBO fibers, and the mixing ratio can be flexibly adjusted according to needs.

[0020] In the intermediate splitting-resistant layer, the resin therein is selected from thermosetting or thermoplastic resin emulsion.

[0021] Preferably, the thermosetting resin can be any one of epoxy resin, phenolic resin, unsaturated polyester resin, urea-formaldehyde resin, thermosetting polyurethane resin, silicone resin, furan resin and the like.

[0022] Preferably, the thermoplastic resin can be selected from any emulsion of polyurethane, polyethylene, polypropylene, polyether ketone, polyether ether ketone, polyphenylene sulfide, polyamide, and polyimide.

[0023] Preferably, in the middle splitting resistant layer, the resin content is adjusted within the range of 30-60% as required.

[0024] The width of the middle splitting-resistant layer can be flexibly adjusted within the range of 50-300 mm according to needs.

[0025] In the surface impact-resistant layer, the mixed fiber multi-dimensional fabric is a two-dimensional woven structure or a three-dimensional fabric structure formed by weaving fibers.

[0026] Preferably, the two-dimensional woven structure can be any one of plain weave, twill weave and satin weave.

[0027] Preferably, the three-dimensional woven structure can be any one of three-dimensional four-directional, three-dimensional five-directional, three-dimensional six-directional and three-dimensional seven-directional.

[0028] In the surface impact-resistant layer, the fibers therein are selected from any one or more combinations of aramid fibers, glass fibers, and PBO fibers, and the mixing ratio thereof can be flexibly adjusted according to requirements.

[0029] In the surface impact-resistant layer, the resin is selected from thermosetting or thermoplastic resin emulsion.

[0030] Preferably, the thermosetting resin can be any one of epoxy resin, phenolic resin, unsaturated polyester resin, urea-formaldehyde resin, thermosetting polyurethane resin, silicone resin, furan resin and the like.

[0031] Preferably, the thermoplastic resin can be selected from any emulsion of polyurethane, polyethylene, polypropylene, polyether ketone, polyether ether ketone, polyphenylene sulfide, polyamide, and polyimide.

[0032] Preferably, the width of the surface impact-resistant layer is within the range of 50-300 mm and can be flexibly adjusted according to needs.

[0033] Preferably, the resin content in the surface impact-resistant layer is adjusted within the range of 30-60% as required.

[0034] Preferably, the overall thickness of the pultruded composite sheet prepared by the present invention is adjusted within the range of 1-20 mm as required.

[0035] Secondly, the present invention also provides a shape-adjustable pultruded composite board, which is characterized in that the resin used to impregnate the fibers in the core rigid layer, the middle splitting-resistant layer, and the surface impact-resistant layer structure of the board are all thermoplastic resin emulsions. Since thermoplastic resins have the properties of softening when heated and hardening when cooled, and do not undergo chemical reactions during hot and cold changes, such properties can be maintained no matter how many times heating and cooling are repeated. After the fibers are impregnated with thermoplastic resin emulsion, the resulting composite board can be heated again to change its shape after molding according to specific shape requirements, so that the board prepared by the present invention can be further adapted to more environments.

[0036] Furthermore, the method for preparing the pultruded composite board of the present invention further comprises using ultrasonic oscillation treatment during the process of impregnating the fibers with resin.

[0037] The ultrasonic time is the same as the impregnation time, and preferably, the ultrasonic frequency is 150Khz-300Khz. This is because the macromolecular resin only forms a surface film on the surface of the woven fiber, and is not well impregnated into the carbon fiber preform fabric. As a result, there are a large number of micropores in the manufactured composite board, which greatly reduces the mechanical properties of the board cross section. The board prepared by the present invention is mainly a force-bearing component. Insufficient mechanical properties will not only affect the service life of the board, but also bring serious safety hazards. Therefore, after further research, the present invention found that the use of ultrasonic treatment while impregnating the fiber with resin can solve the above problems well, because ultrasonic treatment can just accelerate the movement of resin molecules into the fiber preform fabric, so that the resin can be fully distributed in the fiber preform fabric, solving the problem of affecting the mechanical properties of the board.

[0038] Finally, the present invention also discloses the application of the pultruded composite sheet and the shape-adjustable pultruded composite sheet in building wall reinforcement, secondary processing of thermoplastic profiles, and transportation and protection fields.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The composite board of the present invention is composed of a three-layer structure, including: a pultruded rigid layer in the core, a middle mixed fiber fabric toughness and splitting resistance layer and a surface mixed fiber fabric high-strength impact-resistant layer. The three-layer structure is arranged in a stacked manner and is integrally formed by a pultrusion process. The composite board has the ability to resist deformation due to the middle rigid core layer, and the middle splitting resistance layer and the surface impact-resistant layer have both high toughness and impact resistance. Therefore, the composite board can be widely used in various building wall reinforcements, secondary processing of thermoplastic profiles, and transportation, protection and other fields. At the same time, the composite board prepared by the present invention has low affinity with cement. After construction, it is convenient and quick to dismantle the composite board, which can well solve the problem that wooden or steel boards used in the traditional construction field are easy to absorb water, rot or rust, and the difficulty of demoulding caused by the good affinity of the board frame of the metal material with cement, which may cause quality accidents and low construction efficiency.

[0041] (2) The shape-adjustable pultruded composite sheet prepared by the present invention using thermoplastic resin can be reheated to change its shape according to specific shape requirements after molding, so that the sheet prepared by the present invention can be further applied to more environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The drawings in the specification, which constitute a part of the present application, are used to provide further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.

[0043] Figure 1 It is a schematic structural diagram of the pultruded composite plate of the present invention.

[0044] The symbols in the accompanying drawings represent: 1-pultruded rigid layer of the core, 2-intermediate splitting resistant layer, 3-surface impact resistant layer. DETAILED DESCRIPTION

[0045] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0046] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0047] As introduced in the background technology, wooden or steel plates used in traditional construction fields are prone to water absorption, rot or rust. At the same time, the plate frame of metal materials must also solve the problem of demolding difficulties caused by the good affinity with cement during construction, which may cause quality accidents and low construction efficiency. Therefore, the present invention proposes a pultruded composite plate, and the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.

[0048] The composite board material prepared in the embodiment of the present invention is integrally formed by a pultrusion process, specifically: the rigid layer of the core is formed by pultrusion of a high modulus unidirectional fiber array impregnated with resin glue; while the rigid core layer is pultruded, prepreg fabric layers formed by mixed fiber multidimensional fabric impregnated with resin are synchronously stacked and pultruded on the upper and lower surfaces of the rigid core layer to form a middle splitting-resistant layer; a prepreg fabric layer formed by mixed fiber multidimensional fabric impregnated with resin is synchronously pultruded on the outermost surface of the board to form a surface impact-resistant layer.

[0049] Example 1

[0050] like Figure 1 As shown, a pultruded composite plate comprises: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 50 mm wide unidirectional fabric of M40 carbon fiber and PBO fiber with a mixed ratio of 1:1 to form a reinforced structure, and the unidirectional fabric is pre-impregnated with an epoxy resin emulsion with a resin content of 30% before pultrusion, and the thickness of the final pultruded rigid core layer is 1 mm.

[0051] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a plain fabric structure with a width of 50 mm, which is woven by mixing aramid fiber KEVLAR129 and UHMWPE fiber in a mixing ratio of 2:1. It is pre-impregnated with phenolic resin emulsion with a resin content of 40% before pultrusion. The thickness of the final pultruded middle splitting-resistant layer is 5 mm.

[0052] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a three-dimensional four-way three-dimensional fabric structure with a width of 50 mm, which is woven by mixing glass fiber and PBO fiber in a mixing ratio of 1:2. It is pre-impregnated with thermosetting polyurethane resin emulsion with a resin content of 38% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 2 mm.

[0053] The final overall thickness of the pultruded composite plate prepared in this embodiment is 7 mm.

[0054] Example 2

[0055] like Figure 1As shown, a pultruded composite sheet includes: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 100mm wide M60J carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 2:1 to form a reinforcement structure, and the unidirectional fabric is pre-impregnated with a urea-formaldehyde resin emulsion with a resin content of 44% before pultrusion. The thickness of the final pultruded rigid core layer is 2mm.

[0056] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a satin fabric structure with a width of 100 mm, which is woven by a mixture of aramid fiber KEVLAR29 and UHMWPE fiber in a mixing ratio of 1.5:1. It is pre-impregnated with a polyurethane emulsion with a resin content of 55% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 2 mm.

[0057] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a three-dimensional four-directional three-dimensional fabric structure with a width of 100 mm, which is woven by a mixture of glass fiber and aramid fiber in a mixing ratio of 3:1. It is pre-impregnated with polyetheretherketone emulsion with a resin content of 42% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 2 mm.

[0058] The final overall thickness of the pultruded composite plate prepared in this embodiment is 5 mm.

[0059] Example 3

[0060] like Figure 1 As shown, a pultruded composite sheet includes: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 150mm wide M55 carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 3:1 to form a reinforcement structure, and the unidirectional fabric is pre-impregnated with an unsaturated polyester resin emulsion with a resin content of 55% before pultrusion. The thickness of the final pultruded rigid core layer is 1.5mm.

[0061] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It is a three-dimensional seven-directional fabric structure with a width of 150 mm, which is woven by a mixture of aramid fiber KEVLAR49 and UHMWPE fiber in a mixing ratio of 2.5:1. It is pre-impregnated with polyphenylene sulfide emulsion with a resin content of 35% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 4 mm.

[0062] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a twill fabric structure with a width of 150 mm, which is woven by S glass fiber and PBO fiber with a mixing ratio of 6:1. It is pre-impregnated with epoxy resin emulsion with a resin content of 60% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 3 mm.

[0063] The final overall thickness of the pultruded composite plate prepared in this embodiment is 8 mm.

[0064] Example 4

[0065] like Figure 1 As shown, a pultruded composite sheet includes: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 300mm wide M60 carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 2.5:1 to form a reinforcement structure, and the unidirectional fabric is pre-impregnated with an epoxy resin emulsion with a resin content of 45% before pultrusion. The thickness of the final pultruded rigid core layer is 1.2mm.

[0066] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a twill fabric structure with a width of 300mm, which is woven by a mixture of aramid fiber KEVLAR129 and UHMWPE fiber in a mixing ratio of 3:1. It is pre-impregnated with a polyurethane emulsion with a resin content of 43% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 4mm.

[0067] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a satin fabric structure with a width of 300 mm, which is woven by S glass fiber and PBO fiber in a mixed ratio of 3:2. It is pre-impregnated with phenolic resin emulsion with a resin content of 60% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 2.5 mm.

[0068] The final overall thickness of the pultruded composite plate prepared in this embodiment is 7 mm.

[0069] Example 5

[0070] like Figure 1 As shown, a pultruded composite plate comprises: a core rigid layer, an intermediate splitting-resistant layer, and a surface impact-resistant layer, wherein the core rigid layer adopts a 50 mm wide unidirectional fabric of M40J carbon fiber and polyamide fiber KEVLAR129 with a mixed ratio of 1:1 to form a reinforced structure, and the unidirectional fabric is pre-impregnated with polyethylene with a resin content of 60% before pultrusion, and the thickness of the final pultruded rigid core layer is 8 mm.

[0071] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a three-dimensional four-directional fabric structure with a width of 50 mm, which is woven by mixing aramid fiber KEVLAR129 and PBO fiber in a mixing ratio of 2:1. It is pre-impregnated with polyethylene emulsion with a resin content of 30% before pultrusion. The thickness of the final pultruded middle splitting-resistant layer is 6 mm.

[0072] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a three-dimensional four-way three-dimensional fabric structure with a width of 50 mm, which is woven by mixing glass fiber and PBO fiber in a mixing ratio of 1:2. It is pre-impregnated with polypropylene emulsion with a resin content of 30% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 7 mm.

[0073] The final overall thickness of the pultruded composite plate prepared in this embodiment is 20 mm.

[0074] Example 6

[0075] like Figure 1 As shown, a pultruded composite plate comprises: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 100mm wide unidirectional fabric of M40 carbon fiber and PBO fiber with a mixed ratio of 1:2 to form a reinforced structure, and the unidirectional fabric is pre-impregnated with a phenolic resin emulsion with a resin content of 50% before pultrusion, and the thickness of the final pultruded rigid core layer is 1mm.

[0076] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a three-dimensional five-directional fabric structure with a width of 50 mm, which is woven by mixing aramid fiber KEVLAR129 and UHMWPE fiber in a mixing ratio of 2:1. It is pre-impregnated with epoxy resin emulsion with a resin content of 60% before pultrusion. The thickness of the final pultruded middle splitting-resistant layer is 5 mm.

[0077] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a plain three-dimensional fabric structure with a width of 50 mm, which is woven by mixing glass fiber and PBO fiber in a mixing ratio of 3:2. It is pre-impregnated with polyethylene emulsion with a resin content of 40% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 2 mm.

[0078] The final overall thickness of the pultruded composite plate prepared in this embodiment is 7 mm.

[0079] Example 7

[0080] like Figure 1As shown, a pultruded composite sheet includes: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 150mm wide M55 carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 2:1 to form a reinforcement structure, and the unidirectional fabric is pre-impregnated with a polyetherketone emulsion with a resin content of 35% before pultrusion. The thickness of the final pultruded rigid core layer is 1.5mm.

[0081] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It is a three-dimensional six-directional fabric structure with a width of 150 mm, which is woven by a mixture of aramid fiber KEVLAR49 and UHMWPE fiber in a mixing ratio of 2:1. It is pre-impregnated with polyetherketone emulsion with a resin content of 40% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 4 mm.

[0082] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a three-dimensional five-directional fabric structure with a width of 150 mm, which is woven by S glass fiber and PBO fiber in a mixing ratio of 4:1. It is pre-impregnated with polyamide emulsion with a resin content of 60% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 3 mm.

[0083] The final overall thickness of the pultruded composite plate prepared in this embodiment is 8 mm.

[0084] Example 8

[0085] like Figure 1 As shown, a pultruded composite sheet includes: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 300mm wide M50 carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 2:1 to form a reinforcement structure, and the unidirectional fabric is pre-impregnated with a polyetheretherketone emulsion with a resin content of 35% before pultrusion. The thickness of the final pultruded rigid core layer is 0.3mm.

[0086] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a twill fabric structure with a width of 300 mm, which is woven by a mixture of aramid fiber KEVLAR129 and UHMWPE fiber in a mixing ratio of 3:1. It is pre-impregnated with urea-formaldehyde resin emulsion with a resin content of 40% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 0.4 mm.

[0087] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a three-dimensional six-directional fabric structure with a width of 300 mm, which is woven by S glass fiber and PBO fiber in a mixing ratio of 3:2. It is pre-impregnated with urea-formaldehyde resin emulsion with a resin content of 60% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 0.4 mm.

[0088] The final overall thickness of the pultruded composite plate prepared in this embodiment is 1 mm.

[0089] Example 9

[0090] like Figure 1 As shown, a pultruded composite sheet includes: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer adopts a 100mm wide M60 carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 2:1 to form a reinforcement structure, and the unidirectional fabric is pre-impregnated with a polyphenylene sulfide emulsion with a resin content of 35% before pultrusion. The thickness of the final pultruded rigid core layer is 2mm.

[0091] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It adopts a satin fabric structure with a width of 100 mm, which is woven by a mixture of aramid fiber KEVLAR29 and UHMWPE fiber in a mixing ratio of 1.5:1. It is pre-impregnated with a polyether ether emulsion with a resin content of 50% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 2 mm.

[0092] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a three-dimensional four-directional three-dimensional fabric structure with a width of 100 mm, which is woven by a mixture of glass fiber and aramid fiber in a mixing ratio of 3:1. Before pultrusion, it is pre-impregnated with polyphenylene sulfide emulsion with a resin content of 36%. The thickness of the final pultruded surface impact-resistant layer is 2 mm.

[0093] The final overall thickness of the pultruded composite plate prepared in this embodiment is 5 mm.

[0094] Example 10

[0095] like Figure 1 As shown, a pultruded composite plate comprises: a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer, wherein the core rigid layer is reinforced by a 150mm wide M55 carbon fiber and PBO fiber unidirectional fabric with a mixed ratio of 3:1, and the unidirectional fabric is pre-impregnated with a polyimide emulsion with a resin content of 45% before pultrusion. The thickness of the final pultruded rigid core layer is 6mm.

[0096] The middle splitting-resistant layer covers the upper and lower surfaces of the core rigid layer. It is a three-dimensional seven-directional fabric structure with a width of 150 mm, which is woven by mixing aramid fiber KEVLAR49 and UHMWPE fiber in a mixing ratio of 2.5:1. It is pre-impregnated with furan resin emulsion with a resin content of 35% before pultrusion. The thickness of the tough splitting-resistant layer of the final pultruded middle mixed fiber fabric is 4 mm.

[0097] The surface impact-resistant layer covers the upper and lower surfaces of the middle splitting-resistant layer. It adopts a twill fabric structure with a width of 150 mm, which is woven by S glass fiber and PBO fiber in a mixing ratio of 6:1. It is pre-impregnated with polyetherketone emulsion with a resin content of 30% before pultrusion. The thickness of the final pultruded surface impact-resistant layer is 5 mm.

[0098] The final overall thickness of the pultruded composite plate prepared in this embodiment is 14 mm.

[0099] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A pultruded composite sheet, characterized in that: The composite sheet is composed of a core rigid layer, an intermediate splitting resistant layer, and a surface impact resistant layer. The composite sheet is integrally formed by a pultrusion process, wherein the core rigid layer is pultruded by a high modulus fiber unidirectional fabric impregnated with a resin emulsion; while the core rigid layer is pultruded, prepreg fabric layers formed by a mixed fiber multidimensional fabric impregnated with a resin emulsion are synchronously stacked and pultruded on the upper and lower surfaces of the core rigid layer to form the intermediate splitting resistant layer; prepreg fabric layers formed by a mixed fiber multidimensional fabric impregnated with a resin emulsion are synchronously stacked and pultruded on the upper and lower surfaces of the intermediate splitting resistant layer to form the surface impact resistant layer; In the middle splitting-resistant layer and the surface impact-resistant layer, the mixed fiber multi-dimensional fabric is a two-dimensional woven structure or a three-dimensional woven structure woven from fibers; Ultrasonic oscillation treatment is used during the process of fiber impregnation with resin emulsion; the ultrasonic time is the same as the impregnation time, and the ultrasonic frequency is 150kHz-300kHz; In the core rigid layer, the high modulus fibers consist of carbon fibers and PBO fibers, or carbon fibers and aramid fibers; The carbon fiber is selected from any one or more of M40, M40J, M55, M60, and M60J; The core rigid layer, the middle splitting resistant layer and the surface impact resistant layer are made of thermosetting resin or thermoplastic resin in the resin emulsion; The thermosetting resin is selected from any one of epoxy resin, phenolic resin, unsaturated polyester resin, urea-formaldehyde resin, thermosetting polyurethane resin, silicone resin, and furan resin; The thermoplastic resin is selected from any one of polyurethane, polyethylene, polypropylene, polyether ketone, polyether ether ketone, polyphenylene sulfide, polyamide, and polyimide; In the middle splitting-resistant layer, the fibers are a combination of aramid fibers and UHMWPE fibers; In the surface impact-resistant layer, the fibers are a combination of glass fibers and PBO fibers; The width of the core rigid layer, the middle splitting resistant layer and the surface impact resistant layer are all controlled within the range of 50-300mm; The overall thickness of the pultruded composite sheet is controlled within the range of 1-20 mm; In the core rigid layer, the middle splitting resistant layer and the surface impact resistant layer, the resin content in the resin emulsion is controlled within the range of 30-60wt%.

2. The pultruded composite sheet according to claim 1, characterized in that: The two-dimensional weaving structure is selected from any one of plain weave, twill weave and satin weave; The three-dimensional braided structure is selected from any one of three-dimensional four-directional, three-dimensional five-directional, three-dimensional six-directional, and three-dimensional seven-directional.

3. Application of the composite board material as claimed in any one of claims 1 to 2 in building wall reinforcement, secondary processing of thermoplastic profiles, and in the fields of transportation and protection.

Citation Information

Patent Citations

  • Preparation method for novel carbon fiber pultrusion plate

    CN103419383A

  • Hybrid fiber elastic web composite material bulletproof plug board and preparation method thereof

    CN104848746A

  • Structure of extruded material with continuous fibre reinforcement and method for manufacturing thereof

    CN1204572A

  • Pultrusion composite board

    CN209700001U

  • Panel for formwork made by thermoplastic compoundmaterial

    KR1020060122044A