Solid electrolytic capacitor components
By using porous anode body and organic functional silane compound bonding technology in solid electrolytic capacitors, the problems of capacitor stability and leakage current under high temperature and high voltage are solved, and high-performance capacitor components are realized.
Patent Information
- Application Number
- CN201780064078.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-10-18
- Filing Date
- 2017-10-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2037-10-12
AI Technical Summary
Existing solid electrolytic capacitors exhibit high leakage current and capacitance degradation at high temperatures and voltages, and are difficult to maintain stability.
Using a capacitor assembly that includes a porous anode body including a valve metal compound, a valve metal oxide dielectric, and a conductive polymer layer, the dielectric is enhanced by forming a porous structure on the anode body and using an organofunctional silane compound to bond with the hydroxyl functional polymer. stability.
It achieves improvements in the stability and electrical performance of capacitors under high temperatures and high voltages, maintains a high percentage of wet-to-dry capacitance and low leakage current, and extends the service life of the capacitor.
Smart Images

Figure CN109844882B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 409,423, filed October 18, 2016, and is hereby incorporated by reference in its entirety. Background Art
[0003] Solid electrolytic capacitors (e.g., tantalum capacitors) are typically manufactured by pressing a metal powder (e.g., tantalum) around a metal lead wire, sintering the pressed component, anodizing the sintered anode, and then applying a solid electrolyte. Intrinsically conductive polymers are often used as solid electrolytes due to their advantageous low equivalent series resistance ("ESR") and "non-combustion / non-ignition" failure mode. For example, such electrolytes can be formed by in-situ chemical polymerization of 3,4-dioxythiophene monomers ("EDOT") in the presence of a catalyst and a dopant. However, conventional capacitors using in-situ polymerized polymers tend to have relatively high leakage currents ("DCL") and fail at high voltages (such as experienced during rapid turn-on or operating current spikes). In an attempt to overcome these problems, dispersions formed from composites of poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) ("PEDOT:PSS") have also been used. While PEDOT:PSS dispersions can produce some improved properties, the capacitance of such materials tends to degrade significantly at high temperatures, particularly when subjected to relatively high voltages.
[0004] As such, there currently exists a need for solid electrolytic capacitors having improved performance. Summary of the invention
[0005] According to one embodiment of the present invention, a capacitor assembly including a capacitor element is disclosed. The capacitor element includes a porous anode body containing a valve metal compound, a dielectric covering the anode body and including an oxide of the valve metal compound, and a solid electrolyte covering the dielectric. The solid electrolyte includes a conductive polymer and a hydroxyl-functional polymer. Further, the capacitor element includes an organic functional silane compound bonded to the oxide of the dielectric and capable of bonding to the hydroxyl-functional polymer.
[0006] According to another embodiment of the present invention, a method of forming a capacitor element is disclosed, which includes anodizing a sintered porous anode body to form a dielectric including an oxide of a valve metal compound; applying a solution including an organofunctional silane compound to the anode; applying a dispersion containing conductive polymer particles and a hydroxyl-functional polymer to form a conductive polymer layer; and bonding the organofunctional silane compound to the oxide of the electrolyte.
[0007] Other features and aspects of the invention are set out in more detail below. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] More particularly, a full and enabling disclosure of the present invention, including the best mode thereof, is given to those skilled in the art in the remainder of the specification with reference to the accompanying drawings, in which:
[0009] Figure 1 A cross-sectional view of one embodiment of a capacitor assembly of the assembly of the present invention;
[0010] Figure 2 A cross-sectional view of another embodiment of a capacitor assembly of the assembly of the present invention;
[0011] Figure 3 a cross-sectional view of another embodiment of a capacitor assembly that is an assembly of the present invention; and
[0012] Figure 4 A top view of another embodiment of a capacitor assembly of the assembly of the present invention is shown. DETAILED DESCRIPTION
[0013] Those skilled in the art will appreciate that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the invention, which are embodied in the exemplary configurations.
[0014] In general, the present invention relates to capacitor components that can exhibit good electrical properties even under a wide range of different conditions. More particularly, the capacitor contains a capacitor element comprising a porous anode body containing a valve metal compound (e.g., tantalum), a dielectric coated on the anode body and comprising an oxide of the valve metal compound (e.g., tantalum pentoxide), and a solid electrolyte coated on the dielectric. The solid electrolyte includes a conductive polymer and a hydroxyl-functional polymer. It is noteworthy that an organofunctional silane compound that is bonded to the oxide of the dielectric and is capable of bonding to the hydroxyl-functional polymer contained in the solid electrolyte is also used. Without intending to be bound by theory, it is believed that this can produce a variety of benefits for the capacitor. For example, it is believed that the bonding of the organofunctional silane compound to the oxide of the dielectric and the hydroxyl-functional polymer can improve the interfacial (interface) adhesion of these layers, which can improve capacitance stability, particularly when subjected to high temperatures and voltages.
[0015] Therefore, as a result of the present invention, the capacitor assembly produced can exhibit various unique and beneficial properties. For example, the capacitor assembly can exhibit excellent electrical properties, even when exposed to high temperatures. For example, the capacitor assembly can be placed in contact with a hot atmosphere having a temperature of about 80°C or higher, in some embodiments, about 100°C to about 150°C, and in some embodiments, about 105°C to about 130°C (e.g., 105°C or 125°C). Even at such high temperatures, the capacitor assembly can still exhibit its high percentage of wet capacitance, which makes it have only a small capacitance loss and / or fluctuation in the presence of atmospheric humidity. This performance feature is quantified by the "wet-to-dry capacitance percentage", which is determined by the following equation:
[0016] Wet-to-dry capacitance = (dry capacitance / wet capacitance) x 100
[0017] The capacitor assembly may exhibit a wet to dry capacitance percentage of about 50% or more, in some embodiments about 60% or more, in some embodiments about 70% or more, and in some embodiments, about 80% to 100%. The dry capacitance may be about 30 nanofarads per square centimeter ("nF / cm 2 ”) or higher, in some embodiments about 100 nF / cm 2 or higher, in some embodiments from about 200 to about 3,000 nF / cm 2 , and in some embodiments, from about 400 to about 2,000 nF / cm 2 , measured at a frequency of 120 Hz. The capacitance may also remain stable at such temperatures for a considerable period of time, such as about 100 hours or longer, in some embodiments, from about 300 hours to about 3000 hours, and in some embodiments, from about 400 hours to about 2500 hours (e.g., about 500 hours). For example, in one embodiment, the ratio of the capacitance value of the component after about 500 hours of exposure to a hot atmosphere (e.g., 125° C.) to the capacitance value of the component when initially exposed to the hot atmosphere is about 0.7 to 1.0, in some embodiments, about 0.75 to 1.0, and in some embodiments, about 0.80 to 1.0.
[0018] It is noteworthy that the high capacitance value can be maintained when a high voltage is applied. For example, the ratio of the capacitance value of the component after exposure to a hot atmosphere (e.g., 125° C.) and a rated voltage (maximum operating voltage) to the initial capacitance value of the component when exposed to the hot atmosphere but before the rated voltage is applied is about 0.7 to 1.0, in some embodiments, about 0.75 to 1.0, and in some embodiments, about 0.80 to 1.0. For example, the rated voltage may be about 15 volts or more, in some embodiments, about 18 volts or more, and in some embodiments, about 20 to about 150 volts. In one embodiment, for example, the capacitance value of the component after being exposed to a hot atmosphere (e.g., 125° C.) at a voltage of 25 volts for about 500 hours to the initial capacitance value of the component in the hot atmosphere but before the voltage is applied may be within the range noted above. The inventors have found that the capacitance is stable and remains within the range noted above even when the rated voltage begins to approach the formation voltage used to form the electrolyte - that is, when the ratio of the formation voltage to the rated voltage ("formation ratio") is about 2.6 or less, in some embodiments, about 2.5 or less, and in some embodiments, about 1.5 to about 2.3 (e.g., 1.7 or 2.1). The high capacitance values can also be maintained when multiple voltage pulses are applied. For example, the ratio of the capacitance value of the component subjected to 1000 pulses (30 second charging) at the rated voltage (e.g., 16 volts) in a hot atmosphere (e.g., 105°C) to the initial capacitance of the component before such pulses are applied is about 0.7 to 1.0, in some embodiments, about 0.75 to 1.0, and in some embodiments, about 0.80 to 1.0.
[0019] In addition to exhibiting good capacitance stability, the capacitor assembly may also exhibit a relatively low leakage current ("DCL") after exposure to a hot atmosphere (e.g., 105° C. or 125° C.) and a high voltage (e.g., 20 or 35 volts) as described above. For example, after being subjected to a hot atmosphere (e.g., 125° C. and a rated voltage (e.g., 20 or 35 volts) for 90 seconds, the capacitor assembly may exhibit a DCL of only about 50 microamperes ("μA") or less, in some embodiments about 40 μA or less, in some embodiments about 20 μA or less, and in some embodiments, about 0.1 to about 10 μA. After exposure to a hot atmosphere and a rated voltage for a considerable period of time, such as about 100 hours or more, in some embodiments about 300 hours to about 3000 hours, and in some embodiments, about 400 hours to about 2500 hours (e.g., about 500 hours), the leakage current may also remain within the above noted range, or even lower.
[0020] Various embodiments of the present invention will now be described in further detail.
[0021] I. Capacitor Components
[0022] A. Anode
[0023] The capacitor element includes an anode containing a dielectric formed on a sintered porous body. The porous anode body can be formed from a powder containing a valve metal compound (i.e., a metal capable of oxidation), such as tantalum, niobium, aluminum, hafnium, titanium, alloys thereof, oxides thereof, nitrides thereof, and the like. Tantalum is particularly suitable. For example, the powder can be formed by a reduction process in which a tantalum salt (e.g., potassium fluorotantalate (K2TaF7), sodium fluorotantalate (Na2TaF7), tantalum pentachloride (TaCl5), etc.) reacts with a reducing agent. The reducing agent can be provided in liquid, gas (e.g., hydrogen) or solid form, such as a metal (e.g., sodium), a metal alloy, or a metal salt. In one embodiment, for example, a tantalum salt (e.g., TaCl5) can be heated at a temperature of about 900°C to about 2,000°C, in some embodiments, from about 1,000°C to about 1,800°C, and in some embodiments, from about 1,100°C to about 1,600°C, to form a vapor that can be reduced in the presence of a gaseous reducing agent (e.g., hydrogen). Additional details of the reduction reaction can be described in Maeshima et al. of WO2014 / 199480. After reduction, the product can be cooled, crushed and washed to form a powder.
[0024] The charge-to-mass ratio of the powder typically varies between about 2,000 and about 800,000 microfarads*volts per gram ("μF*V / g"), depending on the desired application. For example, in certain embodiments, a high charge powder having a charge-to-mass ratio of about 100,000 to about 800,000 μF*V / g may be used, in some embodiments, about 120,000 to about 700,000 μF*V / g, and in some embodiments, about 150,000 to about 600,000 μF*V / g. In other embodiments, a low charge powder having a charge-to-mass ratio of about 2,000 to about 100,000 μF*V / g may be used, in some embodiments, about 5,000 to about 80,000 μF*V / g, and in some embodiments, about 10,000 to about 70,000 μF*V / g. As is known in the art, the charge-to-mass ratio can be determined by multiplying the capacitance by the anodization voltage used and then dividing the product by the weight of the anodized electrode body.
[0025] The powder can be a free-flowing, finely divided powder containing primary particles. Generally, the median particle size (D50) of the primary particles of the powder is about 5 to about 250 nanometers, in some embodiments, about 10 to about 200 nanometers, and in some embodiments, about 20 to about 150 nanometers, such as using a laser particle size distribution analyzer (e.g., LS-230) manufactured by BECKMAN COULTER Corporation, optionally after subjecting the particles to 70 seconds of ultrasonic vibration. Primary particles typically have a three-dimensional granular shape (e.g., knotty or angular). Such particles typically have a relatively low "aspect ratio", which is the average diameter or width of the particles divided by the average thickness ("D / T") . For example, the aspect ratio of the particles can be about 4 or less, in some embodiments, about 3 or less, and in some embodiments, about 1 to about 2. In addition to primary particles, the powder may also contain other types of particles, such as secondary particles formed by agglomerating (or agglomerating) primary particles. Such secondary particles may have a median particle size (D50) of from about 1 to about 500 microns, and in some embodiments, from about 10 to about 250 microns.
[0026] Agglomeration of the particles may occur by heating the particles and / or by using a binder. For example, agglomeration may occur at a temperature of about 0°C to about 40°C, in some embodiments about 5°C to about 35°C, and in some embodiments, about 15°C to about 30°C. Suitable binders may likewise include, for example, poly(vinyl butyral); poly(vinyl acetate); poly(vinyl alcohol); poly(vinyl pyrrolidone); cellulosic polymers such as carboxymethyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose and methyl hydroxyethyl cellulose; random polypropylene, polyethylene; polyethylene glycol (e.g., Carbowax from Dow Chemical Co.); polystyrene, poly(butadiene / styrene); polyamides, polyimides and polyacrylamides, high molecular weight polyethers; copolymers of ethylene oxide and propylene oxide; fluoropolymers such as polytetrafluoroethylene, polyvinylidene fluoride and fluoroolefin copolymers; acrylic polymers such as sodium polyacrylate, poly(lower alkyl acrylates), poly(lower alkyl methacrylates) and copolymers of lower alkyl acrylates and lower alkyl methacrylates; and fatty acids and waxes such as stearic acid and other soap fatty acids, vegetable waxes, microcrystalline waxes (purified paraffin wax), and the like.
[0027] The resulting powder can be compacted to form pellets using any conventional powder compacting equipment. For example, a press die can be used that is a single-station compaction press containing a die and one or more punches. Alternatively, an anvil-type compaction press die can be used that uses only a die and a lower punch. There are several basic types of single-station compaction press dies, such as cam, toggle / knuckle and eccentric / crank presses with different functions, such as single-action, double-action, floating die, movable platen, opposed ram, screw, impact, hot pressing, stamping or sizing. The powder can be compacted around the anode lead, which can be in the form of a wire, sheet, etc. The lead can extend longitudinally from the anode body and can be formed of any conductive material, such as tantalum, niobium, aluminum, hafnium, titanium, etc., and conductive oxides and / or nitrides thereof. Connection of the lead wires may also be accomplished using other known techniques, such as by welding the lead wires to the body or embedding them within the anode body during forming (eg, prior to compacting and / or sintering).
[0028] After pressing, any binder can be removed by heating the pellets at a temperature (e.g., about 150° C. to about 500° C.) under vacuum for several minutes. Alternatively, the binder can also be removed by contacting the pellets with an aqueous solution, such as Bishop et al. 6,197,252 of . Thereafter, the pellets are sintered to form a porous, monolithic mass. Typically, the pellets are sintered at a temperature of about 700°C to about 1600°C, in some embodiments about 800°C to about 1500°C, and in some embodiments, about 900°C to about 1200°C, for a duration of about 5 minutes to about 100 minutes, and in some embodiments, about 8 minutes to about 15 minutes. This can occur in one or more steps. If desired, sintering can occur in an atmosphere that limits the transfer of oxygen atoms to the anode. For example, sintering can occur in a reducing atmosphere, such as in a vacuum, an inert gas, hydrogen, and the like. The reducing atmosphere can be at a pressure of about 10 torr to about 2000 torr, in some embodiments about 100 torr to about 1000 torr, and in some embodiments, about 100 torr to about 930 torr. A mixture of hydrogen and other gases (e.g., argon or nitrogen) can also be used.
[0029] B. Dielectric
[0030] The anode is also coated with a dielectric. The dielectric can be formed by anodizing the sintered anode ("anodizing") to form a dielectric layer on and / or in the anode. For example, a tantalum (Ta) anode can be anodized to tantalum pentoxide (Ta2O5). Typically, anodization is performed by first applying a solution to the anode, such as by immersing the anode in an electrolyte. A solvent, such as water (e.g., deionized water) is generally used. In order to enhance ionic conductivity, a compound that can dissociate (dissociating, ionizing) to form ions in a solvent can be used. Examples of such compounds include, for example, acids, such as described below with respect to electrolytes. For example, an acid (e.g., phosphoric acid) can constitute about 0.01% by weight to about 5% by weight of an anodizing solution, about 0.05% by weight to about 0.8% by weight in some embodiments, and about 0.1% by weight to about 0.5% by weight in some embodiments. If desired, a blend of acids can also be used.
[0031] A current is passed through the anodizing solution to form a dielectric layer. The value of the formation voltage controls the thickness of the dielectric layer. For example, the power supply may be initially set in a constant current mode until the desired voltage is reached. Thereafter, the power supply may be switched to a constant potential mode to ensure that the desired dielectric thickness is formed on the entire surface of the anode. Of course, other known methods, such as pulse or step constant potential methods, may also be used. The voltage range for anodization is typically about 4 to about 250V, and in some embodiments, about 9 to about 200V, and in some embodiments, about 20 to about 150V. During oxidation, the anodizing solution may be maintained at an elevated temperature, such as about 30°C or higher, about 40°C to about 200°C in some embodiments, and about 50°C to about 100°C in some embodiments. Anodization may also be performed at ambient temperature or lower temperatures. The resulting dielectric layer may be formed on the surface of the anode or in its pores.
[0032] Although not required, in some embodiments, the dielectric layer may have different thicknesses throughout the anode, wherein it has a first portion overlying the outer surface of the anode and a second portion overlying the inner surface of the anode. In these embodiments, the first portion is selectively formed so that its thickness is greater than the thickness of the second portion. However, it should be understood that the thickness of the electrolyte layer does not need to be uniform in a particular region. For example, some portions of the dielectric layer adjacent to the outer surface may actually be thinner than a portion of the layer at the inner surface, and vice versa. Nevertheless, the dielectric layer may be formed so that at least a portion of the layer at the outer surface has a thickness greater than at least a portion at the inner surface. Although the exact difference between these thicknesses may vary depending on the specific application, the ratio of the thickness of the first portion to the thickness of the second portion is typically about 1.2 to about 40, about 1.5 to about 25 in some embodiments, and about 2 to about 20 in some embodiments.
[0033] In order to form a dielectric layer with different thicknesses, a multi-stage method is generally used. In each stage of the method, the sintered anode is anodized ("anodized") to form a dielectric layer (e.g., tantalum pentoxide). During the first stage of anodization, a relatively low formation voltage is typically used to ensure that the desired dielectric thickness is achieved for the inner region, such as a formation voltage range of about 1 to about 90 volts, about 2 to about 50 volts in some embodiments, and about 5 to about 20 volts in some embodiments. Thereafter, the sintered body can be anodized in the second stage of the method subsequently to increase the thickness of the dielectric to a desired level. This is generally accompanied by anodization in an electrolyte at a voltage higher than that used during the first stage, such as a formation voltage ranging from about 50 to about 350 volts, about 60 to about 300 volts in some embodiments, and about 70 to about 200 volts in some embodiments. During the first and / or second stages, the electrolyte may be maintained at a temperature ranging from about 15°C to about 95°C, in some embodiments from about 20°C to about 90°C, and in some embodiments, from about 25°C to about 85°C.
[0034] The electrolyte used during the first and second stages of the anodizing method may be the same or different. However, typically, it is desirable to use different solutions to help better facilitate obtaining a higher thickness in the outer portion of the dielectric layer. For example, it is desirable that the electrolyte used in the second stage has a lower ionic conductivity than the electrolyte used in the first stage to prevent the formation of a significant amount of oxide film on the inner surface of the anode. In this regard, the electrolyte used during the first stage may contain an acidic compound, such as hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, polyphosphoric acid, boric acid, boric acid, etc. Such an electrolyte may have a conductivity of about 0.1 to about 100mS / cm, in some embodiments, about 0.2 to about 20mS / cm, and in some embodiments, about 1 to about 10mS / cm, measured at a temperature of 25°C. The electrolyte used during the second stage typically contains a salt of a weak acid, so that the hydronium ion concentration in the pores increases due to the charge channel in the pores. Ion transport or diffusion causes weak acid anions to move into the pores to balance the charge when necessary. As a result, the concentration of the main conductive species (hydrogen ions) is reduced in the establishment of a balance between hydronium ions, acid anions and undissociated acids, thereby forming a material with poorer conductivity. The reduction in the concentration of conductive species results in a relatively high voltage drop in the electrolyte, which hinders further anodization of the interior, while establishing a thicker oxide layer at the outside of the higher formation voltage in the region of continuous high conductivity. Suitable weak acid salts may include, for example, ammonium or alkali metal salts (e.g., sodium, potassium, etc.) of boric acid, boric acid (boronic acid), acetic acid, oxalic acid, lactic acid, adipic acid, etc. Particularly suitable salts include sodium tetraborate and ammonium pentaborate. Such electrolytes typically have a conductivity of about 0.1 to about 20 mS / cm, in some embodiments about 0.5 to about 10 mS / cm, and in some embodiments, about 1 to about 5 mS / cm, measured at a temperature of 25°C.
[0035] If necessary, each stage of anodization may be repeated for one or more cycles to achieve the desired dielectric thickness.Further, after the first and / or second stage, the anode may also be washed or cleaned with another solvent (eg, water) to remove the electrolyte.
[0036] C. Organofunctional silane compounds
[0037] As indicated above, an organofunctional silane compound is also applied to the dielectric that can bond with the oxide of the dielectric (e.g., tantalum pentoxide) and the hydroxyl functional compound in the solid electrolyte. Typically, the organofunctional silane compound has the following general formula (I):
[0038]
[0039] in,
[0040] R1, R2 and R3 are independently alkyl (e.g., methyl, ethyl, propyl, etc.), alkenyl (e.g., vinyl, propenyl, etc.), aryl (e.g., phenyl), heteroaryl (e.g., pyridyl), cycloalkyl (e.g., cyclopropyl, cyclobutyl, etc.), heterocyclyl (e.g., piperidinyl), halogen (e.g., fluorine), haloalkyl (e.g., fluoroalkyl), or hydroxyalkyl (e.g., hydroxymethyl, hydroxyethyl, hydroxypropyl, etc.), or a combination thereof (e.g., alkyl-phenyl); and
[0041] X is a functional group capable of bonding to a hydroxyl group or capable of being converted into a functional group capable of bonding to a hydroxyl group; and
[0042] Z is an organic group that connects the functional group "X" to the silicon atom, such as an alkyl group, an alkenyl group, an aryl group, a heteroaryl group, a cycloalkyl group, a heterocyclyl group, a halogen group, a haloalkyl group or a hydroxyalkyl group, or a combination thereof.
[0043] In certain embodiments, at least one of R1, R2 and R3 may be a hydroxyalkyl group (e.g., OCH3). For example, each of R1, R2 and R3 may be a hydroxyalkyl group. However, in other embodiments, R1 may be an alkyl group (e.g., CH3) and R2 and R3 may be hydroxyalkyl groups (e.g., OCH3). Z may also be an alkyl group (e.g., methyl, propyl, ethyl, butyl, etc.), an aryl group (e.g., phenyl), or an alkyl-aryl group (e.g., phenethyl).
[0044] The specific nature of the functional group "X" may vary. For example, in one embodiment, X is a functional group capable of reacting with a hydroxyl group, such as an amino functional group, an isocyanate functional group, an isocyanurate functional group, and the like. For example, an isocyanate functional group can form a carbamate bond with a hydroxyl functional polymer in a solid electrolyte. In a specific embodiment, an isocyanate functional organosilane compound having the following general formula (II) may be used:
[0045]
[0046] in,
[0047] R1, R2, R3 and Z are as defined above. Suitable isocyanate functional organosilane compounds may include, for example, 3-isocyanatopropyltriethoxysilane (R1, R2 and R3 are OCH2CH3 and Z is propyl), 3-isocyanatopropyltrimethoxysilane (R1, R2 and R3 are OCH3 and Z is propyl), 3-isocyanantopropylmethyldiethoxysilane (R1 is CH3, R2 and R3 are OCH2CH3 and Z is propyl), 3-isocyanatopropylmethyldiethoxysilane (R1 is CH3, R2 and R3 are OCH3 and Z is propyl), and the like.
[0048] In the above-mentioned embodiment, the presence of certain types of functional groups (e.g., isocyanates) can allow direct reaction of organosilane compounds with hydroxy-functional polymers. However, in some cases, it may be desirable to "mask" the functional group during at least a portion of the capacitor manufacturing process. In this way, the possibility of premature degradation of the functional group can be minimized so that it can be mainly used during the use conditions, such as at high temperatures, for reacting with hydroxy-functional polymers. In such an embodiment, X can be a blocking group that can be converted into a functional group (e.g., isocyanate functional group) that can subsequently react with a hydroxyl group. The conversion of the blocking group to the functional group ideally only occurs under certain conditions, such as when heated, when exposed to ultraviolet light, etc. For example, examples of blocking groups that can be converted into isocyanate groups can include thiocyanate groups (-SCN), carbamate groups (-NR4C(O)O-R5-, for example, wherein R4 and R5 are independently hydrogen or alkyl groups), isocyanurate groups, etc. If desired, the functional group and / or the protecting group may also contain other silane groups so that the resulting compound is difunctional, trifunctional, etc. Specific examples of such masked organosilane compounds may include, for example, (thiocyanatomethyl)phenethyl-trimethoxysilane (R1, R2 and R3 are OCH3, Z is -CH2CH2-phenyl-CH2-, and X is SCN), 3-thiocyanatopropyltriethoxysilane (R1, R2 and R3 are OCH2CH3, Z is -CH2CH2CH2-, and X is SCN), N-(3-triethoxysilylpropyl)-o-tert-butylcarbamate (R1, R2 and R3 are OCH2CH3, Z is -CH2CH2-CH2-, and X is NHC(O)O -tert-butyl), triethoxysilylpropylethylcarbamate (R1, R2 and R3 are OCH2CH3, Z is -CH2CH2-CH2-, and X is NHC(O)O-ethyl), N-trimethoxysilylpropylmethylcarbamate (R1, R2 and R3 are OCH2CH3, Z is -CH2CH2-CH2-, and X is NHC(O)O-methyl), tris(3-trimethoxysilylpropyl)isocyanurate (R1, R2 and R3 are OCH3, Z is -CH2CH2-CH2-, and X is isocyanurate-[CH2CH2CH2-Si(OCH3)3]2), etc., and combinations thereof.
[0049] Regardless of the specific compound used, the organofunctional silane compound can be bonded to the dielectric oxide using techniques known in the art. For example, the organofunctional silane compound can be subjected to a hydrolysis reaction, wherein one or more groups (e.g., R1, R2, and / or R3 in formula (I)) are converted to hydroxyl groups. These hydroxyl groups, in turn, react with the dielectric oxide via a condensation reaction, such that the organofunctional silane compound becomes grafted or bonded to the dielectric.
[0050] To initiate the reaction, the organofunctional silane compound may first be dissolved in a solvent to form a solution. Particularly suitable are organic solvents such as hydrocarbons (e.g., benzene, toluene, and xylene); ethers (e.g., tetrahydrofuran, 1,4-dioxane, and diethyl ether); ketones (e.g., methyl ethyl ketone); halogen-based solvents (e.g., chloroform, dichloromethane, and 1,2-dichloroethane); alcohols (e.g., methanol, ethanol, isopropanol, and isobutanol); and the like, as well as any combination of the foregoing. Alcohols are particularly suitable for use in the present invention. The concentration of the organic solvent in the solution may vary, but is typically used in an amount of about 70% to about 99% by weight of the solution, in some embodiments about 80% to about 98% by weight, and in some embodiments, about 85% to about 97% by weight. Similarly, the organofunctional silane compound may constitute about 1% to about 30% by weight of the solution, in some embodiments about 2% to about 20% by weight, and in some embodiments, about 3% to about 15% by weight. Once formed, the solution is applied to the dielectric using any of a variety of known techniques, such as by dipping, dripping, spin coating, spraying, etc. The solution can then be heated to remove the solvent and bond the organofunctional silane compound to the dielectric. The heating can occur at a temperature of 25°C to about 350°C, in some embodiments about 30°C to about 325°C, and in some embodiments, about 50°C to about 300°C. Likewise, the length of time for heating can vary, but is typically about 1 to about 100 minutes, in some embodiments about 2 to about 60 minutes, and in some embodiments, about 4 to about 50 minutes. Once the solvent is removed, a silane network can be generated in which oxygen atoms connect adjacent silicon atoms and also covalently bond silicon atoms to the dielectric. At the interface, the silane reacts with itself and also with the dielectric, crosslinking and mechanically interlocking with the layer.
[0051] As discussed above, the functional groups of the silane compound can also be used to bond to the hydroxyl-functional polymer present in the solid electrolyte. The nature of the bond can vary depending on the specific compound used, such as covalent bonds, ionic bonds, hydrogen bonds, etc. For example, the isocyanate group of the silane compound can form a carbamate bond with the hydroxyl-functional polymer. As noted, the bonding between the organofunctional silane compounds can occur during the formation of the capacitor, or even after the capacitor is formed, depending on the specific use or storage conditions. For example, in some embodiments, the bonding between the silane compound and the hydroxyl-functional polymer can only occur during certain conditions, such as at high temperature and / or voltage. For example, in one embodiment, the masked organosilane compound may contain a protective group (e.g., an isocyanate group) that can be converted to a functional group (e.g., an isocyanate group). The conversion can occur at a relatively high temperature, such as at a temperature of about 100°C or higher, in some embodiments, about 120°C to about 350°C, and in some embodiments, about 150°C to about 250°C.
[0052] D. Solid Electrolyte
[0053] As indicated above, the solid electrolyte overlies the dielectric and generally serves as the cathode of the capacitor assembly. The solid electrolyte contains one or more layers containing extrinsic and / or intrinsic conductive polymers. In certain embodiments, a "non-intrinsic" conductive polymer having a repeating unit of the following formula (IV) may be used in the solid electrolyte:
[0054]
[0055] in,
[0056] R7 is a straight chain or branched chain, C1 to C 18 Alkyl groups (e.g., methyl, ethyl, n-propyl or isopropyl, n-butyl, isobutyl, sec-butyl or tert-butyl, n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1-ethylpropyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 2,2-dimethylpropyl, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, etc.); C5 to C 12 Cycloalkyl groups (e.g., cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, etc.); C6 to C 14 Aryl group (eg, phenyl, naphthyl, etc.); C7 to C 18 Aralkyl groups (e.g., benzyl, o-tolyl, m-tolyl, p-tolyl, 2,3-xylyl, 2,4-xylyl, 2,5-xylyl, 2-6-xylyl, 3-4-xylyl, 3,5-xylyl, (mesityl, etc.); and
[0057] q is an integer from 0 to 8, in some embodiments, from 0 to 2, and in one embodiment, is 0. In a specific embodiment, "q" is 0 and the polymer is poly(3,4-ethylenedioxythiophene). A commercially suitable example of a monomer suitable for forming the polymer is 3,4-ethylenedioxythiophene, which can be found under the name Clevios TM M was obtained from Heraeus.
[0058] The polymers of formula (IV) are generally considered to be "extrinsic" conductive to the extent that they typically require the presence of a separate counterion that is not covalently bonded to the polymer. The counterion may be a sulfonyl ion that may be provided in the form of a monomeric or polymeric anion. For example, the polymeric anion may be a polymeric sulfonic acid (including its salts), such as polystyrene sulfonic acid or sulfonate ("PSS"), polyvinyl sulfonic acid, and the like. The acid may also be a copolymer, such as a copolymer of vinyl carboxylic acid and vinyl sulfonic acid with other polymerizable monomers (such as acrylates and styrene). Similarly, suitable monomeric anions include, for example, the following anions: C1 to C 20 an alkanesulfonic acid or a salt thereof (e.g., dodecanesulfonic acid); an aliphatic perfluorosulfonic acid or a salt thereof (e.g., trifluoromethanesulfonic acid, perfluorobutanesulfonic acid or perfluorooctanesulfonic acid); optionally C1 to C 20 Alkyl group-substituted aromatic sulfonic acid or salt thereof (e.g., benzenesulfonic acid, o-toluenesulfonic acid, p-toluenesulfonic acid or dodecylbenzenesulfonic acid); cycloalkanesulfonic acid or salt thereof (e.g., camphorsulfonic acid or tetrafluoroborate, hexafluorophosphate, perchlorate, hexafluoroantimonate, hexafluoroarsenate or hexachloroantimonate); etc. A particularly suitable polymeric anion is PSS.
[0059] Intrinsically conductive polymers in which the positive charge (which is at least partially compensated by the sulfonate groups covalently bonded to the polymer) is located on the backbone can also be used. For example, one example of a suitable intrinsically conductive polymer may have a repeating unit of the following formula (V):
[0060]
[0061] in,
[0062] R is (CH2) a -O-(CH2) b ;
[0063] a is 0 to 10, in some embodiments 0 to 6, and in some embodiments, 1 to 4 (e.g., 1);
[0064] b is 1 to 18, in some embodiments 1 to 10, and in some embodiments, 2 to 6 (e.g., 2, 3, 4, or 5);
[0065] Z is an anion, such as a sulfonyl anion (e.g. SO3 - CF3SO3 - wait);
[0066] X is a cation such as hydrogen, an alkali metal (eg, lithium, sodium, rubidium, cesium, or potassium), ammonium, or the like.
[0067] In a specific embodiment, Z in formula (V) is SO3, so that the intrinsically conductive polymer contains repeating units of the following formula (VI):
[0068]
[0069] wherein R and X are as defined above. In formula (V) or (VI), a is preferably 1 and b is preferably 3 or 4. Likewise, X is preferably sodium or potassium.
[0070] If desired, the polymer may be a copolymer containing other types of repeating units. In these embodiments, the repeating units of formula (VI) typically constitute about 50 mol% or more of the total amount of repeating units in the copolymer, in some embodiments, about 75 mol% to about 99 mol%, and in some embodiments, about 85 mol% to about 95 mol%. Of course, the polymer may also be a homopolymer, to the extent that it contains 100 mol% of the repeating units of formula (II). Specific examples of such homopolymers include poly (4-(2,3-dihydrothieno-[3,4-b][1,4] ... In-2-ylmethoxy)-1-butane-sulfonic acid, salt) and poly (4-(2,3-dihydrothieno-[3,4-b][l,4]di ((2-((((((((((((((((((((- ...
[0071] A conductive polymer layer can be formed using a variety of methods. For example, an in-situ polymerized layer can be formed by chemically polymerizing the monomer in the presence of an oxidation catalyst. The oxidation catalyst typically includes transition metal cations, such as iron (III), copper (II), chromium (VI), cerium (IV), manganese (IV), manganese (VII) or ruthenium (III) cations, etc. Dopants can also be used to provide excess charge to the conductive polymer and stabilize the conductivity of the polymer. Dopants typically include sulfonyl anions. In certain embodiments, the oxidation catalyst has both catalytic and doping functions because it includes cations (e.g., transition metals) and sulfonyl anions. For example, the oxidation catalyst can be a transition metal salt, which includes iron (III) cations, such as iron (III) halides (e.g., FeCl3) or iron (III) salts of other inorganic acids, such as Fe(ClO4)3 or Fe2(SO4)3 and iron (III) salts of organic acids and inorganic sulfonic acids. Examples of iron (III) salts of inorganic sulfonic acids include, for example, C1 to C 20 Examples of iron (III) salts of sulfuric acid monoesters of alkanols (e.g., iron (III) salts of lauryl sulfate). Similarly, examples of iron (III) salts of organic sulfonic acids include, for example, C1 to C 20 an iron(III) salt of an alkanesulfonic acid (e.g., methane, ethane, propane, butane or dodecanesulfonic acid); an iron(III) salt of an aliphatic perfluorosulfonic acid (e.g., trifluoromethanesulfonic acid, perfluorobutanesulfonic acid or perfluorooctanesulfonic acid); optionally replaced by a C1 to C 20 Iron (III) salts of aromatic sulfonic acids substituted with alkyl groups (e.g., benzenesulfonic acid, o-toluenesulfonic acid, p-toluenesulfonic acid or dodecylbenzenesulfonic acid); iron (III) salts of cycloalkanesulfonic acids (e.g., camphorsulfonic acid); and the like. Mixtures of the above iron (III) salts can also be used. Particularly suitable are iron (III) p-toluenesulfonate, iron (III) o-toluenesulfonate and mixtures thereof. A commercially suitable example of iron (III) p-toluenesulfonate is available under the name Clevios TM C was obtained from Heraeus Clevios.
[0072] The oxidation catalyst and monomer may be applied sequentially or together to initiate the polymerization reaction. Suitable application techniques for applying these components include screen printing, dipping, electrophoretic coating, and spraying. As an example, the monomer may first be mixed with the oxidation catalyst to form a precursor solution. Once the mixture is formed, it may be applied to the anode component and then allowed to polymerize so that a conductive coating is formed on the surface. Alternatively, the oxidation catalyst and monomer may be applied sequentially. In one embodiment, for example, the oxidation catalyst is dissolved in an organic solvent (e.g., butanol) and then applied (applied) as an immersion solution. The component may then be dried to remove the solvent therefrom. Thereafter, the component may be immersed in a solution containing the monomer. In any case, the polymerization is typically carried out at a temperature of about -10°C to about 250°C, and in some embodiments, about 0°C to about 200°C, depending on the oxidizing agent used and the desired reaction time. Suitable polymerization techniques (such as those described above) may be used in the following embodiments. Biler Other methods of applying such conductive coatings are described in more detail in U.S. Pat. No. 7,515,396. Sakata et al. U.S. Patent No. 5,457,862, Sakata et al. 5,473,503 Sakata et al. 5,729,428 and Kudoh et al. of 5,812,367.
[0073] In addition to in situ application, the conductive polymer can also be applied in the form of a dispersion of conductive polymer particles. One benefit of using a dispersion is that it allows the ionic species (e.g., Fe 2+ or Fe 3 +) is minimized, which can cause dielectric breakdown (breakdown) under high electric fields due to ion migration. Therefore, by applying the conductive polymer as a dispersion rather than by in-situ polymerization, the resulting capacitor can exhibit a relatively high "breakdown voltage". In order to enable good impregnation of the anode, the particles used in the dispersion typically have a small size, such as an average size (e.g., diameter) of about 1 to about 150 nanometers, in some embodiments, about 2 to about 50 nanometers, and in some embodiments, about 5 to about 40 nanometers. The diameter of the particles can be determined using known techniques, such as by ultracentrifugation, laser diffraction, etc. The shape of the particles can also vary. In a specific embodiment, for example, the particle shape is spherical. However, it should be understood that other shapes are also considered in the present invention, such as plates, rods, disks, rods, tubes, irregular shapes, etc. The concentration of the particles in the dispersion can vary, depending on the desired dispersion viscosity and the specific way the dispersion is applied to the capacitor. However, the particles typically constitute from about 0.1 to about 10 weight percent of the dispersion, in some embodiments, from about 0.4 to about 5 weight percent, and in some embodiments, from about 0.5 to about 4 weight percent.
[0074] The dispersion may also contain one or more components to enhance the overall properties of the resulting solid electrolyte. For example, the dispersion may contain a binder to further enhance the adhesive properties of the polymer layer and also improve the stability of the particles in the dispersion. The binder may be organic in nature, such as polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl chloride, polyvinyl acetate, polyvinyl butyrate, polyacrylate, polyacrylamide, polymethacrylate, polymethacrylamide, polyacrylonitrile, styrene / acrylate, vinyl acetate / acrylate and ethylene / vinyl acetate copolymers, polybutadiene, polyisoprene, polystyrene, polyether, polyester, polycarbonate, polyurethane, polyamide, polyimide, polysulfone, melamine formaldehyde resin, epoxy resin, silicone resin or cellulose. A crosslinking agent may also be used to enhance the adhesion of the binder. Such a crosslinking agent may include, for example, a melamine compound, a masked isocyanate or a crosslinkable polymer, such as a polyurethane, polyacrylate or polyolefin, and then crosslinked. A dispersing agent may also be used to promote the ability of the layer to be applied to the anode. Suitable dispersing agents include solvents such as aliphatic alcohols (e.g., methanol, ethanol, isopropanol and butanol), aliphatic ketones (e.g., acetone and methyl ethyl ketone), aliphatic carboxylates (e.g., ethyl acetate and butyl acetate), aromatic hydrocarbons (e.g., toluene and xylene), aliphatic hydrocarbons (e.g., hexane, heptane and cyclohexane), chlorinated hydrocarbons (e.g., methylene chloride and ethylene dichloride), aliphatic nitriles (e.g., acetonitrile), aliphatic sulfoxides and sulfones (e.g., dimethyl sulfoxide and sulfolane), aliphatic carboxylic acid amides (e.g., methylacetamide, dimethylacetamide and dimethylformamide), aliphatic and aromatic aliphatic ethers (e.g., diethyl ether and anisole), water, and mixtures of any of the foregoing solvents. A particularly suitable dispersing agent is water.
[0075] In addition to those mentioned above, other ingredients can also be used in the dispersion. For example, conventional fillers having a size of about 10 nanometers to about 100 microns can be used, in some embodiments, about 50 nanometers to about 50 microns, and in some embodiments, about 100 nanometers to about 30 microns. Examples of such fillers include calcium carbonate, silicates, silicon dioxide, calcium sulfate or barium sulfate, aluminum hydroxide, glass fibers or bulbs, wood powder, cellulose powder carbon black, conductive polymers, etc. Fillers can be introduced into the dispersion in powder form, but fillers can also exist in other forms, such as fibers.
[0076] Surface active substances such as ionic or nonionic surfactants may also be used in the dispersion. Further, adhesives such as organofunctional silanes or their hydrolyzates, for example 3-glycidyloxypropyltrialkoxysilane, 3-aminopropyl-triethoxysilane, 3-mercaptopropyl-trimethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane or octyltriethoxysilane may be used. The dispersion may also contain additives that increase the conductivity, such as compounds containing ether groups (e.g., tetrahydrofuran), compounds containing lactone groups (e.g., γ-butyrolactone or γ-valerolactone), compounds containing amide or lactam groups (e.g., caprolactam, N-methylcaprolactam, N,N-dimethylacetamide, N-methylacetamide, N,N-dimethylformamide (DMF), N-methylformamide, N-methylformanilide, N-methylpyrrolidone (NMP), N-octylpyrrolidone or pyrrolidone), sulfones and sulfoxides (e.g., sulfolane (tetramethylene sulfone) or dimethyl sulfoxide (DMSO)), sugars or sugar derivatives (e.g., sucrose, glucose, fructose or lactose), sugar alcohols (e.g., sorbitol or mannitol), furan derivatives (e.g., 2-furancarboxylic acid or 3-furancarboxylic acid), alcohols (e.g., ethylene glycol, glycerol, diethylene glycol or triethylene glycol).
[0077] As shown above, hydroxy-functional polymers are also used in solid electrolytes. The term "hydroxy-functional" generally means a compound containing at least one hydroxy-functional group or capable of having such a functional group in the presence of a solvent. Without wishing to be limited by theory, it is believed that the use of hydroxy-functional polymers with a certain molecular weight can minimize the possibility of chemical decomposition at high voltages. For example, the molecular weight of the hydroxy-functional polymer can be about 100 to 10,000 grams per mole, in some embodiments about 200 to 2,000, in some embodiments about 300 to about 1,200, and in some embodiments, about 400 to about 800.
[0078] Generally, any of the various hydroxy-functional polymers can be used for this purpose. In one embodiment, for example, the hydroxy-functional polymer is a polyalkylene ether. Polyalkylene ethers can include polyalkylene glycols (for example, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyepichlorohydrin, etc.), polyoxetanes, polyphenylene oxides, polyether ketones, etc. Polyalkylene ethers are typically mainly linear hydroxy-functional polymers with terminal hydroxyl groups. Particularly suitable are polyethylene glycol, polypropylene glycol and polytetramethylene glycol (polytetrahydrofuran), which are prepared by adding ethylene oxide, propylene oxide or tetrahydrofuran to water. Polyalkylene ethers can be prepared by diols or polyols by polycondensation. In particular, the diol component can be selected from: saturated or unsaturated, branched or unbranched, aliphatic or aromatic dihydroxy compounds containing 5 to 36 carbon atoms, such as, for example, pentane-1,5-diol, hexane-1,6-diol, neopentyl glycol, bis-(hydroxymethyl)-cyclohexane, bisphenol A, dimer diol, hydrogenated dimer diol or even mixtures of the diols mentioned. In addition, polyols can also be used in the polymerization reaction, including, for example, glycerol, diglycerol and polyglycerol, trimethylolpropane, pentaerythritol or sorbitol.
[0079] In addition to those mentioned above, other hydroxyl functional polymers may also be used in the present invention. Some examples of such polymers include, for example, ethoxylated alkylphenols; ethoxylated or propoxylated C6-C 24 Fatty alcohols; polyoxyethylene glycol alkyl ethers having the following general formula: CH3-(CH2) 10-16 -(O-C2H4) 1-25 -OH (e.g., octaethylene glycol monododecyl ether and pentaethylene glycol monododecyl ether); polyoxypropylene glycol alkyl ethers having the following general formula: CH3-(CH2) 10-16 -(O-C3H6) 1-25 -OH; polyoxyethylene glycol octylphenol ether having the following general formula: C8H 17 -(C6H4)-(O-C2H4) 1-25 -OH (e.g., Triton TM X-100); polyoxyethylene glycol alkylphenol ether having the following general formula: C9H 19 -(C6H4)-(O-C2H4) 1-25 -OH (e.g., nonoxynol-9); C8-C 24Polyoxyethylene glycol esters of fatty acids, such as polyoxyethylene glycol sorbitan alkyl esters (e.g., polyoxyethylene (20) sorbitan monolaurate, polyoxyethylene (20) sorbitan monopalmitate, polyoxyethylene (20) sorbitan monostearate, polyoxyethylene (20) sorbitan monooleate, PEG-20 methyl glucose distearate, PEG-20 methyl glucose sesquistearate, PEG-80 castor oil and PEG-20 castor oil, PEG-3 castor oil, PEG 600 dioleate and PEG 400 dioleate) and polyoxyethylene glyceryl alkyl esters (e.g., polyoxyethylene-23 glyceryl laurate and polyoxyethylene-20 glyceryl stearate); C8-C 24 Polyoxyethylene glycol ethers of fatty acids (e.g., polyoxyethylene-10 cetyl ether, polyoxyethylene-10 stearyl ether, polyoxyethylene-20 cetyl ether, polyoxyethylene-10 oleyl ether, polyoxyethylene-20 oleyl ether, polyoxyethylene-20 isocetyl ether, polyoxyethylene-15 tridecyl ether, and polyoxyethylene-6 tridecyl ether); block copolymers of polyethylene glycol and polypropylene glycol (e.g., Poloxamers); and the like, and mixtures thereof.
[0080] Hydroxy-functional polymers can be incorporated into solid electrolytes in various ways. In certain embodiments, for example, hydroxy-functional polymers can be incorporated into one or more conductive polymer layers formed by dispersions of conductive polymers. In these embodiments, the concentration of hydroxy-functional polymers in the layer can be from about 1 wt % to about 50 wt %, from about 5 wt % to about 40 wt % in some embodiments, and from about 10 wt % to about 30 wt %. However, in other embodiments, hydroxy-functional polymers can be applied separately (separately) after the conductive polymer is formed. In these embodiments, the technology for applying hydroxy-functional polymers can vary. For example, various methods can be used to apply hydroxy-functional polymers in the form of liquid solutions, such as immersion, immersion, pouring, dripping, injection, spraying, spreading, coating or printing, for example, inkjet, or screen printing. Solvents known to those skilled in the art can be used in the solution, such as water, alcohol or a mixture thereof. The concentration of the hydroxyl-functional polymer in such a solution is typically from about 5% to about 95% by weight of the solution, in some embodiments from about 10% to about 70% by weight, and in some embodiments, from about 15% to about 50% by weight. If desired, such a solution may generally be free of a conductive polymer. For example, the conductive polymer may constitute about 2% or less by weight of the solution, in some embodiments about 1% or less by weight, and in some embodiments, about 0.5% or less by weight.
[0081] The dispersion can be applied using a variety of known techniques, such as by spin coating, dipping, pouring, dripping, injecting, spraying, doctor blade coating, brushing, printing (e.g., inkjet, screen printing or pad printing) or immersion. The viscosity of the dispersion is typically from about 0.1 to about 100,000 mPas (at 100 s -1 In some embodiments, the shear rate is about 0.5 to about 10,000 mPas, in some embodiments, about 1 to about 1,500 mPas, and in some embodiments, about 5 to about 1000 mPas.
[0082] D. External polymer coating
[0083] An outer polymer coating overlying the solid electrolyte may also be applied. The outer polymer coating typically contains one or more layers formed of prepolymerized conductive polymer particles, such as described above (e.g., a dispersion of non-intrinsic conductive polymer particles). The outer coating may be able to further penetrate into the edge region of the capacitor body to improve adhesion to the dielectric and produce a more mechanically strong component, which can reduce equivalent series resistance and leakage current. Since it is generally intended to improve edge coverage rather than immerse the interior of the anode body, the size of the particles used in the outer coating is typically larger than the size of the particles used in the solid electrolyte. For example, the average size of the particles used in the outer polymer coating is typically about 1.5 to about 30, in some embodiments about 2 to about 20, and in some embodiments, about 5 to about 15. For example, the average size of the particles used in the dispersion of the outer coating may be about 80 to about 500 nanometers, in some embodiments about 90 to about 250 nanometers, and in some embodiments, about 100 to about 200 nanometers.
[0084] If desired, a crosslinking agent may also be used in the outer polymer coating to enhance adhesion to the solid electrolyte. Typically, the crosslinking agent is applied prior to applying the dispersion for the outer coating. Suitable crosslinking agents are described, for example, in Merker et al. and include, for example, amines (e.g., diamines, triamines, oligoamines, polyamines, etc.); multivalent metal cations, such as salts or compounds of Mg, Al, Ca, Fe, Cr, Mn, Ba, Ti, Co, Ni, Cu, Ru, Ce, or Zn; Compounds, sulfonium compounds, etc. Particularly suitable examples include, for example, 1,4-diaminocyclohexane, 1,4-bis(aminomethyl)cyclohexane, ethylenediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, N,N-dimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,4-butanediamine, etc., and mixtures thereof.
[0085] The crosslinking agent is typically applied from a solution or dispersion having a pH of 1 to 10, in some embodiments 2 to 7, and in some embodiments 3 to 6, measured at 25° C. Acidic compounds may be used to help achieve the desired pH level. Examples of solvents or dispersants for the crosslinking agent include water or organic solvents such as alcohols, ketones, carboxylates, and the like. The crosslinking agent may be applied to the capacitor body by any known method, such as spin coating, dipping, casting, drop coating, spray application, vapor deposition, sputtering, sublimation, scraping, coating, or printing, such as inkjet, screen printing, or pad printing. Once applied, the crosslinking agent may be dried before applying the polymer dispersion. The process may then be repeated until the desired thickness is achieved. For example, the total thickness of the entire outer polymer coating (including the crosslinking agent and dispersion layer) may be from about 1 to about 50 μm, from about 2 to about 40 μm in some embodiments, and from about 5 to about 20 μm in some embodiments.
[0086] E. Other optional components
[0087] If desired, the capacitor element may also contain other layers known in the art. For example, an adhesive layer, such as an adhesive layer formed from a relatively insulating resinous material (natural or synthetic), may be optionally formed between the dielectric and the solid electrolyte. This layer may be applied before, after, or in combination with the organofunctional silane compound. The specific resistivity of the resinous material may be greater than about 10 ohm-cm, in some embodiments greater than about 100, in some embodiments greater than about 1,000 ohm-cm, and in some embodiments greater than about 1x10 5 Ohm-cm, and in some embodiments, greater than about 1x10 10Ohm-cm. Some resinous materials that can be used in the present invention include, but are not limited to, polyurethane, polystyrene, esters of unsaturated or saturated fatty acids (e.g., glycerides), etc. For example, suitable esters of fatty acids include, but are not limited to, esters of lauric acid, myristic acid, palmitic acid, stearic acid, eleostearic acid, oleic acid, linoleic acid, linolenic acid, aleuritic acid, shellolic acid, etc. It has been found that when used in relatively complex combinations to form "drying oils", these esters of fatty acids are particularly useful, which allow the resulting film to quickly polymerize into a stable layer. Such drying oils may include monoglycerides, diglycerides and / or triglycerides, which have a glycerol backbone with one, two and three esterified fatty acyl residues, respectively. For example, some suitable drying oils that can be used include, but are not limited to, olive oil, linseed oil, castor oil, tung oil, soybean oil and shellac. These and other adhesive layer materials are described in more detail in Fife et al. No. 6,674,635 of , which is incorporated herein by reference in its entirety for all purposes.
[0088] If desired, a carbon layer (e.g., graphite) and a silver layer may also be applied to the component separately. The silver coating may, for example, serve as a weldable conductor, contact layer, and / or charge collector for a capacitor and the carbon coating may limit the contact of the silver coating with the solid electrolyte. Such a coating may cover a portion or all of the solid electrolyte.
[0089] II. terminal
[0090] Once formed, the capacitor element can be provided with a terminal, particularly when used in a surface mount application. For example, the capacitor assembly may contain an anode terminal electrically connected to the anode lead of the capacitor element and a cathode terminal electrically connected to the cathode of the capacitor element. Any conductive material can be used to form the terminal, such as a conductive metal (e.g., copper, nickel, silver, nickel, zinc, tin, palladium, lead, copper, aluminum, molybdenum, titanium, iron, zirconium, magnesium and alloys thereof). Particularly suitable conductive metals include, for example, copper, copper alloys (e.g., copper-zirconium, copper-magnesium, copper-zinc or copper-iron), nickel and nickel alloys (e.g., nickel-iron). The thickness of the terminal is generally selected to minimize the thickness of the capacitor. For example, the thickness of the terminal can be from about 0.05 to about 1 mm, from about 0.05 to about 0.5 mm in some embodiments, and from about 0.07 to about 0.2 mm. An exemplary conductive material is a copper-iron alloy metal plate, which can be obtained from Wieland (Germany). If necessary, the surface of the terminal can be plated with nickel, silver, gold, tin, etc., as known in the art to ensure that the final component can be mounted to the circuit board. In a specific embodiment, both surfaces of the terminal are plated with nickel and silver flashes, respectively, and the mounting surface is also plated with a tin solder layer.
[0091] The terminals may be connected to the capacitor element using any technique known in the art. In one embodiment, for example, a lead frame defining a cathode terminal and an anode terminal may be provided. In order to attach the electrolytic capacitor element to the lead frame, a conductive adhesive may first be applied to the surface of the cathode terminal. The conductive adhesive may include, for example, conductive metal particles contained in a resin composition. The metal particles may be silver, copper, gold, platinum, nickel, zinc, bismuth, etc. The resin composition may include a thermosetting resin (e.g., an epoxy resin), a curing agent (e.g., anhydride), and a compound (e.g., a silane compound). Suitable conductive adhesives may be described in Osako et al. The conductive adhesive may be applied to the cathode termination using any of a variety of techniques. For example, printing techniques may be used due to their practical and cost-effective advantages. The anode lead may also be electrically connected to the anode termination using any technique known in the art, such as mechanical welding, laser welding, conductive adhesive, etc. When the anode lead is electrically connected to the anode termination, the conductive adhesive may then be cured to ensure that the electrolytic capacitor element is adequately adhered to the cathode termination.
[0092] III. case
[0093] Due to the ability of the capacitor assembly to exhibit good electrical performance in a variety of environments, it is not necessary to hermetically seal the capacitor element within the housing. Nevertheless, in certain embodiments, it may be desirable to hermetically seal the capacitor element within the housing. In one embodiment, for example, the capacitor element may be hermetically sealed within the housing in the presence of a gaseous atmosphere containing an inert gas, thereby further limiting the amount of moisture supplied to the solid electrolyte of the capacitor element.
[0094] Capacitor element can be sealed in housing in many ways.In some embodiments, for example, capacitor element can be encapsulated in housing, which can be filled with resin material subsequently, such as thermosetting resin (for example, epoxy resin) that can be cured to form hardened housing.The example of such resin includes, for example, epoxy resin, polyimide resin, melamine resin, urea-formaldehyde resin, polyurethane resin, phenol (phenolic) resin, polyester resin etc.Epoxy resin is particularly suitable.Other additives can also be used, such as photoinitiator, viscosity modifier, suspension aid, pigment, stress reducer, non-conductive filler, stabilizer etc.For example, non-conductive filler can include inorganic oxide particles, such as silicon dioxide, aluminum oxide, zirconium oxide, magnesium oxide, iron oxide, copper oxide, zeolite, silicate, clay (for example, montmorillonite clay) etc., and composite material (for example, silicon oxide particles coated with aluminum oxide) and mixture thereof.In any case, resin material can surround and encapsulate capacitor element, so that at least a portion of anode and cathode terminals are exposed for being installed on circuit board. When packaged in this manner, the capacitor element and resinous material form an integral capacitor assembly.
[0095] Of course, in alternative embodiments, it may be desirable to encapsulate the capacitor element in a separate and distinct housing. In this way, the atmosphere of the housing can be gaseous and contain at least one inert gas, such as nitrogen, helium, argon, xenon, neon, krypton, radon, etc., and mixtures thereof. Typically, inert gases constitute the major part of the atmosphere in the housing, such as about 50% by weight to 100% by weight of the atmosphere, about 75% by weight to 100% by weight in some embodiments, and about 90% by weight to about 99% by weight in some embodiments. If desired, relatively small amounts of non-inert gases, such as carbon dioxide, oxygen, water vapor, etc., may also be used. However, in these cases, non-inert gases typically constitute 15% by weight or less of the atmosphere in the housing, 10% by weight or less in some embodiments, about 5% by weight or less in some embodiments, about 1% by weight or less in some embodiments, and about 0.01% by weight to about 1% by weight in some embodiments.
[0096] The housing may be formed using any of a variety of different materials, such as metals, plastics, ceramics, etc. In one embodiment, for example, the housing includes one or more layers of metals, such as tantalum, niobium, aluminum, nickel, hafnium, titanium, copper, silver, steel (e.g., stainless steel), alloys thereof (e.g., conductive oxides), composites thereof (e.g., metals coated with conductive oxides), etc. In another embodiment, the housing may include one or more layers of ceramic materials, such as aluminum nitride, aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, glass, etc., and combinations thereof.
[0097] The housing may have any desired shape, such as cylindrical, D-shaped, rectangular, triangular, prismatic, etc. For example, referring to Figure 1 , shows an embodiment of a capacitor assembly 100 including a housing 122 and a capacitor element 120. In this particular embodiment, the housing 122 is generally rectangular. Typically, the housing and the capacitor element have the same or similar shapes so that the capacitor element can be easily accommodated in the internal cavity. In the illustrated embodiment, for example, both the capacitor element 120 and the housing 122 have a generally rectangular shape.
[0098] If necessary, capacitor assembly of the present invention can present relatively high volumetric efficiency.In order to promote this high efficiency, capacitor element typically occupies most of the volume of the internal chamber of housing.For example, capacitor element can occupy about 30 volume % or higher of the internal chamber of housing, about 50 volume % or higher in some embodiments, about 60 volume % or higher in some embodiments, about 70 volume % or higher in some embodiments, about 80 volume % to about 98 volume % in some embodiments, and about 85 volume % to 97 volume % in some embodiments.For this reason, the difference between the size of capacitor element and the size of the internal chamber defined by housing is typically relatively small.
[0099] Reference Figure 1, for example, the length of the capacitor element 120 (excluding the length of the anode lead 6) can be relatively similar to the length of the internal chamber 126 defined by the housing 122. For example, the ratio of the length of the anode to the length of the internal chamber is about 0.40 to 1.00, in some embodiments, about 0.50 to about 0.99, in some embodiments, about 0.60 to about 0.99, and in some embodiments, about 0.70 to about 0.98. The length of the capacitor element 120 can be about 5 to about 10 millimeters, and the length of the internal chamber 126 can be about 6 to about 15 millimeters. Similarly, the ratio of the height of the capacitor element 120 (in the -z direction) to the height of the internal chamber 126 can be about 0.40 to 1.00, in some embodiments, about 0.50 to about 0.99, in some embodiments, about 0.60 to about 0.99, and in some embodiments, about 0.70 to about 0.98. The ratio of the width of capacitor element 120 (in the -x direction) to the width of interior chamber 126 can be about 0.50 to 1.00, in some embodiments about 0.60 to about 0.99, in some embodiments about 0.70 to about 0.99, in some embodiments about 0.80 to about 0.98, and in some embodiments, about 0.85 to about 0.95. For example, the width of capacitor element 120 can be about 2 to about 7 millimeters and the width of interior chamber 126 can be about 3 to about 10 millimeters, and the height of capacitor element 120 can be about 0.5 to about 2 millimeters and the width of interior chamber 126 can be about 0.7 to about 6 millimeters.
[0100] Although it is by no means necessary, the capacitor element can be attached to the housing in such a way that the anode terminal and the cathode terminal are formed outside the housing for subsequent integration into the circuit. The specific configuration (structure) of the terminal may depend on the intended use. In one embodiment, for example, the capacitor assembly can be formed so that it is surface mountable and still mechanically strong. For example, the anode lead can be electrically connected to external, surface mountable anode and cathode terminals (e.g., pads, sheets, plates, frames, etc.). Such terminals can extend through the housing to connect to the capacitor. Generally, the thickness or height of the terminal is selected to minimize the thickness of the capacitor assembly. For example, the thickness of the terminal can be from about 0.05 to about 1 mm, from about 0.05 to about 0.5 mm in some embodiments, and from about 0.1 to about 0.2 mm. If necessary, the surface of the terminal can be plated with nickel, silver, gold, tin, etc., as known in the art, to ensure that the final component can be mounted to the circuit board. In a specific embodiment, the terminal is deposited with nickel and silver thin coatings, respectively, and the mounting surface is also plated with a tin solder layer. In another embodiment, the termination is deposited with an outer metal layer (eg, gold) over a base metal layer (eg, copper alloy) to further improve conductivity.
[0101] In some embodiments, a connection-type member may be used within the interior chamber of the housing to facilitate connection to the terminal in a mechanically stable manner. Figure 1 , the capacitor assembly 100 may include a connecting member 162 formed by a first portion 167 and a second portion 165. The connecting member 162 may be formed of a conductive material similar to the external terminal. The first portion 167 and the second portion 165 may be separate pieces that are integral or connected together, or directly connected or connected through additional conductive elements (e.g., metal). In the illustrated embodiment, the second portion 165 is provided in a plane that is generally parallel to the lateral direction (e.g., -y direction) in which the lead 6 extends. The first portion 167 is "vertical" in the sense that the first portion 167 is provided in a plane that is generally perpendicular to the lateral direction in which the lead 6 extends. In this way, the first portion 167 can limit the movement of the lead 6 in the horizontal direction to enhance surface contact and mechanical stability during use. If desired, an insulating material 7 (e.g., Teflon) may be used around the lead 6. TM washer).
[0102] The first portion 167 may have a mounting region (not shown) connected to the anode lead 6. The region may have a "U-shape" for further enhancing surface contact and mechanical stability of the lead 6. Any of a variety of known techniques may be used to achieve connection of the region to the lead 6, such as welding, laser welding, conductive adhesives, etc. In a specific embodiment, for example, the region is laser welded to the anode lead 6. However, regardless of the technique selected, the first portion 167 may maintain the anode lead 6 in a substantially horizontal alignment to further enhance the dimensional stability of the capacitor assembly 100.
[0103] Still refer to Figure 1 , shows an embodiment of the present invention, wherein the connection type member 162 and the capacitor element 120 are connected to the housing 122 by the anode and cathode terminals 127 and 129, respectively. More specifically, the housing 122 of this embodiment includes an outer wall 123 and two opposite side walls 124, between which a chamber 126 including the capacitor element 120 is formed. The outer wall 123 and the side walls 124 can be formed by one or more layers of metal, plastic or ceramic materials (as described above). In this particular embodiment, the anode terminal 127 contains a first region 127a placed inside the housing 122 and electrically connected to the connection member 162 and a second region 127b placed outside the housing 122 and providing a mounting surface 201. Similarly, the cathode terminal 129 contains a first region 129a placed inside the housing 122 and electrically connected to the solid electrolyte of the capacitor element 120 and a second region 129b placed outside the housing 122 and providing a mounting surface 203. It should be understood that the entire portion of these regions does not need to be placed inside or outside the housing.
[0104] In the illustrated embodiment, a conductive trace 127c extends in the outer wall 123 of the housing to connect the first region 127a and the second region 127b. Similarly, a conductive trace 129c extends in the outer wall 123 of the housing to connect the first region 127a and the second region 127b. The conductive traces and / or regions of the terminal may be separate or integral. In addition to extending through the outer wall of the housing, the traces may also be placed in other locations, such as outside the outer wall. Of course, the present invention is by no means limited to the use of conductive traces for forming a desired terminal.
[0105] Regardless of which particular configuration is used, the terminals 127 and 129 may be connected to the capacitor element 120 using any known technique, such as welding, laser welding, conductive adhesives, etc. In one particular embodiment, for example, the second portion 165 of the connecting member 162 is connected to the anode terminal 127 using a conductive adhesive 131. Similarly, the cathode of the capacitor element 120 is connected to the cathode terminal 129 using a conductive adhesive 133.
[0106] Optionally, a polymeric restraint may also be placed in contact with one or more surfaces of the capacitor element, such as a rear surface, a front surface, an upper surface, a lower surface, a side surface, or any combination thereof. The polymeric restraint may reduce the likelihood of the capacitor element separating from the housing. In this regard, the polymeric restraint may have a degree of strength that allows it to hold the capacitor element in a relatively fixed position even when it is subjected to vibratory forces, but is not so strong that it cracks. For example, the restraint may have a tensile strength of about 1 to about 150 megapascals ("MPa"), in some embodiments about 2 to about 100 MPa, in some embodiments about 10 to about 80 MPa, and in some embodiments, about 20 to about 70 MPa, measured at a temperature of about 25°C. It is generally desired that the restraint be non-conductive. For example, still referring to Figure 1 , shows an embodiment in which a single polymeric delimiter 197 is placed in contact with the upper surface 181 and the rear surface 177 of the capacitor element 120. Although Figure 1In the embodiment, a single limiter is shown, but it should be understood that separate limiters can be used to achieve the same function. In fact, more generally, any number of polymer limiters can be used to contact with any desired surface of capacitor element. When using multiple limiters, it can contact each other or keep physically separated. For example, in one embodiment, the second polymer limiter (not shown) in contact with the upper surface 181 and front surface 179 of capacitor element 120 can be used. The first polymer limiter 197 and the second polymer limiter (not shown) may or may not contact each other. In another embodiment, the polymer limiter can also contact with the lower surface 183 and / or the side surface of capacitor element 120, or combine with other surfaces or replace other surfaces.
[0107] Regardless of how it is applied, it is typically desirable that the polymeric delimiter also be in contact with at least one surface of the housing to help further mechanically stabilize the capacitor element against possible separation. For example, the delimiter may be in contact with the inner surface of one or more side walls, outer walls, lids, etc. For example, in Figure 1 In the embodiment of the present invention, the polymeric limiter 197 is in contact with the inner surface 107 of the side wall 124 and the inner surface 109 of the outer wall 123. When in contact with the shell, it is still desirable that at least a portion of the chamber defined by the shell remains unoccupied to allow inert gas to flow through the chamber and limit the contact of the solid electrolyte with oxygen. For example, typically, at least about 5% of the chamber volume, and in some embodiments, about 10% to about 50% of the chamber volume remains unoccupied by the capacitor element and the polymer limiter.
[0108] Once connected in the desired manner, the resulting package is hermetically sealed as described above. Figure 1 , the housing 122 may also include a cover 125, which is placed on the upper surface of the side wall 124 after the capacitor element 120 and the polymer limiter 197 are placed in the housing 122. The cover 125 can be formed of ceramic, metal (e.g., iron, copper, nickel, cobalt, etc., and alloys thereof), plastic, etc. If necessary, a sealing member 187 can be disposed between the cover 125 and the side wall 124 to help provide a good seal. In one embodiment, for example, the sealing member may include a glass-to-metal seal, Ring (Goodfellow Camridge, Ltd.), etc. The height of the side wall 124 is generally such that the cover 125 does not contact any surface of the capacitor element 120 so that it is not contaminated. The polymeric limiter 197 may or may not contact the cover 125. When placed in the desired position, the cover 125 is hermetically sealed to the side wall 124 using known techniques, such as welding (e.g., resistance welding, laser welding, etc.), soldering, etc. The hermetic seal generally occurs in the presence of an inert gas as described above, so that the resulting assembly is substantially free of reactive gases, such as oxygen or water vapor.
[0109] It should be understood that the described embodiments are exemplary only, and that various other configurations for hermetically sealing capacitor elements within a housing may be used in the present invention. Figure 2 For example, another embodiment of the capacitor assembly 200 shows the use of a housing 222 including an outer wall 123 and a cover 225, wherein a chamber 126 including a capacitor element 120 and a polymeric limiter 197 is formed between the outer wall 123 and the cover 225. The cover 225 includes an outer wall 223 that is integral with at least one side wall 224. For example, in the illustrated embodiment, two opposing side walls 224 are shown in cross-section. The outer walls 223 and 123 both extend in a transverse direction (-y direction) and are generally parallel to each other and to the transverse direction of the anode lead 6. The side wall 224 extends from the outer wall 223 in a longitudinal direction generally perpendicular to the outer wall 123. The distal end 500 of the cover 225 is defined by the outer wall 223 and the proximal end 501 is defined by the flange 253 of the side wall 224.
[0110] The flange 253 extends from the side wall 224 in a lateral direction, which may be generally parallel to the lateral direction of the outer wall 123. The angle between the side wall 224 and the flange 253 may vary, but is typically about 60° to about 120°, in some embodiments, about 70° to about 110°, and in some embodiments, about 80° to about 100° (e.g., about 90°). The flange 253 also defines a peripheral edge 251, which may be generally perpendicular to the lateral direction in which the flange 253 and the outer wall 123 extend. The peripheral edge 251 is located outside the periphery of the side wall 224 and may be generally coplanar with the edge 151 of the outer wall 123. The flange 253 can be sealed to the outer wall 123 using any known technique, such as welding (e.g., resistance or laser), soldering, gluing, etc. For example, in the illustrated embodiment, a sealing member 287 (e.g., a glass-to-metal seal, In any case, the use of the above-mentioned flanges can make the connection between the components more stable and improve the sealing and mechanical stability of the capacitor assembly.
[0111] Other possible housing configurations may also be used in the present invention. For example, Figure 3 shows a similar Figure 2 The present invention relates to a capacitor assembly 300 of a housing structure of the present invention, except that terminal pins 327b and 329b are used as external terminals of the anode and cathode, respectively. More specifically, the terminal pin 327a extends through a trace 327c formed in the outer wall 323 and is connected to the anode lead 6 using a known technique (e.g., welding). An additional section 327a can be used to fix the pin 327b. Similarly, the terminal pin 329b extends through a trace 329c formed in the outer wall 323 and is connected to the cathode by the conductive adhesive 133 as described above.
[0112] Figure 1-3 The embodiments shown in are discussed herein only in terms of a single capacitor element. However, it should also be understood that multiple capacitor elements may be hermetically sealed within the housing. Any of a variety of different techniques may be used to attach multiple capacitor elements to the housing. For example, referring to Figure 4 , a specific embodiment of a capacitor assembly 400 containing two capacitor elements is shown, and will now be described in more detail. More particularly, the capacitor assembly 400 includes a first capacitor element 420a electrically connected to a second capacitor element 420b. In this embodiment, the capacitor elements are aligned so that their main surfaces are in a horizontal configuration. That is, the main surface of the capacitor element 420a defined by its width (-x direction) and length (-y direction) is placed adjacent to the corresponding main surface of the capacitor element 420b. Therefore, the main surface is generally coplanar. Alternatively, the capacitor elements can be arranged so that their main surfaces are not common surfaces, but perpendicular to each other in a certain direction, such as -z direction or -x direction. Of course, the capacitor elements do not need to extend in the same direction.
[0113] Capacitor elements 420a and 420b are placed within a housing 422 having an outer wall 423 and side walls 424 and 425 that together define a chamber 426. Although not shown, a cover can be used that covers the upper surface of the side walls 424 and 425 and seals the assembly 400 as described above. Optionally, a polymeric restraint can also be used to help limit vibration of the capacitor elements. Figure 4In, for example, separate (separate) polymer limiter 497a and 497b are placed adjacent to capacitor elements 420a and 420b respectively and contact with capacitor elements 420a and 420b.Polymer limiter 497a and 497b can be placed in various positions.Further, one of the limiter can be cancelled, or additional limiters can be used.In certain embodiments, for example, it is desirable to use polymer type limiters between capacitor elements to further improve mechanical stability.
[0114] In addition to the capacitor elements, the capacitor assembly also includes an anode terminal electrically connected to the anode lead of each capacitor element and a cathode terminal electrically connected to the cathode of each capacitor element. Figure 4 , showing that the capacitor elements are connected in parallel (in parallel) to a common cathode terminal 429. In this particular embodiment, the cathode terminal 429 is first provided in a plane generally parallel to the bottom surface of the capacitor element and the cathode terminal 429 can be in electrical contact with a conductive trace (not shown). The capacitor assembly 400 also includes connecting members 427 and 527 connected to the anode leads 407a and 407b of the capacitor elements 420a and 420b, respectively. More specifically, the connecting member 427 contains an upright portion 465 and a planar portion 463 connected to the anode terminal (not shown). Similarly, the connecting member 527 contains an upright portion 565 and a planar portion 563 connected to the anode terminal (not shown). Of course, it should be understood that a variety of other types of connecting mechanisms can also be used.
[0115] Regardless of its specific configuration, the resulting capacitor assembly can exhibit a variety of beneficial properties, as shown above. For example, the capacitor can exhibit a relatively high "breakdown voltage" (the voltage at which the capacitor fails), such as about 50 volts or more, in some embodiments about 100 volts or more, in some embodiments about 150 volts or more, and in some embodiments, about 200 volts to about 300 volts. The capacitor can also exhibit a relatively low equivalent series resistance ("ESR"), such as about 200 milliohms, in some embodiments less than about 150 milliohms, and in some embodiments, about 0.1 to about 100 milliohms, measured at an operating frequency of 100 kHz. It is also believed that the loss factor of the capacitor assembly can be maintained at a relatively low level. The loss factor generally refers to the loss that occurs in the capacitor and is usually expressed as a percentage of the ideal capacitor performance. For example, the loss factor of the capacitor of the present invention is typically about 0.5% to about 25%, in some embodiments about 0.8% to about 10%, and in some embodiments, about 1% to about 5%, measured at a frequency of 120 Hz. The capacitor assembly can also be used in high voltage applications, such as at a rated voltage of about 35 volts or more, in some embodiments about 50 volts or more, and in some embodiments, about 60 volts to about 200 volts. The capacitor assembly can also be able to withstand relatively high surge currents, which are common in high voltage applications. The peak surge current can be, for example, about 100 amperes or more, in some embodiments about 200 amperes or more, and in some embodiments, about 300 amperes to about 800 amperes.
[0116] The present invention may be better understood by reference to the following examples.
[0117] Test steps
[0118] Equivalent Series Resistance (ESR)
[0119] The equivalent series resistance may be measured using a Keithley 3330 Precision LCZ meter with Kelvin Leads, 2.2 volt DC bias and a 0.5 volt peak-to-peak sinusoidal signal. The operating frequency may be 100 kHz and the temperature may be 23°C ± 2°C.
[0120] Loss Factor
[0121] The loss factor may be measured using a Keithley 3330 Precision LCZ meter with Kelvin Leads with a 2.2 volt DC bias and a 0.5 volt peak-to-peak sinusoidal signal. The operating frequency may be 120 Hz and the temperature may be 23°C ± 2°C.
[0122] capacitance
[0123] Capacitance can be measured using a Keithley 3330 Precision LCZ meter with Kelvin Leads using a 2.2 volt DC bias and a 0.5 volt peak-to-peak sinusoidal signal. The operating frequency can be 120 Hz and the temperature can be 23°C ± 2°C. In some cases, "wet-to-dry" capacitance can be determined. "Dry capacitance" refers to the capacitance of the component before the solid electrolyte, graphite, and silver layers are applied, while "wet capacitance" refers to the capacitance of the component after dielectric formation, measured in 14% nitric acid with a 10 volt DC bias and a 0.5 volt peak-to-peak sinusoidal signal after electrolyte soaking for 30 seconds with a reference 1 mF tantalum cathode.
[0124] Leakage Current
[0125] The leakage current may be measured using a leakage tester at a temperature of 23° C.±2° C. and at a rated voltage (eg, 16 volts) after a minimum of 60 seconds (eg, 90 seconds, 180 seconds, or 300 seconds).
[0126] Temperature life test
[0127] Temperature life testing can be performed (e.g., 10 components (parts)) at a temperature of 125°C with different voltages (e.g., 0 volts, 20 volts, or 35 volts). The recovery time after the test condition can be 30 minutes. Capacitance and ESR can be measured after the recovery time.
[0128] Temperature pulse test
[0129] Temperature pulse testing can be performed at 125°C with different voltages (e.g., 25 components (parts)). Resistance can be 33 ohms and 30 seconds of charge / discharge. Capacitance and ESR can be measured at 1000, 2000, and 3000 hours after recovery time.
[0130] Example 1
[0131] Anode samples were formed using 40,000 μFV / g tantalum powder. Each anode sample was embedded with tantalum wire, sintered at 1410°C, and pressed to 5.8 g / cm 3 The resulting pellets were 5.20 x 3.70 x 0.65 mm in size. The pellets were anodized to 49.0 volts at 85°C in a water / phosphoric acid electrolyte with a conductivity of 8.6 mS to form a dielectric layer. The pellets were anodized again to 130 volts for 25 seconds at 30°C in water / boric acid / disodium tetraborate with a conductivity of 2.0 mS to form a thicker oxide layer accumulated on the outside.
[0132] The anode was then immersed directly without pre-coating into a dispersed poly(3,4-ethylenedioxythiophene) (Clevios TM K, Heraeus) to form a conductive polymer coating. After coating, the parts were dried at 125°C for 20 minutes. This process was repeated 10 times. Subsequently, the parts were immersed in a dispersed poly(3,4-ethylenedioxythiophene) (Clevios) with a solid content of 2.0% and a viscosity of 20 mPa.s. TM K, Heraeus). After coating, the parts were dried at 125°C for 20 minutes. This process was repeated 3 times. Subsequently, the parts were immersed in a dispersed poly(3,4-ethylenedioxythiophene) (Clevios TM K, Heraeus). After coating, the component was dried at 125°C for 20 minutes. The process was repeated 8 times. The component was then immersed in a graphite dispersion and dried. Finally, the component was immersed in a silver dispersion and dried. In this way, multiple components (250) of 47μF / 20V capacitors were manufactured and encapsulated in silica resin.
[0133] Example 2
[0134] Capacitors were formed in the manner described in Example 1 except that three pre-coatings of an organometallic compound containing a solution of tris(3-trimethoxysilylpropyl)isocyanurate in acetone (1.0%) were used. Multiple 47 μF / 20V capacitor components (250) were formed and encapsulated in silica resin.
[0135] Example 3
[0136] Capacitors were formed in the manner described in Example 2, except that three pre-coatings of an organometallic compound containing a solution of tris(3-trimethoxysilylpropyl)isocyanurate in acetone (1.0%) were used. Each pre-coating was then reacted with a solution of PEG1000 in acetone (1.0%). Multiple 47μF / 20V capacitor components (250) were formed and encapsulated in a silica resin. The electrical properties of the finished capacitors of Examples 1-3 were then tested. The median results for capacitance (CAP), "wet-to-dry" capacitance (W / D), loss factor (Df), ESR, and leakage current (DCL) are listed in Table 1 below.
[0137] Prior to being encapsulated in silica resin, components (10) of multiple 47μF / 20V capacitors were dried at 150°C for 4 hours and the resulting assembly was completed by placing in a ceramic case purged with nitrogen and hermetically sealed by seam welding. The median results of CAP and leakage current in a 125°C life test at 1.25x rated voltage for components in hermetic packaging are listed in Table 2 below. The median results of ESR and capacitance and leakage current in a 125°C pulse test at rated voltage for components in hermetic packaging are listed in Table 3 below.
[0138] Table 1: Electrical properties
[0139]
[0140]
[0141] Table 2: 125° life test results
[0142]
[0143] Table 3: 125℃ pulse test results
[0144]
[0145]
[0146] Without departing from the spirit and scope of the present invention, those of ordinary skill in the art may implement these and other modifications and variations of the present invention. In addition, it should be understood that the aspects of the various embodiments may be interchangeable in whole or in part. In addition, those of ordinary skill in the art will appreciate that the foregoing description is merely exemplary and is not intended to limit the present invention further described in these appended claims.
Claims
1. A capacitor assembly comprising a capacitor element, the capacitor element comprising: a porous anode body containing a valve metal compound; a dielectric overlying the anode body and comprising an oxide of a valve metal compound; a solid electrolyte overlying the dielectric, wherein the solid electrolyte comprises a conductive polymer and a hydroxyl-functional polymer; and an organofunctional silane compound that bonds to the oxide of the dielectric and is capable of bonding to the hydroxy-functional polymer; The organofunctional silane compound has the following general formula (I): in, R1, R2 and R3 are independently alkyl, alkenyl, aryl, heteroaryl, cycloalkyl, heterocyclyl, halogen, haloalkyl, hydroxyalkyl or a combination thereof; and X is a functional group capable of bonding to a hydroxyl group or capable of being converted into a functional group capable of bonding to a hydroxyl group; and Z is an organic group that connects the functional group X to the silicon atom, applying an outer polymer coating overlying the solid electrolyte, wherein the ratio of the average size of the particles used in the outer polymer coating to the average size of the particles used in any dispersion of the solid electrolyte is from 1.5 to 30, wherein X is a protecting group that can be converted into a functional group that can react with the hydroxy-functional polymer, The protecting group includes a thiocyanate group, a carbamate group, an isocyanurate group, or a combination thereof.
2. The capacitor assembly of claim 1, wherein at least one of R1, R2 and R3 is a hydroxyalkyl group.
3. The capacitor assembly of claim 1, wherein Z is an alkyl group, an aryl group, or a combination thereof.
4. The capacitor assembly of claim 1 wherein X is an isocyanate.
5. The capacitor assembly of claim 4, wherein the organosilane compound comprises 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropylmethyldiethoxysilane, 3-isocyanatopropylmethyldiethoxysilane, or a combination thereof.
6. The capacitor assembly of claim 1, wherein the organosilane compound comprises (thiocyanatemethyl)phenethyl-trimethoxysilane, 3-thiocyanatepropyltriethoxysilane, N-(3-triethoxysilylpropyl)-o-tert-butylcarbamate, triethoxysilylpropylethylcarbamate, N-trimethoxysilylpropylmethylcarbamate, tris(3-trimethoxysilylpropyl)isocyanurate, or a combination thereof.
7. The capacitor assembly of claim 1 wherein the anode body comprises tantalum and the dielectric comprises tantalum pentoxide.
8. The capacitor assembly of claim 1 wherein the solid electrolyte comprises an extrinsic conductive polymer and sulfonyl counterions.
9. The capacitor assembly of claim 8, wherein the extrinsic conductive polymer is poly(3,4-ethylenedioxythiophene).
10. The capacitor assembly of claim 9 wherein the sulfonyl counterion is polystyrene sulfonic acid or a salt thereof.
11. The capacitor assembly of claim 1 wherein the conductive polymer is an intrinsically conductive polymer.
12. The capacitor assembly of claim 11, wherein the intrinsically conductive polymer is poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dihydrothieno- In-2-ylmethoxy)-1-butane-sulfonic acid, salt), poly (4-(2,3-dihydrothieno-[3,4-b][l,4]di ((2-((((((((((((((((((((((((- ...
13. The capacitor assembly of claim 1 wherein the solid electrolyte comprises a layer formed from a dispersion of prepolymerized conductive polymer particles.
14. The capacitor assembly of claim 13 wherein a hydroxyl functional polymer is contained within said layer.
15. The capacitor assembly of claim 1 wherein the hydroxy-functional polymer has a molecular weight of 300 to 1,200 grams per mole.
16. The capacitor assembly of claim 1 wherein the hydroxy-functional polymer is a polyalkylene ether.
17. The capacitor assembly of claim 16 wherein the polyalkylene ether is a polyalkylene glycol.
18. The capacitor assembly of claim 1 further comprising an outer polymer coating overlying the solid electrolyte and comprising prepolymerized conductive polymer particles and a crosslinking agent.
19. The capacitor assembly of claim 1, further comprising: an anode terminal electrically connected to the anode body; a cathode terminal electrically connected to the solid electrolyte; and A housing encloses the capacitor element and exposes at least a portion of the anode termination and the cathode termination.
20. The capacitor assembly of claim 19, wherein the housing is formed of a resinous material encapsulating the capacitor element.
21. The capacitor assembly of claim 19, wherein the housing defines an interior chamber in which the capacitor element is positioned, wherein the interior chamber has a gaseous atmosphere including an inert gas.
22. A method of forming a capacitor element as defined in any one of claims 1 to 21, the method comprising: anodizing the sintered porous anode body to form a dielectric including an oxide of a valve metal compound; applying a solution including an organofunctional silane compound to the anode; applying a dispersion containing conductive polymer particles and a hydroxy-functional polymer to form a conductive polymer layer; and The organofunctional silane compound is bonded to the oxide of the dielectric.
23. The method of claim 22, wherein the solution comprises an organic solvent.