Acrylic acid copolymer and cross-linked products thereof
By synthesizing a composition of specific structural units and crosslinkable monomers in an acrylic copolymer, the problem of insufficient heat resistance at high temperatures in the prior art is solved, and an excellent heat resistance and processability are prepared. Crosslinked substance, suitable for automotive rubber materials.
Patent Information
- Application Number
- CN201780070388.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-11-30
- Filing Date
- 2017-11-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2037-11-22
AI Technical Summary
The existing acrylic rubber materials lack heat resistance at high temperatures, especially under long-term high temperature conditions, and their tension elongation and hardness vary greatly, making it difficult to meet the high-temperature heat resistance requirements of automotive rubber components.
Compositions containing specific alkyl acrylates, alkoxy acrylates, alkyl methacrylates and crosslinking monomers are synthesized in an acrylic copolymer and prepared by emulsion polymerization to form excellent heat resistance and Processable crosslinking.
It realizes acrylic copolymer crosslinker with small elongation change rate and hardness change rate and excellent heat resistance under long-term high temperature conditions, and is suitable for automotive rubber materials such as fuel hoses and air hoses.
Smart Images

Figure GDA0003059929540000211
Abstract
Description
Technical Field
[0001] The present invention relates to an acrylic copolymer and a cross-linked product thereof. Hereinafter, a material composed of the cross-linked product may be referred to as a "rubber material" or a "cross-linked rubber material". Background Art
[0002] Generally, acrylic polymers are polymers containing acrylic ester as a main raw material and are known as materials having excellent physical properties related to durability. They are widely used as industrial rubber materials such as engine gaskets, oil hoses, air hoses, O-rings, and rubber materials for automobiles.
[0003] However, for such automotive rubber components, especially rubber components used in engine compartments, the performance of superchargers (turbochargers) accompanying higher engine output and the tightening of exhaust gas regulations in recent years require further improvement in heat resistance, for example, the degradation of physical properties is required to be small even under high temperature conditions for a long period of time, and in particular, the change rate of elongation at break is required to be small.
[0004] In view of such a situation, as a method for improving heat resistance, Patent Document 1 discloses an acrylic rubber composition obtained by simultaneously blending a condensed heterocyclic compound as an antioxidant and a crosslinking agent in specific amounts into an acrylic rubber.
[0005] However, rubber parts used in automobile-related fields and the like are required to have even higher long-term heat resistance at high temperatures, and a rubber material having heat resistance at even higher temperatures is desired.
[0006] In addition, Patent Document 2 discloses an acrylic rubber characterized in that it is obtained by copolymerizing 10 to 100 parts by weight of an alkyl methacrylate and 0.5 to 4 parts by weight of a crosslinking monomer with respect to 100 parts by weight of an acrylic ester, and as specific examples of the combination of the alkyl methacrylate and the crosslinking monomer, a combination of methyl methacrylate and glycidyl methacrylate, a combination of n-butyl methacrylate and glycidyl methacrylate, etc. are disclosed. Moreover, it is believed that such an acrylic rubber has a small change rate in elongation at break before and after heat aging, and it is disclosed that among the specific combinations, a combination of methyl methacrylate and glycidyl methacrylate has the best heat aging resistance. However, even so, a rubber material is still sought that has a significantly reduced elongation at break after undergoing a heat history and is more excellent in heat resistance.
[0007] In addition, Patent Document 3 discloses a crosslinked product obtained by crosslinking an acrylic elastomer composition containing an acrylic elastomer obtained by copolymerizing an acrylic ester and a crosslinking point monomer, wherein the molar fractions of oxygen atoms and nitrogen atoms in the acrylic elastomer are set to a certain value or less, and the volume change when the acrylic elastomer is immersed in distilled water under certain conditions is specified. However, the heat resistance of the crosslinked product obtained in this manner has not been evaluated.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application No. 2011-551930
[0011] Patent Document 2: International Publication No. 2009 / 099113
[0012] Patent Document 3: International Publication No. 2016 / 136697 Summary of the invention
[0013] Technical Problems to be Solved by the Invention
[0014] An object of the present invention is to provide a cross-linked product of an acrylic copolymer for providing a rubber material, wherein the cross-linked product has a small change rate of elongation and hardness even under high temperature conditions for a long period of time and has excellent heat resistance, an acrylic copolymer used therefor, and a composition containing the acrylic copolymer.
[0015] Technical means to solve technical problems
[0016] The inventors of the present application have conducted various studies and, as a result, have found that the object can be achieved by an acrylic copolymer containing a structural unit derived from an acrylic ester having an alkyl group having 1 to 8 carbon atoms and / or a structural unit derived from an acrylic ester having an alkoxyalkyl group having 2 to 8 carbon atoms, a structural unit derived from an alkyl methacrylate having an alkyl group having 3 to 16 carbon atoms, and a structural unit derived from a crosslinkable monomer having a carboxyl group, a composition containing the acrylic copolymer and a crosslinking agent, and a crosslinked product obtained by crosslinking the composition, thereby completing the present invention.
[0017] The embodiments of the present invention are as follows.
[0018] Item 1. An acrylic copolymer comprising: 45 to 89.5% by weight of structural units derived from an acrylic acid ester having an alkyl group having 1 to 8 carbon atoms and / or structural units derived from an acrylic acid ester having an alkoxyalkyl group having 2 to 8 carbon atoms (A), 10 to 50% by weight of structural units derived from an alkyl methacrylate having an alkyl group having 3 to 16 carbon atoms (B), and 0.5 to 5% by weight of structural units derived from a cross-linking monomer having a carboxyl group (C).
[0019] Item 2. The acrylic copolymer according to Item 1, wherein the structural unit (A) is a structural unit derived from an acrylic acid ester having an alkyl group having 1 to 8 carbon atoms.
[0020] Item 3. The acrylic copolymer according to Item 1 or 2, wherein the structural unit (A) comprises both a structural unit (A1) derived from an acrylic acid ester having an alkyl group having 1 to 3 carbon atoms and a structural unit (A2) derived from an acrylic acid ester having an alkyl group having 4 to 8 carbon atoms.
[0021] Item 4. The acrylic copolymer according to Item 3, wherein a weight ratio of the structural unit (A1) to the structural unit (A2) (A1):(A2) is 10:90 to 90:10.
[0022] Item 5. The acrylic copolymer according to Item 3, wherein a weight ratio of the structural unit (A1) to the structural unit (A2) (A1):(A2) is 30:70 to 70:30.
[0023] Item 6. The acrylic copolymer according to any one of Items 1 to 5, wherein the alkyl group of the structural unit (B) has 4 to 9 carbon atoms.
[0024] Item 7. The acrylic copolymer according to any one of Items 1 to 6, wherein the crosslinkable monomer of the structural unit (C) is an ethylenically unsaturated dicarboxylic acid monoester.
[0025] Item 8. The acrylic copolymer according to any one of Items 1 to 7, which has a Mooney viscosity (ML 1+4 ) is 10 to 100.
[0026] Item 9. An acrylic copolymer-containing composition, comprising the acrylic copolymer according to any one of Items 1 to 8 and a crosslinking agent.
[0027] Item 10. The acrylic copolymer-containing composition according to Item 9, which has a Mooney scorch time t5 of 1 to 10 minutes at a temperature of 125° C. when it is made into an uncrosslinked sheet having a thickness of about 2 to 2.5 mm.
[0028] Item 11. A cross-linked product prepared using the acrylic copolymer-containing composition according to Item 9 or 10.
[0029] Item 12. The cross-linked product according to Item 11, which exhibits at least one of the following properties (i) and (ii):
[0030] (i) Elongation at break EB is 100-400%;
[0031] (ii) Type A Durometer hardness Hs is 30 to 100.
[0032] Item 13. The cross-linked product according to Item 11 or 12, wherein the change rate (%) of the elongation at break EB before and after heating at 190° C. for 336 hours is -48 or more.
[0033] Item 14. The cross-linked product according to any one of Items 11 to 13, wherein the cross-linked product has a type A durometer hardness Hs after heating at 190° C. for 336 hours and has a change within ±20 relative to the type A durometer hardness Hs before heating.
[0034] Effects of the Invention
[0035] The composition containing the acrylic copolymer of the present invention has excellent processability, and the cross-linked product prepared using the composition containing the acrylic copolymer of the present invention (specifically, cross-linked) has excellent normal physical properties and heat resistance under long-term high temperature without impairing cold resistance, and is therefore suitable as a rubber material for automobiles such as fuel hoses, air hoses, and pipe materials. DETAILED DESCRIPTION
[0036] First, the acrylic copolymer of the present invention will be described.
[0037] The acrylic copolymer of the present invention contains 45 to 89.5% by weight of a structural unit derived from an acrylic acid ester having an alkyl group with 1 to 8 carbon atoms and / or a structural unit (A) derived from an acrylic acid ester having an alkoxyalkyl group with 2 to 8 carbon atoms, 10 to 50% by weight of a structural unit (B) derived from an alkyl methacrylate with 3 to 16 carbon atoms, and 0.5 to 5% by weight of a structural unit (C) derived from a crosslinkable monomer having a carboxyl group. In addition, the proportion of each of the structural units is preferably a proportion when the entire acrylic copolymer is set to 100% by weight, and the acrylic copolymer may also contain structural units other than the structural unit (A), the structural unit (B) and the structural unit (C). In the acrylic copolymer, the total of the structural unit (A), the structural unit (B) and the structural unit (C) is, for example, 55.5% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, particularly preferably 90% by weight or more, and may also be 100% by weight.
[0038] Acrylic acid esters having an alkyl group having 1 to 8 carbon atoms are alkyl acrylates, and the carbon number of the alkyl group is preferably 1 to 8. Acrylic acid esters having an alkoxyalkyl group having 2 to 8 carbon atoms are alkoxyalkyl acrylates, and the carbon number of the alkoxyalkyl group is preferably 2 to 8.
[0039] Among the structural units (A) derived from an acrylate having an alkyl group having 1 to 8 carbon atoms and / or the structural units (A) derived from an acrylate having an alkoxyalkyl group having 2 to 8 carbon atoms, the structural units (A) derived from an acrylate having an alkyl group having 1 to 8 carbon atoms are preferred. The structural unit (A) may be a structural unit derived from one type of acrylate, or may be a structural unit derived from two or more types of acrylates.
[0040] Specific examples of the structural unit derived from an acrylic acid ester having an alkyl group having 1 to 8 carbon atoms include structural units derived from acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, and cyclohexyl acrylate, and structural units derived from ethyl acrylate and n-butyl acrylate are preferred.
[0041] Specific examples of the structural unit derived from an acrylate having an alkoxyalkyl group having 2 to 8 carbon atoms include structural units derived from acrylates such as methoxymethyl acrylate, methoxyethyl acrylate, ethoxymethyl acrylate, 2-ethoxyethyl acrylate, 2-propoxyethyl acrylate, 2-butoxyethyl acrylate, 2-methoxypropyl acrylate, 2-ethoxypropyl acrylate, 3-methoxypropyl acrylate, 3-ethoxypropyl acrylate, 4-methoxybutyl acrylate, and 4-ethoxybutyl acrylate, and preferred are structural units derived from methoxyethyl acrylate.
[0042] The content of the structural unit derived from an acrylic acid ester having an alkyl group having 1 to 8 carbon atoms and / or the structural unit (A) derived from an acrylic acid ester having an alkoxyalkyl group having 2 to 8 carbon atoms in the acrylic acid copolymer of the present invention is 45 to 89.5% by weight, preferably 50 to 89.5% by weight, and more preferably 60 to 89.5% by weight of the total structural units of the acrylic acid copolymer. The structural unit (A) being within the above range is preferred in terms of cold resistance or oil resistance.
[0043] In the acrylic copolymer of the present invention, the structural units (A) derived from an acrylic acid ester having an alkyl group having 1 to 8 carbon atoms and / or the structural units (A) derived from an acrylic acid ester having an alkoxyalkyl group having 2 to 8 carbon atoms preferably contain both structural units (A1) derived from an acrylic acid ester having an alkyl group having 1 to 3 carbon atoms and structural units (A2) derived from an acrylic acid ester having an alkyl group having 4 to 8 carbon atoms. The weight ratio of the structural units (A1) to the structural units (A2) is preferably 10 to 90:90 to 10 (i.e., (A1):(A2)=10:90 to 90:10), more preferably 20 to 80:80 to 20 (20:80 to 80:20). Further preferably, it is 30:70 to 70:30, and most preferably, it is 40:60 to 60:40.
[0044] The alkyl methacrylate having an alkyl group having 3 to 16 carbon atoms (preferably 4 to 16 carbon atoms) means that the alkyl group of the alkyl methacrylate has 3 to 16 carbon atoms (preferably 4 to 16 carbon atoms). Examples of the structural unit (B) derived from the alkyl methacrylate include structural units derived from alkyl methacrylates such as n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, n-decyl methacrylate, isodecyl methacrylate, n-dodecyl methacrylate, n-lauryl methacrylate, and n-octadecyl methacrylate, and preferably structural units derived from alkyl methacrylates selected from n-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, isodecyl methacrylate, and n-lauryl methacrylate. More preferably, the structural unit (B) is derived from an alkyl methacrylate having an alkyl group with 4 to 9 carbon atoms (more preferably 8 to 9 carbon atoms, further preferably 7 to 9 carbon atoms, and particularly preferably 6 to 6 carbon atoms), for example, more preferably a structural unit derived from n-butyl methacrylate, n-hexyl methacrylate, or 2-ethylhexyl methacrylate. It may be a structural unit derived from one alkyl methacrylate, or may be a structural unit derived from two or more alkyl methacrylates.
[0045] The content of the structural unit (B) derived from the alkyl methacrylate having 3 to 16 carbon atoms in the acrylic copolymer of the present invention is 10 to 50% by weight, preferably 10 to 40% by weight, and more preferably 10 to 30% by weight of the total structural units of the acrylic copolymer. In addition, 10 to 48% by weight, 10 to 38% by weight, etc. are also preferred. When the structural unit (B) is within the above range, it is preferred in terms of heat resistance, oil resistance, and cold resistance.
[0046] As the structural unit (C) derived from a cross-linkable monomer having a carboxyl group, a structural unit having a structural unit derived from a cross-linkable monomer having a carboxyl group is preferred.
[0047] Examples of the structural unit derived from a cross-linking monomer having a carboxyl group include structural units derived from ethylenically unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, 2-pentenoic acid, and cinnamic acid; structural units derived from ethylenically unsaturated dicarboxylic acids such as fumaric acid, maleic acid, and itaconic acid; structural units derived from monoalkyl fumarate such as monomethyl fumarate, monoethyl fumarate, monopropyl fumarate, monobutyl fumarate, monohexyl fumarate, and monooctyl fumarate; monoalkyl maleate such as monomethyl maleate, monoethyl maleate, monopropyl maleate, monobutyl maleate, monopentyl maleate, and monodecyl maleate; and monoalkyl maleate such as monomethyl itaconate, monoethyl itaconate, monopropyl itaconate, and monobutyl itaconate. As the structural unit derived from the crosslinkable monomer having a carboxyl group, an ethylenically unsaturated dicarboxylic acid monoester is preferred, a fumaric acid monoalkyl ester is more preferred, and a fumaric acid monoalkyl ester having an alkyl group with 1 to 4 carbon atoms is most preferred.
[0048] The content of the structural unit (C) derived from the crosslinkable monomer having a carboxyl group in the acrylic copolymer of the present invention is 0.5 to 5% by weight, preferably 0.5 to 2% by weight of the total structural units. The structural unit (C) derived from the crosslinkable monomer having a carboxyl group is preferably within the above range in terms of physical properties such as strength and compression set and processability.
[0049] Furthermore, the acrylic copolymer of the present invention may contain structural units derived from other monomers copolymerizable with the structural units (A) to (C) in addition to the structural units (A) to (C). Examples of the other structural units include structural units derived from ethylenically unsaturated nitrile, structural units derived from (meth)acrylamide monomers, structural units derived from aromatic vinyl monomers, structural units derived from conjugated diene monomers, structural units derived from non-conjugated dienes, and structural units derived from other olefins.
[0050] Examples of the structural unit derived from an ethylenically unsaturated nitrile include structural units derived from compounds such as acrylonitrile, methacrylonitrile, α-methoxyacrylonitrile, and vinylidene cyanide.
[0051] Examples of the structural unit derived from a (meth)acrylamide monomer include structural units derived from compounds such as acrylamide, methacrylamide, diacetone acrylamide, diacetone methacrylamide, N-butoxymethyl acrylamide, N-butoxymethyl methacrylamide, N-butoxyethyl acrylamide, N-butoxyethyl methacrylamide, N-methoxymethyl acrylamide, N-methoxymethyl methacrylamide, N-propoxymethyl acrylamide, N-propoxymethyl methacrylamide, N-methyl acrylamide, N-methyl methacrylamide, N,N-dimethyl acrylamide, N,N-dimethyl methacrylamide, N,N-diethyl acrylamide, N,N-diethyl methacrylamide, N-hydroxymethyl acrylamide, N-hydroxymethyl methacrylamide, ethyl acrylamide, crotonamide, cinnamamide, maleic acid diamide, itaconamide, methyl maleic acid amide, methyl itaconamide, maleimide, and itaconimide.
[0052] Examples of the structural unit derived from an aromatic vinyl monomer include structural units derived from compounds such as styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, o-ethylstyrene, p-ethylstyrene, α-fluorostyrene, p-trifluoromethylstyrene, p-methoxystyrene, p-aminostyrene, p-dimethylaminostyrene, p-acetoxystyrene, styrenesulfonic acid or its salts, α-vinylnaphthalene, 1-vinylnaphthalene-4-sulfonic acid or its salts, 2-vinylfluorene, 2-vinylpyridine, 4-vinylpyridine, divinylbenzene, diisopropenylbenzene, and vinylbenzyl chloride.
[0053] Examples of the structural unit derived from the conjugated diene monomer include structural units derived from compounds such as 1,3-butadiene, 2-methyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,2-dichloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-neopentyl-1,3-butadiene, 2-bromo-1,3-butadiene, 2-cyano-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, chloroprene, and piperylene.
[0054] Examples of the structural unit derived from non-conjugated dienes include structural units derived from non-conjugated diene compounds such as 1,4-pentadiene, 1,4-hexadiene, ethylidene norbornene, norbornadiene, and dicyclopentadiene.
[0055] Examples of the structural units derived from other olefin monomers include structural units derived from esters such as dicyclopentadienyl acrylate, dicyclopentadienyl methacrylate, dicyclopentadienyl ethyl acrylate, and dicyclopentadienyl ethyl methacrylate, and compounds such as ethylene, propylene, vinyl chloride, vinylidene chloride, 1,2-dichloroethylene, vinyl acetate, vinyl fluoride, vinylidene fluoride, 1,2-dichloroethylene, vinyl bromide, vinylidene bromide, 1,2-dibromide, ethyl vinyl ether, and butyl vinyl ether.
[0056] When the acrylic copolymer of the present invention contains structural units derived from other copolymerizable monomers, the content of the structural units is 0 to 45% by weight, preferably 0 to 20% by weight, based on all the structural units.
[0057] In the acrylic copolymer of the present invention, the content of the structural unit can be determined by nuclear magnetic resonance spectrum of the obtained polymer.
[0058] <Method for preparing acrylic acid copolymer>
[0059] The acrylic copolymer used in the present invention can be obtained by polymerizing various monomers. The monomers used may be commercially available products and are not particularly limited.
[0060] As the form of the polymerization reaction, any of emulsion polymerization, suspension polymerization, bulk polymerization and solution polymerization can be used, but from the perspective of ease of control of the polymerization reaction, emulsion polymerization under normal pressure, which is commonly used as a method for preparing acrylic copolymers known in the past, is preferred.
[0061] When the polymerization is carried out by emulsion polymerization, a common method may be used, and conventionally known agents such as a polymerization initiator, an emulsifier, a chain transfer agent, and a polymerization terminator may be used.
[0062] The emulsifier used in the present invention is not particularly limited, and nonionic emulsifiers and anionic emulsifiers commonly used in emulsion polymerization can be used. As nonionic emulsifiers, for example, polyoxyethylene alkyl ethers, polyoxyethylene alcohol ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, polyoxyethylene fatty acid esters, and polyoxyethylene sorbitan anhydride fatty acid esters can be listed. As anionic emulsifiers, alkylbenzene sulfonates, alkyl sulfate ester salts, polyoxyethylene alkyl ether sulfate ester salts, polyoxyalkylene alkyl ether phosphates or their salts, fatty acid salts, etc. can be listed. These emulsifiers can be used alone or in combination. As anionic emulsifiers, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and triethanolamine dodecyl sulfate can also be used.
[0063] The amount of the emulsifier used in the present invention is the amount commonly used in the emulsion polymerization method. Specifically, it is in the range of 0.01 to 10% by weight, preferably 0.03 to 7% by weight, and more preferably 0.05 to 5% by weight relative to the amount of the added monomer. When a reactive surfactant is used as a monomer component, it is not necessary to add an emulsifier.
[0064] The polymerization initiator used in the present invention is not particularly limited, and a polymerization initiator commonly used in the emulsion polymerization method can be used. As specific examples thereof, there can be listed inorganic peroxide-based polymerization initiators represented by persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate, 2,2-bis(4,4-di-(tert-butylperoxy)cyclohexyl)propane, 1-di-(tert-hexylperoxy)cyclohexane, 1,1-di-(tert-butylperoxy)cyclohexane, 4,4-di-(tert-butylperoxy)butyl valerate, 2,2-di(tert-butylperoxy)butane, tert-butyl hydroperoxide, isopropylbenzene hydroperoxide, diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, tert-butyl isopropylbenzene peroxide, di-tert-butyl peroxide, di-tert-hexyl peroxide, bis(2-tert-butylperoxy)butyl isopropyl) benzene, diisopropyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide, dibenzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl (3-methylbenzoyl) peroxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, isopropyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoyl peroxy)hexane, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxylaurate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoyl peroxy)hexane, tert-butyl peroxyacetate, tert-hexyl peroxybenzoate, tert-butyl peroxybenzoate, 2,5-dimethyl-2,5-bis(tert-butyl peroxy)hexane and other organic peroxides azobis(2-(2-imidazolin-2-yl)propane), 2,2'-azobis(propane-2-guanidine), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamide], 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2,2'-azobis(1-imino-1-pyrrolidinyl-2-methylpropane), and 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}.These polymerization initiators may be used alone or in combination of two or more.
[0065] The amount of the polymerization initiator used in the present invention may be an amount commonly used in emulsion polymerization, specifically, in the range of 0.01 to 5 wt %, preferably 0.01 to 4 wt %, and more preferably 0.02 to 3 wt % relative to the amount of the added monomer.
[0066] In addition, organic peroxides and inorganic peroxides as polymerization initiators can be used as redox polymerization initiators by combining with reducing agents. The reducing agents used in combination are not particularly limited, and examples thereof include compounds containing metal ions in a reduced state such as ferrous sulfate and cuprous naphthenate, methane compounds such as sodium methanesulfonate, amine compounds such as dimethylaniline, ascorbic acid and its salts, alkali metal salts of sulfurous acid and thiosulfate, and other reducing inorganic salts. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 0.0003 to 10.0 parts by weight relative to 100 parts by weight of the added monomer.
[0067] The chain transfer agent can be used as needed. Specific examples of the chain transfer agent include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, tert-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, and n-octadecanethiol, xanthate compounds such as 2,4-diphenyl-4-methyl-1-pentene, 2,4-diphenyl-4-methyl-2-pentene, dimethyl xanthate disulfide, and diisopropyl xanthate disulfide, terpinolene, tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetramethylthiuram monosulfide. The chain transfer agents include phenolic compounds such as 2,6-di-tert-butyl-4-methylphenol and styrenated phenol, allyl compounds such as allyl alcohol, halogenated hydrocarbon compounds such as dichloromethane, dibromomethane and carbon tetrabromide, vinyl ethers such as α-benzyloxystyrene, α-benzyloxyacrylonitrile and α-benzyloxyacrylamide, triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, thiomalic acid, 2-ethylhexylthioglycolate, etc. These chain transfer agents can be used alone or in combination. The amount of these chain transfer agents is not particularly limited, but is usually 0 to 5 parts by weight relative to 100 parts by weight of the added monomer.
[0068] Examples of the polymerization terminator include hydroxylamine, hydroxylamine sulfate, diethylhydroxylamine, hydroxylamine sulfonic acid and its alkali metal salts, sodium dimethyldithiocarbamate, and quinone compounds such as hydroquinone. The amount of the polymerization terminator used is not particularly limited, but is generally 0 to 2 parts by weight relative to 100 parts by weight of all monomers.
[0069] Furthermore, the polymer obtained by the above method can be adjusted to pH by using a base as a pH adjuster as needed. Specific examples of the base include sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonia, inorganic ammonium compounds, organic amine compounds, etc. The pH range is pH 1 to 11, preferably pH 1.5 to 10.5, and more preferably pH 2 to 10.
[0070] In addition to the above substances, polymerization auxiliary materials such as a particle size regulator, a chelating agent, and an oxygen scavenger may be used as necessary.
[0071] Emulsion polymerization can be any of batch, semi-batch, and continuous. The polymerization time and polymerization temperature are not particularly limited. They can be appropriately selected according to the type of polymerization initiator used, but generally the polymerization temperature is 10 to 100° C. and the polymerization time is 0.5 to 100 hours.
[0072] The method for recovering the polymer obtained by the above method is not particularly limited, and a commonly used method can be used. As an example of this method, a method of continuously or batch-feeding a polymer solution into an aqueous solution containing a coagulant can be cited, and a coagulated slurry can be obtained by this operation. At this time, since the temperature of the aqueous solution containing a coagulant is affected by the type and amount of the monomer used, the shear force caused by stirring, etc., it cannot be generally specified, but is usually above 50°C, preferably in the range of 60°C to 100°C.
[0073] The coagulant that can be used for this purpose is not particularly limited, but an inorganic metal salt is preferred, and specific examples thereof include sodium sulfate, magnesium sulfate, aluminum sulfate, sodium chloride, and calcium chloride.
[0074] In order to remove the coagulant, it is preferred to wash the coagulated slurry obtained by the above method with water. If water washing is not performed at all or the washing is insufficient, there is a possibility that ion residues from the coagulant will precipitate during the molding process.
[0075] The acrylic copolymer can be obtained by removing water from the coagulated slurry after washing and drying. The drying method is not particularly limited, but it is usually dried using a flash dryer or a fluidized dryer. In addition, a dehydration step using a centrifuge or the like may also be performed before the drying step.
[0076] From the viewpoint of processability, the Mooney viscosity (ML) at 100°C in the Mooney scorch test specified in JIS K 6300 is used. 1+4 ) represents that the molecular weight range of the acrylic copolymer used in the present invention prepared in the above manner is preferably 10 to 100, more preferably 15 to 90, and further preferably 20 to 80.
[0077] <Composition containing acrylic copolymer>
[0078] The acrylic copolymer-containing composition of the present invention contains at least the above-mentioned acrylic copolymer and a cross-linking agent.
[0079] As the crosslinking agent, conventionally known crosslinking agents generally used for crosslinking of rubbers such as polyamine compounds, polyvalent epoxy compounds, polyvalent isocyanate compounds, aziridine compounds, sulfides, basic metal oxides and organic metal halides can be used. Among these crosslinking agents, polyamine compounds are preferably used.
[0080] Examples of the polyamine compound include aliphatic polyamine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-biscinnamaldehyde-1,6-hexanediamine; and aromatic polyamine compounds such as 4,4'-methylenedianiline, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)diphenylamine, 4,4'-(p-phenylenediisopropylidene)diphenylamine, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, 1,3,5-phenyltriamine, 1,3,5-phenyltriaminomethyl ester, and isophthalic acid dihydrazide.
[0081] Examples of the polyvalent epoxy compound include glycidyl ether epoxy compounds such as phenol novolac epoxy compounds, cresol novolac epoxy compounds, cresol epoxy compounds, bisphenol A epoxy compounds, bisphenol F epoxy compounds, brominated bisphenol A epoxy compounds, brominated bisphenol F epoxy compounds, and hydrogenated bisphenol A epoxy compounds; and other polyvalent epoxy compounds such as alicyclic epoxy compounds, glycidyl ester epoxy compounds, glycidyl amine epoxy compounds, and isocyanurate epoxy compounds.
[0082] Examples of the polyisocyanate compound include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, hexamethylene diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, 1,5-naphthylene diisocyanate, 1,3,6-hexamethylene triisocyanate, 1,6,11-undecane triisocyanate, and bicycloheptane triisocyanate.
[0083] Examples of the aziridine compound include tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, tris[1-(2-methyl)aziridinyl]phosphine oxide, and hexa[1-(2-methyl)aziridinyl]triphosphatriazine.
[0084] Examples of the sulfide include sulfur, 4,4′-dithiomorpholine, tetramethylthiuram disulfide, and tetraethylthiuram disulfide.
[0085] Examples of the basic metal oxide include zinc oxide, lead oxide, calcium oxide, and magnesium oxide.
[0086] Examples of the organic metal halide include dicyclopentadienyl metal dihalide, and examples of the metal include titanium, zirconium, and the like.
[0087] These crosslinking agents may be used alone or in combination of two or more. The amount of each crosslinking agent is 0.05 to 20 parts by weight, preferably 0.1 to 10 parts by weight, based on 100 parts by weight of the acrylic copolymer of the present invention.
[0088] In addition, the acrylic copolymer-containing composition of the present invention can be arbitrarily blended with other additives commonly used in the technical field, such as lubricants, antioxidants, light stabilizers, fillers, reinforcing agents, plasticizers, processing aids, pigments, colorants, crosslinking accelerators, crosslinking aids, crosslinking delay agents, antistatic agents, foaming agents, etc.
[0089] Furthermore, within the scope of not departing from the gist of the present invention, mixing with rubber, resin, etc., which is generally performed in the technical field, can be performed. If the rubber used in the present invention is exemplified, butadiene rubber, styrene-butadiene rubber, isoprene rubber, natural rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-isoprene rubber, ethylene-propylene-diene rubber, epichlorohydrin rubber, etc. can be listed, and if the resin is exemplified, PMMA (polymethyl methacrylate) resin, PS (polystyrene) resin, PUR (polyurethane) resin, PVC (polyvinyl chloride) resin, EVA (ethylene / vinyl acetate) resin, AS (styrene / acrylonitrile) resin, PE (polyethylene) resin, etc. can be listed.
[0090] The total amount of the rubber and the resin blended is 50 parts by weight or less, preferably 10 parts by weight or less, and more preferably 1 part by weight or less, based on 100 parts by weight of the acrylic copolymer of the present invention.
[0091] As a method for blending the acrylic copolymer-containing composition of the present invention, any means conventionally used in the field of polymer processing can be utilized, for example, an open roll, a Banbury mixer, various kneading machines, etc. can be utilized.
[0092] The blending step can be carried out according to the usual steps in the field of polymer processing. For example, the following steps can be used: first, only the polymer is kneaded, then a kneading mixture A is prepared by adding a blending agent other than a crosslinking agent and a crosslinking accelerator, and then a crosslinking agent and a crosslinking accelerator are added to the mixture B for kneading.
[0093] The composition of the present invention can be made into a cross-linked product by heating to 100 to 250° C. The cross-linking time varies depending on the temperature, but is generally carried out between 0.5 and 300 minutes. The cross-linking molding can be any of the following cases: a case where cross-linking and molding are carried out integrally; or a case where a cross-linked product is made by heating the previously molded acrylic copolymer-containing composition again; or a case where heating is first performed and then a process for molding the cross-linked product is performed. As a specific method for cross-linking molding, any method such as compression molding using a metal mold, injection molding, steam tank, air bath, infrared or microwave heating can be used.
[0094] The acrylic copolymer-containing composition of the present invention obtained in this manner has excellent roll processability during processing. In addition, when the acrylic copolymer-containing composition of the present invention is made into a sheet (uncrosslinked sheet) having a thickness of about 2 to 2.5 mm, its Mooney scorch time (t5) (JIS K6300) at 125° C. is, for example, 1 to 10 minutes, preferably about 2 to 8 minutes.
[0095] Furthermore, in the present invention, not only the roll processability of the composition containing the acrylic copolymer is excellent, but also the normal physical properties and heat resistance of the obtained cross-linked product under long-term high temperature are excellent. For example, the tensile elongation at break EB (%) as the normal physical property of the cross-linked product can be determined according to JIS K6251, for example, 100 to 400%, preferably 120 to 350%. In addition, the A-type Durometer hardness Hs (JIS A) as the normal physical property of the cross-linked product can be determined according to JIS K6253, for example, 30 to 100, preferably 40 to 80.
[0096] In addition, the heat resistance after the heat aging test at 190°C for 336 hours can be evaluated by the change rate of the tensile elongation before and after the test (ΔEB (%) = {(EB (%) after the heat aging test - EB (%) before the heat aging test) / EB (%) before the heat aging test} × 100 (%)) and the difference in hardness Hs before and after the test (ΔHs = Hs after the heat aging test - Hs before the heat aging test). The ΔEB (%) of the crosslinked product of the present invention is, for example, -48 or more, preferably -45 or more, more preferably -40 or more, further preferably -30 or more, particularly preferably -20 or more, and most preferably -10 or more. In addition, the upper limit of ΔEB (%) is not particularly limited, and can be +30, +20, +10, or about +5.
[0097] ΔHs is, for example, within ±20, preferably within ±15, and more preferably within ±10.
[0098] The cross-linked product of the present invention can be suitably used as various gaskets such as an O-ring, a gasket, a diaphragm, an oil seal, a shaft seal, a bearing seal, a mechanical seal, a wellhead seal, a seal for electrical and electronic equipment, a seal for pneumatic equipment, a cylinder head gasket installed at the connection between a cylinder block and a cylinder head, a rocker cover gasket installed at the connection between a rocker cover and a cylinder head, an oil pan gasket installed at the connection between an oil pan and a cylinder head or a transmission, a gasket for a fuel cell diaphragm installed between a pair of housings that sandwich a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and a gasket for a top cover of a hard disk drive by taking advantage of the above-mentioned properties.
[0099] Furthermore, the cross-linked product of the present invention can be used as a rubber material, as an extrusion-molded product and a molded-cross-linked product for automobile use, and is suitable for various hoses such as fuel hoses, filler hoses, vent hoses, steam hoses, fuel oil hoses around fuel tanks, such as oil hoses, air hoses such as turbo air hoses and emission control hoses, radiator hoses, heater hoses, brake hoses, and air conditioning hoses.
[0100] This application claims the benefit of priority based on Japanese Patent Application No. 2016-233279 filed on November 30, 2016. The entire contents of the specification of Japanese Patent Application No. 2016-233279 filed on November 30, 2016 are incorporated herein by reference.
[0101] Example
[0102] The present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0103] In the present example and comparative example, the preparation of acrylic copolymers, the physical properties of acrylic copolymer-containing compositions containing the obtained acrylic copolymers and a crosslinking agent, and crosslinked products obtained by crosslinking the acrylic copolymer-containing compositions were evaluated.
[0104] [Example 1]
[0105] (Preparation of acrylic acid copolymer A)
[0106] Into a polymerization reactor equipped with a thermometer, a stirring device, a nitrogen inlet pipe and a decompression device, 200 parts by weight of water, 1.7 parts by weight of polyoxyalkylene alkyl ether phosphate, 41.4 parts by weight of ethyl acrylate as a monomer, 45.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of n-butyl methacrylate and 1.4 parts by weight of monoethyl fumarate were added, degassing and nitrogen replacement based on reduced pressure were repeated, and after oxygen was fully removed, 0.1 parts by weight of sodium ascorbate and 0.1 parts by weight of potassium persulfate were added to initiate emulsion polymerization at normal pressure and room temperature, and the reaction was continued until the polymerization conversion rate reached 95%, and 0.0075 parts by weight of hydroquinone was added to terminate the polymerization. The obtained emulsion polymerization liquid was coagulated with a sodium sulfate aqueous solution, washed with water, and dried to obtain an acrylic copolymer A.
[0107] [Example 2]
[0108] (Preparation of acrylic acid copolymer B)
[0109] Acrylic copolymer B was obtained in the same manner as in Example 1, except that the added monomers and their amounts were changed to 47.4 parts by weight of ethyl acrylate, 39.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of n-hexyl methacrylate and 1.4 parts by weight of monoethyl fumarate.
[0110] [Example 3]
[0111] (Preparation of Acrylic Copolymer C)
[0112] Acrylic copolymer C was obtained in the same manner as in Example 1, except that the added monomers and their amounts were changed to 49.4 parts by weight of ethyl acrylate, 37.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of 2-ethylhexyl methacrylate and 1.4 parts by weight of monoethyl fumarate.
[0113] [Example 4]
[0114] (Preparation of acrylic acid copolymer D)
[0115] Acrylic copolymer D was obtained in the same manner as in Example 1 except that the added monomers and their amounts were changed to 59.4 parts by weight of ethyl acrylate, 27.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of isodecyl methacrylate and 1.4 parts by weight of monoethyl fumarate.
[0116] [Example 5]
[0117] (Preparation of acrylic acid copolymer E)
[0118] Acrylic copolymer E was obtained in the same manner as in Example 1 except that the added monomers and their amounts were changed to 69.4 parts by weight of ethyl acrylate, 17.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of lauryl methacrylate and 1.4 parts by weight of monoethyl fumarate.
[0119] [Example 6]
[0120] (Preparation of acrylic acid copolymer G)
[0121] The same procedure as in Example 1 was followed, except that the monomers and their amounts were changed to 35.0 parts by weight of ethyl acrylate, 52.0 parts by weight of n-butyl acrylate, 11.8 parts by weight of isopropyl methacrylate and 1.4 parts by weight of monoethyl fumarate, to obtain acrylic copolymer G.
[0122] [Example 7]
[0123] (Preparation of Acrylic Copolymer H)
[0124] Acrylic copolymer H was obtained in the same manner as in Example 1, except that the added monomers and their amounts were changed to 41.4 parts by weight of ethyl acrylate, 37.4 parts by weight of n-butyl acrylate, 19.8 parts by weight of n-butyl methacrylate and 1.4 parts by weight of monoethyl fumarate.
[0125] [Example 8]
[0126] (Preparation of Acrylic Copolymer I)
[0127] Acrylic copolymer I was obtained in the same manner as in Example 1, except that the added monomers and their amounts were changed to 43.4 parts by weight of ethyl acrylate, 43.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of isobutyl methacrylate and 1.4 parts by weight of monoethyl fumarate.
[0128] [Comparative Example 1]
[0129] (Preparation of acrylic acid copolymer F)
[0130] Acrylic copolymer F was obtained in the same manner as in Example 1 except that the monomers and their amounts were changed to 49.3 parts by weight of ethyl acrylate, 49.3 parts by weight of n-butyl acrylate and 1.4 parts by weight of monoethyl fumarate.
[0131] [Comparative Example 2]
[0132] (Preparation of Acrylic Copolymer J)
[0133] Acrylic copolymer J was obtained in the same manner as in Example 1 except that the monomers and their amounts were changed to 19.4 parts by weight of ethyl acrylate, 59.4 parts by weight of n-butyl acrylate, 19.8 parts by weight of methyl methacrylate and 1.4 parts by weight of glycidyl methacrylate.
[0134] [Comparative Example 3]
[0135] (Preparation of Acrylic Acid Copolymer K)
[0136] The same procedure as in Example 1 was carried out except that the monomers and their amounts were changed to 41.4 parts by weight of ethyl acrylate, 45.4 parts by weight of n-butyl acrylate, 11.8 parts by weight of n-butyl methacrylate and 1.4 parts by weight of glycidyl methacrylate to obtain acrylic copolymer K.
[0137] <Mooney viscosity (ML 1+4 , 100℃)>
[0138] The acrylic copolymers A to K were subjected to a Mooney viscosity test in accordance with the physical testing methods for uncrosslinked rubber in accordance with JIS K6300. The Mooney viscosity (ML) at 100° C. was measured using Mooney Viscometer AM-3 manufactured by TOYO SEIKI KOGYO CO. LTD. 1+4 The results are shown in Table 1.
[0139] (Preparation of Composition Containing Acrylic Copolymer)
[0140] 100 parts by weight of each acrylic copolymer A to K, 60 parts by weight of carbon black (classified according to ASTM D1765; N550), 2 parts by weight of stearic acid (dispersant and softener for carbon black) and 2 parts by weight of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (anti-aging agent) were kneaded at 120°C using a kneader, and then 0.6 parts by weight of hexamethylenediamine carbamate (aliphatic diamine crosslinking agent) and 2 parts by weight of di-o-tolylguanidine (crosslinking accelerator) were added, and kneaded using a kneading roll at room temperature to prepare each acrylic copolymer-containing composition.
[0141] (Manufacturing of Uncrosslinked Sheet)
[0142] The acrylic copolymer-containing compositions obtained above were kneaded using a kneader and an open roll to produce an uncrosslinked sheet having a thickness of 2 to 2.5 mm.
[0143] (Mooney scorch test)
[0144] The obtained uncrosslinked sheet was used to measure the Mooney scorch test specified in JIS K 6300 at 125°C using Mooney Viscometer AM-3 manufactured by TOYO SEIKI KOGYO CO. LTD.
[0145] (Preparation of cross-linked product)
[0146] The uncrosslinked rubber sheet obtained above was subjected to a press treatment at 180° C. for 10 minutes, and was further heated at 180° C. for 3 hours in an air oven to obtain a crosslinked product.
[0147] (Cold resistance test)
[0148] Evaluation was performed by a Gilman torsion test using TM-2533 manufactured by Ueshima Seisakusho Co., Ltd. in accordance with JIS K 6261, and the temperature (T10) at which the modulus at room temperature (25° C.) becomes 10 times was measured. The lower the temperature of T10, the better the cold resistance.
[0149] (Test of normal physical properties)
[0150] The obtained cross-linked product was subjected to tensile test and hardness test evaluation using TG-2kN manufactured by MinebeaMitsumi Inc. The tensile test was performed using a No. 3 dumbbell test piece in accordance with the method described in JIS K 6251, and the hardness test was performed in accordance with the method described in JIS K 6253.
[0151] (Heat aging test)
[0152] The crosslinked product was subjected to heat aging at 190° C. for 336 hours. After the heat aging, the tensile test and hardness test were evaluated in the same manner as in the normal physical property test.
[0153] Table 1 shows the test results of Examples and Comparative Examples obtained by the above-mentioned respective test methods.
[0154] In each table, t5 represents the Mooney scorch time specified in the Mooney scorch test of JIS K6300, EB represents the tensile elongation at break specified in the tensile test of JIS K6251, and Hs represents the A-type durometer hardness specified in the hardness test of JIS K6253. ΔEB and ΔHs are the change rate of EB relative to the normal physical property (before the heat aging test) (ΔEB (%) = {(EB after the heat aging test (%) - EB before the heat aging test) / EB before the heat aging test (%)} × 100 (%)) and the difference in Hs (= Hs after the heat aging test - Hs before the heat aging test).
[0155]
[0156] ※1Tensile test could not be performed due to curing.
[0157] As shown in Table 1, the results of the heat aging test for Examples 1 to 8, which are crosslinked products formed by crosslinking the copolymer of the present invention, are as follows: the elongation change rate (ΔEB) and hardness change (ΔHs) after heat aging are small compared to the comparative examples. In particular, when n-butyl methacrylate is used as a copolymer component, the elongation change rate (ΔEB) is smaller while maintaining cold resistance, and the heat resistance is improved. From these results, it can be seen that the crosslinked product formed by crosslinking the acrylic copolymer of the present invention has a small elongation change rate and hardness change even when exposed to high temperature for a long time, and is excellent in heat resistance.
[0158] Industrial Applicability
[0159] The acrylic copolymer of the present invention can be widely used as a material for rubber products or resin products that exhibit excellent heat resistance, weather resistance, ozone resistance, and abrasion resistance, or as a raw material for adhesives or coatings. In particular, a cross-linked product prepared using the acrylic copolymer of the present invention is very effective for automotive applications such as fuel hoses, air hoses, and pipe materials.
Claims
1. An acrylic copolymer comprising: 45 to 89.5% by weight of a structural unit (A) derived from an acrylic acid ester having an alkyl group having 1 to 8 carbon atoms, 10 to 30% by weight of a structural unit (B) derived from at least one selected from the group consisting of n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, n-decyl methacrylate, isodecyl methacrylate and n-lauryl methacrylate, and 0.5 to 5% by weight of a structural unit (C) derived from a monoalkyl fumarate, The total amount of the structural unit (A), the structural unit (B), and the structural unit (C) is 100% by weight.
2. The acrylic copolymer according to claim 1, wherein The structural unit (A) contains both a structural unit (A1) derived from an acrylic acid ester having an alkyl group having 1 to 3 carbon atoms and a structural unit (A2) derived from an acrylic acid ester having an alkyl group having 4 to 8 carbon atoms.
3. The acrylic copolymer according to claim 2, wherein The weight ratio of the structural unit (A1) to the structural unit (A2) (A1):(A2) is 10:90 to 90:
10.
4. The acrylic copolymer according to claim 2, wherein The weight ratio of the structural unit (A1) to the structural unit (A2) (A1): (A2) is 30:70 to 70:
30.
5. The acrylic copolymer according to claim 1 or 2, wherein The alkyl group of the structural unit (B) has 4 to 9 carbon atoms.
6. The acrylic copolymer according to claim 1 or 2, wherein the Mooney viscosity (ML 1+4 ) is 10 to 100.
7. A composition containing an acrylic copolymer, characterized in that: The present invention comprises the acrylic copolymer according to any one of claims 1 to 6 and a cross-linking agent.
8. The acrylic copolymer-containing composition according to claim 7, when made into an uncrosslinked sheet having a thickness of about 2 to 2.5 mm, has a Mooney scorch time t5 of 1 to 10 minutes at a temperature of 125°C.
9. A cross-linked product prepared using the acrylic copolymer-containing composition according to claim 7 or 8.
10. The cross-linked product according to claim 9, which exhibits at least one of the following characteristics (i) and (ii): (i) Elongation at break EB is 100-400%; (ii) Type A Durometer hardness Hs is 30 to 100.
11. The cross-linked product according to claim 9 or 10, wherein the change rate (%) of the elongation at break EB before and after heating at a temperature of 190°C for 336 hours is -48 or more.
12. The cross-linked product according to claim 9 or 10, wherein the type A durometer hardness Hs after heating at 190°C for 336 hours shows a change within ±20 relative to the type A durometer hardness Hs before heating.