Preparation method and application of cobalt-nickel bimetallic sulfide / carbon paper composite material

The preparation of cobalt-nickel bimetallic sulfide/carbon paper composite interlayer material through one-step hydrothermal method is used for lithium-sulfur battery separator, which solves the problems of low sulfur positive conductivity and 'shuttle effect' in lithium-sulfur batteries, and significantly improves the battery's Electrochemical properties and cyclic stability.

CN109786628BActive Publication Date: 2024-11-05HENAN ANHUINENG NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910219512.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-03-20
Publication Date
2024-11-05
Estimated Expiration
2039-03-20

AI Technical Summary

Technical Problem

The performance degradation in lithium-sulfur batteries due to the low conductivity of sulfur positive electrode, easy structure damage and the "shuttle effect", especially the diffusion of lithium polysulfide reduces the circulation performance and sulfur utilization rate of lithium-sulfur batteries.

Method used

A one-step hydrothermal method is used to prepare cobalt-nickel bimetallic sulfide/carbon paper composite interlayer material. As part of the separator, carbon paper is used as a metal sulfide growth carrier to form cobalt-nickel bimetallic sulfide nanoparticles to adsorb and block polysulfide diffusion.

Benefits of technology

The electrochemical performance of lithium-sulfur batteries has been significantly improved, with the first charge and discharge specific capacity reaching 1513.7mAh/g, the capacity retention rate has been improved, and the circulation performance and stability have also been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109786628B_ABST
    Figure CN109786628B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method and application of a cobalt-nickel bimetallic sulfide / carbon paper composite material, belonging to the technical field of composite materials. The preparation method is as follows: (1) pretreatment of carbon paper: cutting the carbon paper, putting it into a muffle furnace, keeping it warm for 12-18 hours, and removing surface impurities; cutting the pretreated carbon paper for standby use; (2) adding a cobalt source, a nickel source and a solvent into a container, stirring and dissolving, adding a sulfur source, and continuing to stir to obtain a reaction solution; (3) transferring the reaction solution to a hydrothermal reactor, and putting the pretreated carbon paper into it, after sealing, transferring it to an oven at 100-200°C, hydrothermally reacting for 10-16 hours, and obtaining a CNS2 / CP composite interlayer material after natural cooling. The preparation method of the present invention is simple and low in cost. The prepared CNS2 / CP composite interlayer material is used as a part of a diaphragm in a lithium-sulfur battery, which can suppress the shuttle effect and significantly improve the electrochemical performance of the lithium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the technical field of composite material preparation and application, and in particular to a preparation method and application of a cobalt-nickel bimetallic sulfide / carbon paper composite material. [Background technology]

[0002] With the development of new energy technology, the widely used lithium-ion batteries have been unable to meet the market demand. Therefore, in recent years, new next-generation secondary batteries have emerged, including lithium-air batteries, zinc-air batteries and lithium-sulfur batteries. Among them, lithium-sulfur batteries have a high theoretical specific capacity (1672mAhg -1 ), specific energy (2600whkg -1 ), low cost and environmental friendliness, etc., and has attracted extensive attention and research from researchers, becoming an important research direction for the next generation of lithium batteries.

[0003] Lithium-sulfur batteries are composed of a positive-sulfur composite material, a lithium negative electrode, a separator, and an electrolyte. Although lithium-sulfur batteries have a high theoretical specific capacity, they also have some defects. First, the conductivity of the sulfur positive electrode is very low, only 5×10 -30 S / cm; in addition, the volume change of the positive electrode before and after the lithium-sulfur battery reaction is large, which can easily lead to structural damage and failure; finally, the intermediate product long-chain lithium polysulfide produced in the redox reaction is easily dissolved in the lithium-sulfur battery electrolyte, resulting in a "shuttle effect", which reduces the utilization rate of sulfur and the cycle performance, which is also the most serious problem in lithium-sulfur batteries.

[0004] In order to alleviate the "shuttle effect", researchers have proposed many means and methods to overcome it, such as designing special structures of positive electrode host materials, new electrolyte systems, protection of lithium negative electrodes and modification of diaphragms. The diaphragm is also an important component in lithium-sulfur batteries, acting as an electronic insulator to prevent battery short circuits. At present, most commercial diaphragms are polymer membranes with a large number of nanopores, and the pore size is much larger than that of polysulfides. Therefore, soluble polysulfides will freely pass through the diaphragm, diffuse to the negative electrode and react with metallic lithium, resulting in the decomposition of metallic lithium. Therefore, researchers have proposed functional modification of the diaphragm to inhibit the shuttle effect. At present, a variety of methods and materials for modifying diaphragms have emerged, including carbon-based materials, organic polymer materials, inorganic metal oxide materials and other new functional materials. The modification of the diaphragm can be roughly divided into two types, one is to coat the modified material on the diaphragm for battery, and the other is to insert an independent modified interlayer as part of the diaphragm for battery. Regardless of the method used to modify the diaphragm, the modified material needs to have the following characteristics: 1) chemical / physical adsorption of soluble polysulfides, 2) sufficient space for the storage of polysulfides, and 3) good conductive channels to reuse the adsorbed / bonded polysulfides in electrochemical reactions.

[0005] The document is titled "Performance Study of Carbon Paper as a Functional Interlayer for Lithium-Sulfur Batteries". Li Wenhui, a master's thesis from Beijing Institute of Technology, disclosed the use of three different thicknesses of carbon paper, namely 100μm, 200μm, and 300μm thick carbon paper, which were cut into the size of the separator after alkaline treatment, and the carbon materials of different thicknesses were characterized. The materials used for the positive electrode were measured, and finally the electrochemical performance of the batteries assembled with the three thicknesses was tested. The data showed that the 300μm thick carbon paper had stronger conductivity and stronger barrier effect on polysulfides, so that after 200 weeks of positive electrode material, the retained capacity of CP-300 was 489mAhg -1 , and the capacity retention rate was 57%. This study used carbon paper directly as the separator material after physical treatment. Although it suppressed the shuttle effect to a certain extent and improved the electrical performance of lithium-sulfur batteries, the improvement was still limited. [Summary of the invention]

[0006] The present invention aims at the biggest problem faced by lithium-sulfur batteries and provides a method for preparing cobalt-nickel bimetallic sulfide (CNS 2 ) and carbon paper composite sandwich material, the method mainly adopts a one-step hydrothermal method, uses carbon paper as a metal sulfide growth carrier, and prepares CNS 2 / CP composite interlayer and use it as part of the separator in lithium-sulfur batteries to suppress the "shuttle effect" and significantly improve the electrical performance of lithium-sulfur batteries.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a cobalt-nickel bimetallic sulfide / carbon paper composite material comprises the following steps:

[0009] (1) Carbon paper pretreatment: After cutting the carbon paper, place it in a muffle furnace and keep it warm for 12-18 hours to remove surface impurities; cut the pretreated carbon paper into required specifications and set aside;

[0010] (2) adding a cobalt source, a nickel source and a solvent into a container, stirring until fully dissolved, then adding a sulfur source, and continuing to stir evenly to obtain a reaction solution;

[0011] (3) The reaction solution is transferred to a hydrothermal reactor, and the pretreated carbon paper is placed in the reactor. After sealing, the reaction solution is transferred to an oven at 100-200°C for 10-16 hours. After cooling naturally, CNS is obtained. 2 / CP composite sandwich material.

[0012] Preferably, in step (1), the carbon paper pretreatment is carried out at a holding temperature of 300-500°C.

[0013] Preferably, the cobalt source is one or more of cobalt nitrate hexahydrate, cobalt chloride hexahydrate and cobalt acetate tetrahydrate.

[0014] Preferably, the nickel source is one or more of nickel nitrate hexahydrate, nickel chloride hexahydrate and nickel acetate tetrahydrate.

[0015] Preferably, the sulfur source is one or more of sodium thiosulfate pentahydrate, L-cysteine ​​and thiourea.

[0016] Preferably, the solvent is one or more of deionized water, ethanol, ethylene glycol and isopropanol.

[0017] Preferably, the molar ratio of cobalt element to nickel element in the reaction solution is 1-3:1.

[0018] Preferably, the molar ratio of cobalt element, nickel element and sulfur element in the reaction solution is 1-3:1:3-8; and the molar concentration of cobalt element in the reaction solution is 0.008-0.015 mol / L.

[0019] Another aspect of the present invention provides the CNS prepared as above 2 The / CP composite interlayer material is used in the preparation of a lithium-sulfur battery, which includes a graphene / sulfur composite positive electrode, a metal lithium sheet, a separator and an electrolyte. The application method is to introduce the composite interlayer material synthesized above between the separator and the positive electrode sheet as a part of the separator for the lithium-sulfur battery.

[0020] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0021] 1. The present invention adopts a one-step hydrothermal method to synthesize CNS 2 / CP composite sandwich materials only need to dissolve the raw materials in the solvent, stir them thoroughly, and put them into the hydrothermal cooperation device. It has the advantages of simple synthesis steps and low production cost, which is conducive to promoting its further industrialization.

[0022] 2. The cobalt-nickel bimetallic sulfide / carbon paper composite interlayer synthesized in the present invention is used for diaphragm modification. Different from the traditional monometallic sulfide modified carbon paper and unmodified carbon paper, the presence of cobalt and nickel metal ions can form more metal-sulfur bonds to adsorb polysulfide ions. In addition, the carbon paper with good conductivity can not only physically block the polysulfide ions from passing through the diaphragm to the lithium negative electrode, but also provide a good conductive skeleton. On the other hand, the carbon paper with high specific surface area can also provide sufficient growth sites for the growth of bimetallic sulfides to form cobalt-nickel bimetallic sulfide nanoparticles.

[0023] 3. The present invention prepares the obtained CNS 2 / CP is used as a composite interlayer material as part of the diaphragm in lithium-sulfur batteries and exhibits excellent electrochemical performance. The first charge and discharge specific capacity reaches 1513.7mAh / g at a charge and discharge voltage range of 1.7V-2.8V and a rate of 0.1C, which is much higher than the first charge and discharge specific capacity of 1116.8mAh / g without using an interlayer.

Brief Description of the Drawings

[0024] Figure 1 The CNS prepared in Example 2 2 / SEM image of CP;

[0025] Figure 2 The CNS prepared in Example 2 was used 2 The first charge and discharge curve of the lithium-sulfur battery with composite interlayer material of / CP at the current density of 0.1C;

[0026] Figure 3 This is the first charge and discharge curve of a lithium-sulfur battery using a simple CP interlayer at a current density of 0.1C for the comparative example;

[0027] Figure 4 The CNS of Example 2 is applied 2 Rate diagram of lithium-sulfur battery with / CP composite interlayer and comparative example CP interlayer;

[0028] Figure 5 The CNS of Example 2 is applied 2 Cycling performance diagram of lithium-sulfur battery with composite interlayer of / CP and comparative example CP interlayer at 1C current density. [Specific implementation method]

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] A method for preparing a cobalt-nickel bimetallic sulfide / carbon paper composite material comprises the following steps:

[0032] (1) Carbon paper pretreatment: After cutting the commercial carbon paper, put it into a muffle furnace and keep it at 300°C for 18 hours to remove surface impurities; the pretreated carbon paper is further cut to a size according to the purpose and object of use and placed aside;

[0033] (2) adding 0.3 mmol of cobalt nitrate hexahydrate as a cobalt source, adding 0.3 mmol of nickel nitrate hexahydrate as a nickel source, adding 40 ml of deionized water and ethanol as a solvent, and the volume ratio of deionized water to ethanol is 1:1, stirring until fully dissolved, adding 0.6 mmol of sodium thiosulfate pentahydrate as a sulfur source, and continuing to stir evenly to obtain a reaction solution;

[0034] (3) The reaction solution was transferred to a hydrothermal reactor, and the pretreated carbon paper was placed in the reactor. After sealing, the reaction solution was transferred to a 200°C oven for hydrothermal reaction for 10 hours. After cooling naturally, CNS was obtained. 2 / CP composite sandwich material.

[0035] Example 2

[0036] A method for preparing a cobalt-nickel bimetallic sulfide / carbon paper composite material comprises the following steps:

[0037] (1) Carbon paper pretreatment: After cutting the commercial carbon paper, put it into a muffle furnace and keep it at 400°C for 15 hours to remove surface impurities; the pretreated carbon paper is further cut to a size according to the purpose and object of use and placed aside;

[0038] (2) adding 0.4 mmol of cobalt chloride hexahydrate as a cobalt source, adding 0.2 mmol of nickel chloride hexahydrate as a nickel source, adding 50 ml of deionized water and ethylene glycol as a solvent, and the volume ratio of deionized water to ethylene glycol is 1:1, stirring until fully dissolved, adding 1.6 mmol of sodium thiosulfate pentahydrate as a sulfur source, and continuing to stir evenly to obtain a reaction solution;

[0039] (3) The reaction solution was transferred to a hydrothermal reactor, and the pretreated carbon paper was placed in the reactor. After sealing, the reaction solution was transferred to an oven at 180°C for 12 hours. After cooling naturally, CNS was obtained. 2 / CP composite sandwich material.

[0040] Example 3

[0041] A method for preparing a cobalt-nickel bimetallic sulfide / carbon paper composite material comprises the following steps:

[0042] (1) Carbon paper pretreatment: After cutting the commercial carbon paper, put it into a muffle furnace and keep it at 450°C for 15 hours to remove surface impurities; the pretreated carbon paper is further cut to a size according to the purpose and object of use and placed aside;

[0043] (2) adding 0.9 mmol of cobalt acetate tetrahydrate as a cobalt source, 0.3 mmol of nickel acetate tetrahydrate as a nickel source, 60 ml of deionized water and ethylene glycol as solvents, and the volume ratio of deionized water to ethylene glycol is 3:1, stirring until fully dissolved, adding 1.5 mmol of thiourea as a sulfur source, and continuing to stir evenly to obtain a reaction solution;

[0044] (3) The reaction solution was transferred to a hydrothermal reactor, and the pretreated carbon paper was placed in the reactor. After sealing, the reaction solution was transferred to an oven at 150°C for 12 hours. After cooling naturally, CNS was obtained. 2 / CP composite sandwich material.

[0045] Example 4

[0046] A method for preparing a cobalt-nickel bimetallic sulfide / carbon paper composite material comprises the following steps:

[0047] (1) Carbon paper pretreatment: After cutting the commercial carbon paper, put it into a muffle furnace and keep it at 500°C for 12 hours to remove surface impurities; the pretreated carbon paper is further cut to a size according to the purpose and object of use and placed aside;

[0048] (2) Add 0.3 mmol of cobalt nitrate hexahydrate and 0.3 mmol of cobalt chloride hexahydrate as a cobalt source to a container, add 0.3 mmol of nickel nitrate hexahydrate and 0.2 mmol of nickel chloride hexahydrate, add 50 ml of deionized water and ethylene glycol as a solvent, and the volume ratio of deionized water to ethylene glycol is 3:1, stir until fully dissolved, add 1.8 mmol of L-cysteine ​​as a sulfur source, and continue to stir evenly to obtain a reaction solution;

[0049] (3) The reaction solution was transferred to a hydrothermal reactor, and the pretreated carbon paper was placed in the reactor. After sealing, the reaction solution was transferred to a 100°C oven for hydrothermal reaction for 16 hours. After cooling naturally, CNS was obtained. 2 / CP composite sandwich material.

[0050] Example 5

[0051] A method for preparing a cobalt-nickel bimetallic sulfide / carbon paper composite material comprises the following steps:

[0052] (1) Carbon paper pretreatment: After cutting the commercial carbon paper, put it into a muffle furnace and keep it at 400°C for 15 hours to remove surface impurities; the pretreated carbon paper is further cut to a size according to the purpose and object of use and placed aside;

[0053] (2) adding 0.6 mmol of cobalt nitrate hexahydrate as a cobalt source, 0.2 mmol of nickel chloride hexahydrate as a nickel source, and 60 ml of isopropanol as a solvent, wherein the volume ratio of deionized water to ethylene glycol is 3:1, and stirring until fully dissolved, adding 1.2 mmol of L-cysteine ​​as a sulfur source, and continuing to stir evenly to obtain a reaction solution;

[0054] (3) The reaction solution was transferred to a hydrothermal reactor, and the pretreated carbon paper was placed in the reactor. After sealing, the reaction solution was transferred to a 100°C oven for hydrothermal reaction for 16 hours. After cooling naturally, CNS was obtained. 2 / CP composite sandwich material.

[0055] Performance Testing:

[0056] (1) Electron microscopy analysis: Figure 1 is the CNS prepared in Example 2 2 Scanning electron microscope image (SEM image) of the / CP composite interlayer material. As can be seen from the figure, the granular structure formed by the cobalt-nickel bimetallic sulfide grows on the carbon paper skeleton, the average size of the particles reaches the nanometer level, and the distribution is uniform. The cobalt-nickel bimetallic sulfide particles thus formed have a large specific surface area, exposing more catalytic active sites and accelerating the conversion between polysulfides. In addition, the double metal sulfur bond adsorbs more polysulfides, slows down the diffusion of polysulfides, and effectively inhibits the shuttle effect, thereby improving the electrochemical performance of the battery.

[0057] (2) Electrochemical performance test:

[0058] CNS 2 / CP group: To evaluate CNS 2 The graphene / sulfur composite material was used as a part of the separator in lithium-sulfur batteries. The effect of the graphene / sulfur composite material on the electrochemical performance of the lithium-sulfur battery was studied. The graphene / sulfur composite material was used as the positive electrode, the metal lithium sheet was used as the negative electrode, the separator was a glass fiber separator, and the electrolyte was 1M lithium bistrifluoromethanesulfonyl imide (LiTFSI) dissolved in 1,3-dioxolane (DOL) / ethylene glycol dimethyl ether (DME) = 1:1V%, and 1% LiNO was added. 3 The above materials were assembled into button cells in a glove box under a pure argon atmosphere. During the assembly, the CNS prepared in Example 2 2 The / CP composite material is inserted between the separator and the positive electrode. The materials required for assembling the above-mentioned battery can be purchased from commercial sources, and the battery assembly method is a conventional technical means in the art and will not be described in detail here.

[0059] Comparative Example CP Group: Using untreated carbon paper instead of CNS in Example 2 2 / CP, as a part of the diaphragm, was inserted between the diaphragm and the positive electrode plate, and assembled into another group of button batteries, which served as the comparative example group of the present invention.

[0060] CNS 2 The electrical performance of lithium-sulfur batteries in the / CP group and the comparative CP group was tested. The results are shown in Figure 2-5 .

[0061] Depend on Figure 2 and Figure 3 For CNS 2 First charge and discharge diagram of the composite interlayer of / CP and CP interlayer battery at 0.1C current density, CNS 2 The / CP group showed excellent electrochemical performance, with the first charge and discharge specific capacity reaching 1513.7 mAh / g at a charge and discharge voltage range of 1.7V-2.8V and a rate of 0.1C, which is much higher than the first charge and discharge specific capacity of 1116.8 mAh / g of the CP interlayer.

[0062] Figure 4 The rate performance of the two membrane batteries is shown, from 0.1C to 1C and then back to 0.1C. It can be seen that CNS 2 The specific capacity of the / CP group is always higher than that of the comparative CP group. At the same current density, the stability of the batteries of the two groups is good. However, with the increase of discharge cycles and current density, the difference in specific capacity between the two groups of batteries becomes larger, indicating that the battery stability of the present invention group is better.

[0063] Figure 5 Shows CNS 2 Cycling performance diagram of CNS / CP composite interlayer and CP interlayer battery at 1C current density, 2 The initial specific capacity of the / CP group reached more than 920mAh / g, and remained at about 700mAh / g after 500 cycles, while the initial capacity of the CP group was only 700mAh / g, which dropped to about 500mAh / g after 500 cycles, indicating that the capacity retention rate of the inventive group was also higher than that of the comparative group, reflecting a better capacity retention rate.

[0064] It can be seen from the above performance tests that the present invention synthesizes CNS by hydrothermal method 2 / CP composite interlayer material, when used as part of the diaphragm in lithium-sulfur batteries, can more effectively inhibit the sulfur shuttle effect and improve the overall performance of lithium-sulfur batteries compared to using carbon paper as part of the diaphragm.

[0065] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.

Claims

1. CNS 2 Application of / CP composite interlayer materials in the preparation of lithium-sulfur batteries, Features: The lithium-sulfur battery comprises a graphene / sulfur composite positive electrode, a metal lithium sheet, a separator and an electrolyte. The application method is to introduce the synthesized composite interlayer material between the separator and the positive electrode sheet as a part of the separator for the lithium-sulfur battery; The CNS 2 The preparation method of the / CP composite sandwich material comprises the following steps: (1) Carbon paper pretreatment: After cutting the carbon paper, put it into a muffle furnace and keep it warm for 12-18 hours to remove surface impurities; Cut the pretreated carbon paper into required specifications and place it aside for later use; the pretreatment temperature of the carbon paper is 300-500℃; (2) adding a cobalt source, a nickel source and a solvent into a container, stirring until fully dissolved, then adding a sulfur source, and continuing to stir evenly to obtain a reaction solution; the molar ratio of the cobalt element, the nickel element and the sulfur element in the reaction solution is 1-3:1:3-8; (3) The reaction solution is transferred to a hydrothermal reactor, and the pretreated carbon paper is placed in the reactor. After sealing, the reaction solution is transferred to an oven at 100-200°C for 10-16 hours. After cooling naturally, CNS is obtained. 2 / CP composite sandwich material.

2. The use according to claim 1, Features: The cobalt source is one or more of cobalt nitrate hexahydrate, cobalt chloride hexahydrate and cobalt acetate tetrahydrate.

3. The use according to claim 1, Features: The nickel source is one or more of nickel nitrate hexahydrate, nickel chloride hexahydrate and nickel acetate tetrahydrate.

4. The use according to claim 1, Features: The sulfur source is one or more of sodium thiosulfate pentahydrate, L-cysteine ​​and thiourea.

5. The use according to claim 1, Features: The solvent is one or more of deionized water, ethanol, ethylene glycol and isopropanol.

6. The CNS-containing product obtained by the application of claim 1 2 Lithium-sulfur battery based on / CP composite interlayer material.