Ultra-thin metal composite bipolar plate and preparation method thereof and fuel cell containing the same

By using a method for preparing ultrathin metal composite bipolar plates, the problems of excessive thickness and insufficient flow channel size in PEMFC bipolar plates have been solved, resulting in reduced fuel cell volume and increased energy density, lower production costs, and suitability for industrial applications.

CN109360998BActive Publication Date: 2024-11-12SHANDONG DAIQING NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811230641.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-10-22
Publication Date
2024-11-12
Estimated Expiration
2038-10-22

AI Technical Summary

Technical Problem

Existing proton exchange membrane fuel cells (PEMFCs) have thick and heavy bipolar plates, and the flow channel size cannot meet the battery performance requirements, resulting in low energy density, high production costs, and complex manufacturing processes.

Method used

An ultrathin metal composite bipolar plate is fabricated by using precision coating and laser etching technology to prepare ultra-fine flow channels, combined with bonding and pressing processes. The ultrathin metal composite bipolar plate includes a cathode, an anode, and a liquid flow field plate, with a flow channel depth and width of 50-500 micrometers.

Benefits of technology

This technology has achieved a reduction in fuel cell size, an increase in energy density, a simplification of the manufacturing process, a reduction in cost, and good uniformity in the flow channel design, resulting in high current density and suitability for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109360998B_ABST
    Figure CN109360998B_ABST
Patent Text Reader

Abstract

The present invention relates to an ultra-thin metal composite bipolar plate, a preparation method thereof, and a fuel cell containing the same. Precision coating and laser etching technology are used to prepare a flow field with ultra-fine flow channels on the surface of an ultra-thin metal substrate. Compared with traditional bipolar plates, the bipolar plate has both ultra-thin thickness and ultra-fine flow channels, which can effectively reduce the volume of the fuel cell, increase the membrane electrode current density, and thus increase the energy density of the battery stack. The present invention does not require the design and manufacture of molds, has a short production cycle, can achieve industrial batch production, and reduce the cost of fuel cells. The present invention also relates to a fuel cell prepared with such an ultra-thin metal composite bipolar plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of fuel cells, and in particular to an ultra-thin metal composite bipolar plate, a preparation method thereof, and a fuel cell comprising the same. Background Art

[0002] Fuel cells are highly efficient green power generation devices that can directly convert chemical energy stored in fuels such as hydrogen and oxidants such as air into electrical energy in an efficient and environmentally friendly manner. Among them, proton exchange membrane fuel cells (PEMFCs) have the advantages of high efficiency and energy saving, stable operation, moderate operating temperature, and short cold start time. They have important application prospects in the fields of automotive and marine power supply, backup power supply, combined heat and power, special military use, etc.

[0003] At present, how to improve the energy density of PEMFC and reduce production costs is an important issue facing its large-scale commercialization. The main measures include selecting lower-cost materials, reducing the amount of materials used, simplifying or changing the battery structure, optimizing the production process of batteries and their components, and realizing mass production.

[0004] The main components of the PEMFC stack include membrane electrode, diffusion layer, bipolar plate, and end plate. Among these components, the end plate is only two at each end of the stack composed of dozens or hundreds of single cells, and the membrane electrode is only tens of microns. The two occupy only a small part (about 20%) of the volume of the entire PEMFC stack, and the graphite bipolar plate used in the traditional PEMFC stack is 3-8 microns thick. Therefore, the bipolar plate occupies the vast majority of the stack volume (about 70-80%). Therefore, in order to reduce the volume of PEMFC and increase energy density, the preparation of bipolar plates as thin as possible is the most important measure. The bipolar plate (also known as the flow field plate) is the core component of the fuel cell, playing the role of gas barrier, gas diversion and distribution, conductivity, and support for the membrane electrode. Generally, when fuel and oxidant enter a fuel cell composed of a membrane electrode, a diffusion layer, a bipolar plate, and a seal, they must first pass through the flow field on the bipolar plate to be distributed to the gas diffusion layer, then enter the catalyst layer to undergo an electrocatalytic reaction and be converted into electrical energy. The generated water diffuses to the surface of the gas diffusion layer and is then discharged from the fuel cell through the flow field.

[0005] Traditional PEMFC bipolar plates are made by machining flow channels on graphite plates. Since graphite is brittle and has limited mechanical strength, the thickness of the graphite bipolar plates and the size of the grooves and ridges of the flow field carved on them are relatively large, mostly in the order of several millimeters, which results in thick and heavy PEMFC stacks with low energy density. Later, people mixed graphite or carbon materials with resins and used a die-casting method to directly prepare composite bipolar plates with flow channels. Although this can reduce manufacturing costs, it is only suitable for mass production. At the same time, due to problems with the mold and preparation process, the flow channel width of this die-cast bipolar plate cannot be made very narrow, mostly above 400 microns. At the same time, the plates prepared by this process cannot be made very thin due to material strength limitations, and their overall thickness can only be reduced to 2-4 mm.

[0006] Another bipolar plate material is metal bipolar plates, which are mostly made of stainless steel or titanium alloy sheets stamped into flow channel parts, and then assembled with other parts through bonding or welding. This method can also be produced on a large scale, but the process is more complicated. The initial investment in mold preparation is huge, and due to the limitation of mold accuracy, its thickness can only be about 1-2 mm. How to control the stress and deformation of metal sheets during the forming process is also a big problem.

[0007] In fuel cells, the size of the flow channel plays an important role in battery performance. In recent years, there are more or less deficiencies in the newly developed and designed flow field plates in various countries around the world. For example, the airflow distribution of the flow field plate is not uniform enough, the water generated by the reaction is easy to accumulate and difficult to discharge, the flow field structure design is easy to cause reaction dead zones, and the local temperature of the membrane electrode is too high, which affects the battery operation performance. Generally speaking, the narrower the flow channel, the narrower the flow channel in the effective working area, the more uniform the gas distribution and heat transfer, and the higher the current density the battery can achieve. However, due to the limitation of mold precision, the flow channel width of mold-cast composite graphite plates or stamped metal bipolar plates can only reach 0.3-1.0 mm, which is still difficult to meet battery requirements. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a process for preparing a composite bipolar plate with ultra-thin and ultra-fine flow channels, and a proton exchange membrane fuel cell (PEMFC) using the composite bipolar plate in view of the deficiencies of the prior art.

[0009] The present invention relates to an ultra-thin metal composite bipolar plate, comprising: a cathode flow field single plate, the cathode flow field single plate comprising an ultra-thin metal substrate and a conductive adhesive layer coated on one side of the ultra-thin metal substrate, the conductive adhesive layer of the cathode flow field single plate having an oxygen / air flow field; an anode flow field single plate, the anode flow field single plate comprising an ultra-thin metal substrate and a conductive adhesive layer coated on one side of the ultra-thin metal substrate, the conductive adhesive layer of the anode flow field single plate having a hydrogen flow field having an ultra-fine flow channel etched by laser; a liquid flow field single plate, the liquid flow field single plate comprising an ultra-thin metal substrate and a conductive adhesive layer coated on one side of the ultra-thin metal substrate, the conductive adhesive layer of the liquid flow field single plate having a liquid flow field having an ultra-fine flow channel etched by laser; the ultra-thin metal substrate surface of the cathode flow field single plate is bonded and connected to the ultra-thin metal substrate surface of the liquid flow field single plate, and the conductive adhesive layer surface of the liquid flow field single plate is bonded and connected to the ultra-thin metal substrate surface of the anode flow field single plate.

[0010] Further, one end of the ultra-thin metal composite bipolar plate is provided with an oxygen / air inlet, a liquid inlet and a hydrogen inlet, and the oxygen / air inlet, the liquid inlet and the hydrogen inlet are all hole-shaped flow channels formed by stacking through holes correspondingly arranged on the cathode flow field single plate, the anode flow field single plate and the liquid flow field plate; the other end of the ultra-thin metal composite bipolar plate is provided with an oxygen / air outlet, a liquid outlet and a hydrogen outlet, and the oxygen / air outlet, the liquid outlet and the hydrogen outlet are all hole-shaped flow channels formed by stacking through holes correspondingly arranged on the cathode flow field single plate, the anode flow field single plate and the liquid flow field plate;

[0011] The oxygen / air inlet and the oxygen outlet are both connected to the oxygen flow field, the liquid inlet and the liquid outlet are both connected to the liquid flow field, and the hydrogen inlet and the hydrogen outlet are both connected to the hydrogen flow field.

[0012] Furthermore, the oxygen / air flow field includes a plurality of ultrafine channels, the depth of the ultrafine channels is 50-500 microns, and the width of the ultrafine channels is 50-500 microns; the liquid flow field includes a plurality of ultrafine channels, the depth of the ultrafine channels is 50-500 microns, and the width of the ultrafine channels is 50-500 microns; the hydrogen flow field includes a plurality of ultrafine channels, the depth of the ultrafine channels is 50-500 microns, and the width of the ultrafine channels is 50-500 microns.

[0013] The present invention also provides a method for preparing an ultra-thin metal composite bipolar plate, comprising the following steps:

[0014] S1) preparing a cathode flow field single plate, an anode flow field single plate and a liquid flow field single plate respectively by precision coating and laser etching technology;

[0015] S2) bonding and pressing the cathode flow field single plate, the anode flow field single plate and the liquid flow field single plate together to obtain an ultra-thin metal bipolar plate.

[0016] Further, the step S1) includes:

[0017] S1-1) cutting the ultra-thin metal substrate into sheets of designed size and shape, punching three through holes at both ends of the sheet, washing it, and drying it for later use;

[0018] S1-2) uniformly coating a layer of polymer-based conductive adhesive layer on one side of the ultra-thin metal sheet by precision coating technology, and obtaining a coated substrate having a conductive adhesive layer of a certain thickness by heat treatment;

[0019] S1-3) The coated substrate is placed on the base of the laser etching equipment, fixed by a vacuum adsorption device, and then laser-etched according to the pre-designed drawings of the hydrogen flow field, oxygen / air flow field and liquid flow field shapes to obtain a cathode flow field single plate, an anode flow field single plate and a liquid flow field single plate with ultra-fine flow channels.

[0020] Furthermore, the step S2) includes: taking the cathode flow field single plate, the anode flow field single plate and the liquid flow field single plate prepared in step S1, coating the ultrafine metal substrate surface side of the cathode flow field single plate and the anode flow field single plate and the edge sealing area on both sides of the liquid flow field single plate with a sealing adhesive, and then aligning the three single plates in the order of the cathode flow field single plate, the ultrafine metal substrate and the anode flow field single plate, placing them in a pressing device and pressing them, and after the sealing adhesive is cured, an ultrathin metal composite bipolar plate is obtained.

[0021] Furthermore, the ultra-thin metal substrate is a surface-treated metal foil, and the metal foil is any one of stainless steel foil, gold foil, silver foil, copper foil, and titanium foil, with a thickness of 50-600 microns; the polymer-based conductive adhesive is a composite of a polymer and a conductive filler, and the polymer is a mixture of one or more of phenolic resin, epoxy resin, silicone resin, PEFT resin, urea-formaldehyde resin, ethylene propylene diene monomer resin, polyimide, etc., and the conductive filler is a mixture of one or more of silver powder, graphite powder, mesophase carbon microspheres, chopped carbon fibers, conductive carbon powder, graphene, carbon nanotubes, etc. The viscosity of the conductive adhesive is between 1000-20000 centipoise, the curing temperature is 50-150°C, the curing time is less than 6 hours, and the volume resistivity after curing is less than 0.1Ωcm.

[0022] Furthermore, the coating method is blade coating, extrusion coating or micro-gravure; the heat treatment temperature after coating is 50-200°C for 30 minutes to 6 hours, and the thickness of the adhesive layer after coating is 50-500 microns.

[0023] Furthermore, the sealing adhesive is a commercial silicone sealant, epoxy sealant or phenolic sealant, and its curing condition is required to be room temperature-150°C and the curing time is within 0.5-24 hours; the sealing adhesive is applied by brushing, spraying, roller coating or dispensing.

[0024] The beneficial effects of the present invention are as follows: compared with the prior art, the fuel cell bipolar plate prepared by the method has both ultra-thin thickness and ultra-fine flow channels, which can effectively reduce the volume of the fuel cell, increase the membrane electrode current density, and thus improve the energy density of the battery stack. In addition, the process has the characteristics of no external force impact, no deformation, and good flatness during the production process; no need for mold design and manufacturing, short production cycle, fast response, etc., which can realize industrialized batch production and reduce the cost of fuel cells.

[0025] The present invention also provides a proton exchange membrane fuel cell, comprising the ultrathin metal bipolar plate as described above, wherein a membrane electrode, a diffusion layer, an ultrathin metal bipolar plate, an end plate and other auxiliary components are stacked to obtain a proton exchange membrane fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of cathode (oxygen / air) flow field in an embodiment of the present invention;

[0027] Figure 2 Schematic diagram of anode (hydrogen) flow field in an embodiment of the present invention;

[0028] Figure 3 Schematic diagram of liquid flow field in an embodiment of the present invention;

[0029] Figure 4 It is a schematic diagram of the cross-sectional combination of the cathode flow field plate, the anode flow field plate, the liquid flow field plate and the bipolar plate in an embodiment of the present invention.

[0030] Description of reference numerals:

[0031] 1. Cathode flow field single plate, 2. Anode flow field single plate, 3 Liquid flow field single plate, 4 Hydrogen inlet, 5 Hydrogen outlet, 6. Liquid outlet, 7. Oxygen outlet, 8. Oxygen / air inlet, 9. Liquid inlet, 10. Ridge, 11. Flow channel, 12. Oxygen / air flow field, 13 Oxygen / air flow field edge sealing area, 14. Hydrogen flow field, 15. Hydrogen flow field edge sealing area, 16. Liquid flow field, 17. Liquid flow field edge sealing area, 18. Metal substrate, 19. Conductive adhesive layer. DETAILED DESCRIPTION

[0032] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0033] The ultra-thin metal double-plate and its preparation method, as well as the proton exchange membrane fuel cell provided by the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0034] It should be noted that the drawings of the present invention are only schematic diagrams provided for the convenience of describing the embodiments of the present invention, and are not drawn to scale. The disclosed embodiments are only demonstrations of the present invention that may be implemented in a variety of alternative forms. The specific details and process conditions disclosed herein are not to be construed as limitations, but are only basic representations of any aspect of the present invention or basic representations to teach those skilled in the art to use the present invention in a variety of ways. In addition, those skilled in the art may also make other changes within the spirit of the present invention. Of course, these changes made in accordance with the spirit of the present invention should be included in the scope of protection claimed by the present invention.

[0035] The present invention provides a method for preparing an ultra-thin composite double-plate, which comprises the following steps:

[0036] S1: Single board preparation

[0037] S1-1) Pre-cutting: The ultra-thin metal substrate for preparing the bipolar plate is cut according to the design size and shape of the bipolar plate (such as Figure 1-3 As shown), laser cutting or mechanical punching is used to cut corresponding holes at the fluid inlet and outlet positions, and sheets of corresponding sizes are cut, washed, and dried for later use.

[0038] S1-2) Coating: A layer of polymer-based conductive adhesive is evenly coated on one side of the ultra-thin metal sheet through precision coating technology, and a coated substrate with a conductive adhesive layer of a certain thickness is obtained through heat treatment.

[0039] S1-3) Laser etching to prepare flow field:

[0040] The coated substrate is placed on the base of the laser etching equipment and fixed by a vacuum adsorption device; the pre-designed drawings of the flow fields of hydrogen (anode), oxygen, air (cathode) and cooling liquid are input into the operating system of the laser etching equipment, and laser etching is performed according to the designed drawings to etch away the glue layer of the fluid flow channel part in the drawing to obtain cathode and anode flow field single plates and liquid flow single plates with grooves (i.e., flow channels) and ridge structures.

[0041] S2: Bonding and sealing

[0042] The cathode flow field plate, the anode flow field plate, the back side of the gas flow field, and the edge sealing areas on both sides of the liquid flow field plate are coated with sealing adhesive, and then the three plates are strictly aligned in sequence (that is, the gas flow field faces outward), placed in a pressing device and pressed, so that the three plates fit tightly, and pressed at a certain temperature for a certain time. After the sealing adhesive is cured, the ultra-thin metal bipolar plate of the present invention is obtained.

[0043] In the above step S1-1:

[0044] The substrate for preparing the bipolar plate is an ultra-thin metal substrate, including but not limited to stainless steel foil, copper foil, titanium foil, etc., and its thickness is 50-600 microns.

[0045] The bipolar plates described above have hydrogen, oxygen (air), cooling liquid inlets and outlets and fluid channels of certain shapes and sizes. When the fuel cell is working, the above fluids enter through the inlet, then enter the channel, and finally exit the battery through the outlet. The channel plays a role in evenly distributing the fluid in the battery, making the electrochemical reaction on the membrane electrode surface uniform and the current uniform. At the same time, it also plays a role in taking away the water and heat generated by the battery. The channel type (such as serpentine channel, parallel channel, straight channel, co-chi channel, island channel), channel size (channel width, depth, ridge width), fluid inlet and outlet size, quantity, position, etc. will have an important impact on battery performance. Generally speaking, the design of the bipolar plate flow field required for different battery types and application scenarios is different. The drawings of the present invention are only for the convenience of describing the process. Other flow field types can also be implemented according to the process described in the present invention, and are also within the scope of protection of the present invention.

[0046] Before the preparation of the bipolar plate, the substrate is cut into sheets of corresponding size according to the designed size and shape of the bipolar plate by laser cutting or mechanical punching, and then corresponding holes are cut at the fluid inlet and outlet positions. The obtained sheets are washed and dried for later use.

[0047] In the above step S1-2:

[0048] Through precision coating technology, a layer of polymer-based conductive adhesive layer is evenly coated on one side of the pre-cut metal sheet, and after heat treatment, a coated substrate with a conductive adhesive layer of a certain thickness is obtained. In the subsequent steps, this cured conductive adhesive layer is laser-etched to form grooves of designed shapes to obtain flow field channels. The metal substrate under the adhesive layer plays a role in blocking gases and liquids and providing mechanical support.

[0049] The coating method is blade coating, extrusion coating, micro-gravure coating or other industrially available methods that can accurately control the coating thickness.

[0050] The thickness of the coated glue layer is 50-500 microns, that is, the depth of the flow channel or the thickness of the ridge in the future flow field cannot exceed 50-500 microns.

[0051] The conductive adhesive material can be a commercial product on the market, or it can be prepared by a professional manufacturer according to the use requirements. Its main components are a composite of a polymer (such as a mixture of one or more of phenolic resin, epoxy resin, silicone resin, PEFT resin, urea-formaldehyde resin, etc.) and a conductive filler (such as a mixture of one or more of silver powder, graphite powder, mesophase carbon microspheres, chopped carbon fibers, conductive carbon powder, graphene, carbon nanotubes, etc.). The performance requirements for the conductive adhesive are as follows: it has fluidity suitable for screen printing (viscosity of 1000-20000 centipoise), a suitable curing temperature (50-200°C), a curing time of less than 6 hours, and a volume resistivity of less than 0.1Ωcm after curing.

[0052] The heat treatment temperature is 50-200° C. for 15 minutes to 6 hours. The heat treatment process is used to ensure that the conductive adhesive layer is completely cured and to eliminate the stress generated during the processing.

[0053] In the above steps S1-3:

[0054] The preparation process of the bipolar plate is as follows: the coated substrate is placed into the base of the laser etching equipment and fixed by a vacuum adsorption device; the pre-designed drawings of the shapes of hydrogen (anode), oxygen (air) (cathode) and cooling liquid flow fields are input into the laser etching equipment operating system, and laser etching is performed according to the design drawings. The glue layer of the fluid flow channel in the drawing is etched away, and the etched part constitutes the distribution channel and flow channel (groove) of the fluid. The remaining part of the glue layer is the ridge and edge sealing area of ​​the flow field. The width and depth of the flow channel (groove) are controlled by the operating parameters of the laser etching equipment according to the pre-designed drawings. The depth of the groove (i.e., flow channel) is 50-500 microns, and at the same time, it must be 5-50 microns less than the thickness of the glue layer to avoid damage to the anti-corrosion coating of the metal substrate; the design width of the flow channel and the ridge is basically the same, within the range of 50-500 microns. After the above steps, cathode flow field single plate, anode flow field single plate and liquid flow field single plate with designed structures are obtained.

[0055] In the above step S2:

[0056] The bipolar plate is obtained by bonding and pressing three single plates (cathode flow field single plate, anode flow field single plate and liquid flow field single plate). A sealing adhesive is applied to the back side of the gas flow field of the cathode flow field single plate and the anode flow field single plate and the edge sealing area on both sides of the liquid flow field single plate. Then, the three single plates are strictly aligned in sequence (i.e., the gas flow field faces outward), and are placed in a pressing device and pressed to make the three single plates fit tightly. At room temperature -150°C, they are kept for 30 minutes to 24 hours. After the sealing adhesive is cured, the ultra-thin metal bipolar plate of the present invention is obtained.

[0057] like Figure 4As shown, the two sides outside the bipolar plate are gas flow fields, including a hydrogen flow field (anode) and an oxygen and air flow field (cathode), and the middle is a liquid flow field.

[0058] The sealing adhesive is a commercial silicone sealant, epoxy sealant, phenolic sealant, etc. To ensure production efficiency, the curing condition is required to be room temperature-150° C. and the curing time is within 30 minutes-24 hours.

[0059] The sealing adhesive is applied by brushing, spraying, rolling or dispensing.

[0060] The prepared ultra-thin bipolar plate, membrane electrode and diffusion layer form a single cell, and multiple single cells and auxiliary components such as end plates are stacked to obtain a PEMFC fuel cell stack, namely a proton exchange membrane fuel cell.

[0061] Example 1

[0062] (1) Take the surface treated stainless steel 316L foil (thickness 100 μm) and cut it by laser according to the design size and shape of the bipolar plate. Figure 1-3 Cut out corresponding holes at the fluid inlet and outlet positions shown, and cut out sheets of corresponding sizes, wash them, and dry them for later use.

[0063] A layer of phenolic / graphite powder-based conductive adhesive was evenly coated on one side of the sheet by a doctor blade coating method, and then placed in a drying device for heat treatment at 110° C. for 60 minutes to obtain a coated substrate. The thickness of the conductive adhesive layer was controlled at 200 μm.

[0064] The coated substrate is placed on the base of the laser etching equipment and fixed by a vacuum adsorption device; the pre-designed drawings of the hydrogen (anode), oxygen (air) (cathode) and cooling liquid flow field shapes are input into the laser etching equipment operating system, and laser etching is performed according to the design drawings to etch away the glue layer of the fluid flow channel in the drawings. The etched part constitutes the distribution channel and flow channel (groove) of the fluid, and the remaining part of the glue layer is the ridge and edge sealing area of ​​the flow field. According to the pre-designed drawings, the depth of the flow channel etched by the laser etching equipment operating parameters is 180 microns, and the width of the flow channel and the ridge is 200 microns.

[0065] Through the above steps, a single plate with hydrogen (anode), oxygen, air (cathode) and cooling liquid flow fields having ultra-fine flow channels is obtained.

[0066] The edge sealing areas ( Figure 4 - ), coated with silane sealant adhesive by brushing, and then the three single plates are strictly aligned in sequence (that is, the gas flow field faces outward), placed in a pressing device and pressed to make the three single plates fit tightly, kept at 120°C for 0.5 hour, and after the sealing adhesive is cured and the surface is cleaned, the ultra-thin metal composite bipolar plate of the present invention is obtained.

[0067] The bipolar plate prepared in this embodiment has a thickness of 750 microns. Testing shows that the volume resistivity is 0.06Ωcm. It is combined with a 20-micron thick membrane electrode (Pt loading 0.4 mg / cm2) and a 200-micron thick diffusion layer to form a single cell for electrical performance testing. Under the conditions of hydrogen (air) inlet pressure of 1.0 atm and battery operating temperature of 70°C, the current density at a battery voltage of 0.65V is as high as 1.9A / cm2.

[0068] Example 2

[0069] (1) Take the surface treated titanium foil (thickness 50 μm) and cut it by laser according to the design size and shape of the bipolar plate. Figure 1-3 Cut out corresponding holes at the fluid inlet and outlet positions shown, and cut out sheets of corresponding sizes, wash them, and dry them for later use.

[0070] A layer of epoxy / silver powder-based conductive adhesive was evenly coated on one side of the sheet by extrusion coating, and then placed in a drying device for heat treatment at 100° C. for 2 hours to obtain a coated substrate. The thickness of the conductive adhesive layer was controlled at 100 μm.

[0071] The coated substrate is placed on the base of the laser etching equipment and fixed by a vacuum adsorption device; the pre-designed drawings of the hydrogen (anode), oxygen (air) (cathode) and cooling liquid flow field shapes are input into the laser etching equipment operating system, and laser etching is performed according to the design drawings to etch away the glue layer of the fluid flow channel in the drawings. The etched part constitutes the distribution channel and flow channel (groove) of the fluid, and the remaining part of the glue layer is the ridge and edge sealing area of ​​the flow field. According to the pre-designed drawings, the depth of the flow channel etched by the laser etching equipment operating parameters is 80 microns, and the width of the flow channel and the ridge is 50 microns.

[0072] Through the above steps, a single plate with hydrogen (anode), oxygen, air (cathode) and cooling liquid flow fields having ultra-fine flow channels is obtained.

[0073] The edge sealing areas ( Figure 4 - ), coated with epoxy-based sealing adhesive by roll coating, and then the three single plates are strictly aligned in sequence (i.e., the gas flow field faces outward), placed in a pressing device and pressed to make the three single plates fit tightly, kept at 150°C for 0.5 hour, and after the sealing adhesive is cured and the surface is cleaned, the ultra-thin metal composite bipolar plate of the present invention is obtained.

[0074] The bipolar plate prepared in this embodiment has a thickness of 450 μm. The volume resistivity is 0.02 Ω cm. The bipolar plate prepared in this embodiment has a thickness of 450 μm. The volume resistivity is 0.02 Ω cm. 2 ), 260 micron thick diffusion layer to form a single cell, electrical performance test, hydrogen, oxygen inlet pressure 0.8atm, battery operating temperature 80℃ conditions, measured battery voltage 0.65V when the current density is as high as 2.3A / cm 2 .

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An ultra-thin metal composite bipolar plate, It is characterized in that include: A cathode flow field single plate (1), the cathode flow field single plate (1) comprising an ultra-thin metal substrate and a conductive adhesive layer coated on one side of the ultra-thin metal substrate, the conductive adhesive layer of the cathode flow field single plate (1) having an oxygen / air flow field (12); An anode flow field single plate (2), the anode flow field single plate (2) comprising an ultra-thin metal substrate and a conductive adhesive layer coated on one side of the ultra-thin metal substrate, the conductive adhesive layer of the anode flow field single plate (2) being laser-etched with a hydrogen flow field (14) having an ultra-fine flow channel; A liquid flow field single plate (3), the liquid flow field single plate (3) comprising an ultra-thin metal substrate and a conductive adhesive layer coated on one side of the ultra-thin metal substrate, the conductive adhesive layer of the liquid flow field single plate (3) being laser-etched to form a liquid flow field (16) having ultra-fine flow channels; The ultra-thin metal substrate surface of the cathode flow field single plate (1) is bonded to the ultra-thin metal substrate surface of the liquid flow field single plate (3), and the conductive adhesive layer of the liquid flow field single plate (3) is bonded to the ultra-thin metal substrate surface of the anode flow field single plate (2); The method for preparing the ultra-thin metal composite bipolar plate comprises the following steps: S1) preparing a cathode flow field single plate, an anode flow field single plate and a liquid flow field single plate respectively by precision coating and laser etching technology; S2) bonding and pressing the cathode flow field single plate, the anode flow field single plate and the liquid flow field single plate together to obtain an ultra-thin metal bipolar plate; The step S1) comprises: S1-1) cutting the ultra-thin metal substrate into sheets of designed size and shape, punching three types of through holes at both ends of the sheets, washing them, drying them and setting them aside; S1-2) uniformly coating a layer of polymer-based conductive adhesive layer on one side of the ultra-thin metal sheet by precision coating technology, and obtaining a coated substrate having a conductive adhesive layer of a certain thickness by heat treatment; S1-3) placing the coated substrate on a base of a laser etching device, fixing it with a vacuum adsorption device, and performing laser etching processing according to pre-designed drawings of hydrogen flow field, oxygen / air flow field and liquid flow field shapes, respectively, to obtain a cathode flow field single plate, an anode flow field single plate and a liquid flow field single plate with ultra-fine flow channels; The coating method is blade coating, extrusion coating or micro-gravure; the heat treatment temperature after coating is 50-200°C for 30 minutes to 6 hours, and the thickness of the adhesive layer after coating is 50-500 microns.

2. The ultra-thin metal composite bipolar plate according to claim 1, It is characterized in that An oxygen / air inlet (8), a liquid inlet (6) and a hydrogen inlet (4) are provided at one end of the ultra-thin metal composite bipolar plate, and the oxygen / air inlet (8), the liquid inlet (6) and the hydrogen inlet (4) are all hole-shaped flow channels formed by stacking through holes correspondingly provided on the cathode flow field single plate (1), the anode flow field single plate (2) and the liquid flow field single plate (3); an oxygen outlet (7), a liquid outlet (9) and a hydrogen outlet (5) are provided at the other end of the ultra-thin metal composite bipolar plate, and the oxygen outlet (7), the liquid outlet (9) and the hydrogen outlet (5) are all hole-shaped flow channels formed by stacking through holes correspondingly provided on the cathode flow field single plate (1), the anode flow field single plate (2) and the liquid flow field single plate (3); The oxygen / air inlet (8) and the oxygen outlet (7) are both connected to the oxygen flow field (12), the liquid inlet (6) and the liquid outlet (9) are both connected to the liquid flow field (16), and the hydrogen inlet (4) and the hydrogen outlet (5) are both connected to the hydrogen flow field (14).

3. The ultra-thin metal composite bipolar plate according to claim 1, It is characterized in that The oxygen / air flow field (12) includes a plurality of ultrafine channels, the depth of the ultrafine channels is 50-500 microns, and the width of the ultrafine channels is 50-500 microns; the liquid flow field (16) includes a plurality of ultrafine channels, the depth of the ultrafine channels is 50-500 microns, and the width of the ultrafine channels is 50-500 microns; the hydrogen flow field (14) includes a plurality of ultrafine channels, the depth of the ultrafine channels is 50-500 microns, and the width of the ultrafine channels is 50-500 microns.

4. A proton exchange membrane fuel cell, It is characterized in that It comprises the ultra-thin metal composite bipolar plate as described in any one of claims 1 to 3.

5. The ultra-thin metal composite bipolar plate according to claim 1, It is characterized in that The step S2) comprises: taking the cathode flow field single plate, the anode flow field single plate and the liquid flow field single plate prepared in the step S1, coating the ultrafine metal substrate surface side of the cathode flow field single plate and the anode flow field single plate and the edge sealing area on both sides of the liquid flow field single plate with a sealing adhesive, and then aligning the three single plates in the order of the cathode flow field single plate, the ultrafine metal substrate and the anode flow field single plate, placing them in a pressing device and pressing them, and after the sealing adhesive is cured, an ultrathin metal composite bipolar plate is obtained.

6. The ultra-thin metal composite bipolar plate according to claim 1, It is characterized in that The ultra-thin metal substrate is a surface-treated metal foil, and the metal foil is any one of stainless steel foil, gold foil, silver foil, copper foil, and titanium foil, and has a thickness of 50-600 microns; the polymer-based conductive adhesive is a composite of a polymer and a conductive filler, and the polymer is a mixture of one or more of phenolic resin, epoxy resin, silicone resin, PEFT resin, urea-formaldehyde resin, ethylene propylene diene monomer resin, polyimide, etc., and the conductive filler is a mixture of one or more of silver powder, graphite powder, mesophase carbon microspheres, chopped carbon fibers, conductive carbon powder, graphene, carbon nanotubes, etc. The viscosity of the conductive adhesive is between 1000-20000 centipoise, the curing temperature is 50-150°C, the curing time is less than 6 hours, and the volume resistivity after curing is less than 0.1Ωcm.

7. The ultra-thin metal composite bipolar plate according to claim 5, It is characterized in that The sealing adhesive is a commercial silicone sealant, epoxy sealant or phenolic sealant, and its curing condition is required to be room temperature-150°C and the curing time is within 0.5-24 hours; the sealing adhesive is applied by brushing, spraying, roller coating or dispensing.