Preparation method of latex solidified material and edge-pressed latex mold cup, preparation method and application

The latex mold cup prepared through the edge-pressing, shaping and vulcanization process solves the problems of uneven density and inaccurate edges of the latex mold cup, achieving a latex bra with high density, uniform edges and healthy standards, and improving the processing efficiency and product quality of the bra.

CN110281452BActive Publication Date: 2024-10-18LONGNAN JIANYING UNDERWEAR CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201910678059.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-25
Publication Date
2024-10-18
Estimated Expiration
2039-07-25

AI Technical Summary

Technical Problem

The existing latex mold cup process has problems such as uneven density, inaccurate edges, the use of toxic substances, complex processes, and low efficiency, which prevents latex bras from being widely used in the bra industry.

Method used

The edge-pressing latex mold cup is prepared using the edge-pressing shaping and vulcanization process. By mixing the raw latex with the dispersion, stirring and foaming, spraying and adding gelling agent, it is then heated and pressure-vulcanized in the vulcanizer to form a high-density, precise edge. Latex mold cups, avoid using toxic substances such as sodium fluorosilicate.

Benefits of technology

It achieves high density, uniform edges, and no steel ring support effect of the latex mold cup, improves the processing speed and product quality of the bra, reduces production costs, is suitable for large-scale applications, and complies with health standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110281452B_ABST
    Figure CN110281452B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a latex solidified material and a pressed edge latex mold cup, a preparation method and an application. The method for preparing the pressed edge latex mold cup comprises: transferring the latex solidified material into a mold cup mold of a vulcanizer; heating and pressurizing the vulcanizer to press, shape and vulcanize the latex solidified material; leaching with hot water and drying. The pressed edge latex mold cup provided by the present invention adopts a full-health additive and is free of toxic substances such as sodium fluorosilicate. The product is healthier and more suitable for skin-friendly use, especially for women's delicate breast skin, and has a high plastic deformation retention rate, and is very good in elasticity and strength. Secondly, the present invention creates a new process method to prepare latex foam sponges of different densities from the same latex foaming material, which is not limited to the underwear industry. More foamed products can be processed more simply because of this process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of female bra cups and latex, and in particular to a method for preparing a latex solidified material and a pressed edge latex cup, a preparation method and an application thereof. Background Art

[0002] In recent years, bras made of latex mold cups are developing rapidly. However, the bras made of latex mold cups are subject to process restrictions. The production process of latex pillows and mattresses is still used. This process adopts the Dunlop process: first, the foamed mature latex is poured into the mold cavity, and after vulcanization into a latex mold cup, the edge is cut for use.

[0003] The main reasons why latex cups prepared by Dunlop process cannot be widely used in the underwear industry are as follows:

[0004] The overall density of the mold cup is the same. If the mold cup is very thin, the edge of the mold cup will be very thin, and it will be easy to break during the sewing process of the whole bra. Even if it is well sewn, it will break under the force when the consumer wears it, resulting in the product being scrapped. If the mold cup is thick, the edge of the mold cup will be very thick. During the sewing process of the whole bra, the edge of the mold cup will be impossible to sew or extremely difficult to sew because it is too thick. Even if the thickness of the edge is more than 5mm, its bearing capacity is still not ideal, and the edge will still break if a little force is applied when wearing or washing the bra.

[0005] The mold cup is a precision product. The latex foaming process is limited by shrinkage and edge accuracy. After latex foaming and vulcanization, it needs to be dried. The electrolyzed water of rubber particles and the water content of latex will cause the product to have a shrinkage rate of 7%-8%. The final forming process of the mold cup cannot reach a constant value, and the edge accuracy cannot be accurate to less than 1mm. Whether it is the curvature, edge thickness, or length, even a difference of 1mm will lead to a "slight error, a thousand miles away". This is one of the important reasons why the underwear industry cannot use latex foam cotton to make mold cups on a large scale.

[0006] The mold of the existing latex foaming process needs to be prepared into a mold suitable for filling, that is, the mold consists of an upper and lower mold. The upper mold has a glue injection hole, and the latex is poured in from the upper part for vulcanization molding. The polyurethane sponge mold of the existing industry is completely unusable, which is not only a waste of the existing mold cup industry, but also will lead to a large number of unemployment of employees in the existing mold cup industry. The mature mold cup shapes used by various underwear processing companies cannot be used, and the gathering and shaping effect cannot be guaranteed. This is one of the important factors that the industry cannot use latex as a new material for mold cups on a large scale.

[0007] The design of the bra cup is the focus of bra design. The various force factors and their combination in the cup design affect the pressure size and pressure distribution when the bra is worn, which in turn affects the breast health, the comfort, fit, and body shaping beauty of the bra. The cup part of the bra is the most direct part that contains and supports the breasts, directly acts on the female chest, adapts to the shaking of the breasts, conforms to the strain and slippage of the skin, and shapes the female chest shape, playing a very important role. At present, all the latex bras sold on the market are prepared by mold filling and vulcanization process. The disadvantage of the products is that the prepared cups have scattered and expanded breast shapes when worn, and cannot achieve the effect of gathering and shaping. The main reason is that the density around the four sides of the cup is too low, which makes the cup unable to withstand a certain force. It is precisely because it cannot withstand a certain force that the gathering, support, and pull-up processes of the bra have no focus. Due to the process limitations of latex cup processing, latex bras cannot flourish in the bra industry. The processing is difficult, the processing efficiency is low, the processing cost is high, and the product gathering and shaping effects cannot be achieved.

[0008] The latex cup products currently seen on the market are all prepared by latex foaming, and their processes still use two processes of latex sponge: one is the Dunlop process, and the other is the Traley process. The process of the Dunlop method is: the raw latex that meets the requirements after ammonia removal is added to each dispersion and then matured. After maturity, a soap foaming agent is added to the rubber material. While mechanically foaming, zinc oxide and sodium fluorosilicate (also called sodium silicofluoride) are injected, and then the mixed latex is injected into the model for gelation and vulcanization to obtain the corresponding products. Among them, the gelling agent sodium fluorosilicate is a moderately toxic substance with a median lethal dose of 125mg / kg, which is irritating and toxic in contact with the skin. It hydrolyzes slowly and is not easy to be eliminated in the leaching process in the production process. Therefore, the Dunlop process is not suitable for skin-fitting products, especially for women's breast skin, which is relatively delicate; and because rubber hydrocarbons are hydrophobic molecules and human skin is hydrophilic, sodium fluorosilicate will repel rubber hydrocarbon molecules after hydrolysis of human sweat and combine with human hydrophilic skin, causing great harm to human skin. This point has not been sufficiently recognized in latex bedding, especially for women's breast skin which is so close to human skin.

[0009] In the Dunlop process, the ammonia removal process is an unpleasant process. First of all, the smell of ammonia water is quite irritating. There are usually two methods in the process of ammonia removal, one is stirring to remove ammonia, and the other is formaldehyde to remove ammonia. Both methods are not environmentally friendly. It is difficult to recover ammonia gas by stirring to remove ammonia, and the phenomenon of secret discharge is serious. Secondly, formaldehyde to remove ammonia, if the amount of latex is large, formaldehyde will make the product have a pungent taste after being added to latex. At the same time, formaldehyde is toxic and harmful to the human body and is not good for the health of production workers.

[0010] Latex sponge is a low-density, porous, open, continuous foam of rubber. The Dunlop process is generally used to manufacture latex sponge: latex ammonia removal - adding compounding agent - mechanical bubbles and adding gelling agent - injection molding - gelling and vulcanization - demoulding - washing and drying. The products produced by this process have been vulcanized and cannot be processed for secondary shaping like polyurethane sponge. Latex sponge cannot be processed for secondary shaping, so the current solution is to use the process of latex pillows and latex mattresses, and use mold filling to prepare latex mold cups. Summary of the invention

[0011] In order to solve the above problems, based on a lot of research, one of the technical problems solved by the present invention is to provide a latex mold cup with pressed edge prepared by a process of latex pressing, shaping and vulcanization.

[0012] The second technical problem solved by the present invention is to provide a method for preparing the above-mentioned edge-pressed latex mold cup.

[0013] The third technical problem solved by the present invention is to provide the application of the above-mentioned edge-pressed latex mold cup.

[0014] The fourth technical problem solved by the present invention is to provide a latex solidified material and a preparation method thereof.

[0015] To achieve the above object, the present invention provides the following technical solutions:

[0016] A method for preparing a latex solidified material comprises the following steps:

[0017] S01: mixing the raw latex and the dispersion, stirring and foaming to obtain latex foam;

[0018] S02: spraying latex foam onto a carrier;

[0019] S03: Adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 65-75° C. for 5-15 minutes to obtain a latex solid.

[0020] A latex solidified material is prepared by adopting the above method.

[0021] As a preferred technical solution, the raw latex in step S01 is natural rubber and / or synthetic rubber.

[0022] As a further preferred technical solution, the raw latex in step S01 consists of 65-75wt% natural rubber and 25-35wt% synthetic rubber.

[0023] As a preferred technical solution, the nitrogen content in the natural rubber is 0.1-0.6wt%.

[0024] As a preferred technical solution, the synthetic rubber is at least one of styrene-butadiene rubber, nitrile rubber, and polyisoprene rubber.

[0025] As a preferred technical solution, the mass ratio of the raw latex and the dispersion in step S01 is (8.5-9.5): (0.5-1.5).

[0026] As a preferred technical solution, the dispersion in step S01 includes a vulcanizing agent, an accelerator, an antioxidant, an activator, and a foaming agent.

[0027] As a further preferred technical solution, the dispersion in step S01 includes 1.5-2.5 parts by weight of a vulcanizing agent, 0.8-1.2 parts by weight of an accelerator, 2-3 parts by weight of an antioxidant, 1-1.5 parts by weight of an activator, and 1-2 parts by weight of a foaming agent.

[0028] As a preferred technical solution, in step S02, the surface of the carrier is sprayed with an anti-adhesion substance, which is Teflon, silicone or a release agent.

[0029] As a preferred technical solution, the carrier in step S02 is a stainless steel plate or a conveyor belt of an assembly line. The stainless steel plate is 250-350 mm long and 150-250 mm wide.

[0030] As a preferred technical solution, the thickness of the latex foam sprayed on the carrier in step S02 is 2-20 mm, preferably 3-10 mm.

[0031] As a preferred technical solution, the gelling agent in step S03 includes organopolysiloxane, ammonium sulfate, ammonium acetate, ammonium acetate, and polyethylene glycol ether substances.

[0032] As a preferred technical solution, the amount of the gelling agent added in step S03 is 2.8-3.6% of the weight of the raw latex; the gelling agent in step S03 includes organic polysiloxane, ammonium sulfate, ammonium acetate, ammonium acetate, polyethylene glycol isooctylphenyl ether, and arylethylphenyl polyethylene glycol ether.

[0033] As a further preferred technical solution, the gelling agent in step S03 includes organopolysiloxane, polyethylene glycol p-isooctylphenyl ether, and arylethylphenyl polyethylene glycol ether.

[0034] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0035] S04: transferring the latex solidified product into a cup mold of a vulcanizing machine;

[0036] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0037] S06: hot water leaching and drying.

[0038] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0039] S01: mixing the raw latex and the dispersion, stirring and foaming to obtain latex foam;

[0040] S02: spraying latex foam onto a carrier;

[0041] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 65-75° C. for 5-15 minutes to obtain a latex solid;

[0042] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0043] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0044] S06: hot water leaching and drying.

[0045] As a preferred technical solution, the cup mold used in step S04 is a mold commonly used in the cup mold industry for existing polyurethane sponge hot pressing.

[0046] As a preferred technical solution, in step S05, the temperature of the vulcanizer is heated to 90-115°C and the pressure is adjusted to 180-220kg / cm 3 .

[0047] As a preferred technical solution, the hot water leaching in step S06 is performed by soaking and leaching in 50-80° C. hot water for 1-5 minutes.

[0048] As a preferred technical solution, the drying in step S06 is spin drying and / or baking.

[0049] The invention provides a process for preparing an edge-pressed latex mold cup without using sodium fluorosilicate as a gelling agent.

[0050] The second aspect of the present invention provides a pressed edge latex mold cup, which is prepared by the method for preparing the pressed edge latex mold cup as described above.

[0051] The third aspect of the present invention provides the use of the above-mentioned pressed edge latex mold cup in a natural rubber latex bra.

[0052] The edge-pressed latex mold cup is fixed in the cup by sewing, gluing, inserting and the like to produce a natural latex bra.

[0053] Beneficial effects: The edge-pressed latex mold cup provided by the present invention adopts all-health additives and does not contain toxic substances such as sodium fluorosilicate. The product is healthier and more suitable for use next to the skin, especially for the delicate breast skin of women. It has a very high plastic deformation retention rate, and has good elasticity and strength. The bra made from it is easy to accommodate and support the breasts to adapt to the shaking of the breasts, conform to the strain and slippage of the skin, and is beneficial to shaping and correcting the female breast shape. The edge-pressed natural latex mold cup of the present invention has good mechanical properties, and has excellent mechanical properties such as a good steel ring-free supporting part, a gathered force-bearing part, a supporting force-bearing part and a lifting force-bearing part; secondly, the present invention creates a new process method to prepare latex foam sponges of different densities from the same latex foaming material, which is not limited to the underwear industry. More foaming products can be processed more simply because of this process.

[0054] Specifically, the present invention has the following advantages:

[0055] (1) The precision of the latex foaming mold cup product prepared by the edge-pressed latex mold cup used in the present invention is guaranteed. After edge pressing, the edge density is large, the thickness is thin, and the load-bearing capacity is uniform, which is infinitely close to the very mature processing technology of polyurethane sponge mold cups, and provides the basic process conditions for the underwear industry to apply latex sponge mold cups to process bras on a large scale. Compared with the existing latex mold cups, the product is more precise, with a small middle density, a large edge density, and a thin processing position, and can be generally applied to the bra processing industry.

[0056] (2) The edge-pressed latex mold cup used in the present invention has greatly improved the stress points around the cup after edge pressing, and the edge of the mold cup can withstand a certain amount of force. This provides processing conditions for the subsequent processing of the bra: the non-wire support part, the gathered stress-bearing part, the support stress-bearing part, the upward pull-up stress-bearing part, etc. Compared with the existing latex mold cup, the edge is firm and has a certain stress-bearing capacity, providing a force guarantee for the development of the mold cup.

[0057] (3) The edge-pressed latex mold cup used in the present invention improves the processing speed and efficiency when sewing the bra mold cup after edge pressing, reduces the low efficiency caused by edge rot when sewing ordinary latex mold cups, and thus saves labor costs.

[0058] (4) The edge-pressed latex cup used in the present invention improves the product quality of the latex bra after edge pressing, making the suture between the latex cup and the bra more secure, increasing the time consumers can use the product, and greatly improving the tensile stress strength when worn and the strength when washed. Compared with the existing latex cup, the edge is firm, and there is no high probability of edge rot during wearing and washing.

[0059] (5) The edge-pressed latex cup mold used in the present invention adopts the edge-pressing process, can be grafted with the mature cup shape currently sold on the market, and can use the same mold as the polyurethane foam sponge cup mold, without the need to develop a latex cup mold separately. This avoids the increased development cost of new materials and the waste of existing industries, thereby achieving the environmental protection effect of energy saving and emission reduction.

[0060] (6) The edge-pressed latex mold cup used in the present invention adopts an edge-pressing process, which allows bra processing companies to popularize the bra processing of latex mold cups more quickly and reduce the time and cost of mold cup and mold development. Compared with the existing latex mold cup process, the existing latex mold cup filling mold is completely different from the mature polyurethane sponge mold cup mold and needs to be redeveloped. For precision products such as mold cups, debugging a qualified cup shape requires a lot of manpower, time and money. This process can graft the mature cup shape of the polyurethane sponge mold. Save development investment, quickly enter the latex bra market, and lower the threshold for latex materials to enter the underwear industry.

[0061] (7) The process system used in the present invention does not contain toxic materials such as sodium fluorosilicate, and the produced underwear meets health requirements. Sodium fluorosilicate is a moderately toxic substance with a median lethal dose of 125 mg / kg, which is irritating and toxic in contact with the skin. It hydrolyzes slowly and is not easy to be completely eliminated in the leaching process in the production process. The edge-pressing latex mold cup process used in the present invention uses WS preparation as the gelling material, which is cured by a high-pressure and high-temperature finalizing vulcanization process, replacing the existing sodium fluorosilicate gelling material. The applicant unexpectedly discovered that the WS preparation has the effect of a latex stabilizer below 25°C, which has a good production control effect for large-scale production, has a heat-sensitive effect above 25°C, and can obtain a uniform and delicate latex foaming solid at 60°C-70°C.

[0062] (8) The latex cotton process system used in the present invention is completely different from the existing Dunlop and Trale processes. The applicant combines dry rubber with latex processes in the present invention, and integrates some dry rubber refining, calendering, molding, vulcanization and other methods in the process. Combined with the colloidal properties of latex, a high-temperature and high-pressure latex product process is invented. In this way, different density requirements of an item can be met, and its density can increase or decrease in a step-by-step manner. It has a wide range of applications and contributes to the level of latex cotton preparation technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 It is a schematic diagram of the structure of the vulcanizing machine in step S05.

[0064] Among them, 1-upper mold; 2-lower mold; 3-pressure cylinder; 4-upper heating plate; 5-lower heating plate.

[0065] Figure 2 It is a structural schematic diagram of a pressed edge latex mold cup.

[0066] Among them, 21 is a natural latex foam; 22 is a crease portion; 23 is a press edge portion; 24 is a surrounding press edge portion.

[0067] Figure 3 It is a schematic diagram of the structure of a natural latex bra with a pressed edge latex mold cup.

[0068] Among them, 31-left cup; 32-right cup; 33-back bra and other accessories; 34-shoulder strap; 35-pressed latex mold cup. DETAILED DESCRIPTION

[0069] The following is a further clear and complete description of the technical features in the technical solution provided by the present invention in conjunction with specific implementation methods, which is not intended to limit the scope of protection thereof.

[0070] The words "preferred", "further preferred" and the like in the present invention refer to embodiments of the present invention that can provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0071] When a numerical range is disclosed herein, the above range is deemed to be continuous and includes the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all sub-ranges included therein. For example, a specified range from "1 to 10" should be deemed to include any and all sub-ranges between a minimum of 1 and a maximum of 10. Exemplary sub-ranges of ranges 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.

[0072] The meaning of "upper and lower" in the present invention refers to that when the reader is facing the attached drawing, the upper side of the view shown to the reader is the upper side, and the lower side of the reader is the lower side, rather than a specific limitation on the device mechanism of the present invention.

[0073] A method for preparing a latex solidified material comprises the following steps:

[0074] S01: mixing the raw latex and the dispersion, stirring and foaming to obtain latex foam;

[0075] S02: spraying latex foam onto a carrier;

[0076] S03: Adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 65-75° C. for 5-15 minutes to obtain a latex solid.

[0077] A latex solidified material is prepared by adopting the above method.

[0078] In one embodiment, the latex solid is used in foamed latex cotton precision products.

[0079] In one embodiment, the foamed latex precision products of the present invention include dipped products, sponge products, woven products, and the like.

[0080] The latex solidified material can be obtained through conventional molding and heat vulcanization processes to obtain the foamed latex precision product.

[0081] The molding can be performed by compression molding, and the pressure of the molding machine used in the compression molding can be 0.4-1.0 MPa.

[0082] The thermal vulcanization temperature may be 100-120°C.

[0083] In one embodiment, the sponge products include pillows, mattresses, seat cushions, back cushions, sofas, waist protectors, neck protectors, insoles, bras, bra cups, etc.

[0084] In one embodiment, the latex cotton precision product is a bra cup mold.

[0085] The main raw material of the preparation method provided in the present invention is natural latex, and no ammonia is required. A vulcanizing agent, an accelerator, an antioxidant, etc. are directly added to prepare a dispersion, and then foamed by a continuous mechanical foaming machine and directly injected into a rust-free steel plate or sprayed onto a conveyor belt of an assembly line. The stainless steel plate with a certain thickness of latex foam is sprayed with a gelling agent and cured by heating to obtain a solidified product. The obtained solidified product is moved to a vulcanizing machine. Figure 1 The mold is pressurized and heated to vulcanize and shape. After a certain period of time, the mold is opened for leaching, drying and drying to obtain a pressed edge latex mold cup. The pressed edge latex mold cup is placed in a bra cup, and a steel ring or a strapping strip is placed at the pressed edge to prepare a latex mold cup bra.

[0086] In one embodiment, the stirring speed of the stirring and foaming in step S01 is 500-1500 r / min, preferably 800-1200 r / min; the time is 3-30 min, preferably 5-15 min.

[0087] In one embodiment, the raw latex in step S01 is natural rubber and / or synthetic rubber.

[0088] In one embodiment, the raw latex in step S01 consists of 65-75 wt % natural rubber and 25-35 wt % synthetic rubber.

[0089] In one embodiment, the raw latex in step S01 consists of 70 wt % natural rubber and 30 wt % synthetic rubber.

[0090] In one embodiment, the nitrogen content in the natural rubber is 0.1-0.6 wt %.

[0091] In one embodiment, the synthetic rubber is at least one of styrene-butadiene rubber, nitrile-butadiene rubber, and polyisoprene rubber.

[0092] In one embodiment, the mass ratio of the raw latex to the dispersion in step S01 is (8.5-9.5): (0.5-1.5).

[0093] In one embodiment, the mass ratio of the raw latex to the dispersion in step S01 is (8.6-9.2): (0.8-1.4).

[0094] In one embodiment, the mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0095] In one embodiment, the dispersion in step S01 includes a vulcanizing agent, an accelerator, an antioxidant, an activator, and a foaming agent.

[0096] In one embodiment, the dispersion in step S01 includes 1.5-2.5 parts by weight of a vulcanizing agent, 0.8-1.2 parts by weight of an accelerator, 2-3 parts by weight of an antioxidant, 1-1.5 parts by weight of an activator, and 1-2 parts by weight of a foaming agent.

[0097] In one embodiment, the dispersion in step S01 includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent.

[0098] In one embodiment, the vulcanizing agent is sulfur.

[0099] In one embodiment, the accelerator is a thiazole accelerator and / or a dithiocarbamate accelerator. The thiazole accelerator is selected from at least one of 2-mercaptobenzothiazole, 2-thiolbenzothiazole, dibenzothiazole disulfide, and 2-(4-morpholinyldithio)benzothiazole. The dithiocarbamate accelerator is selected from at least one of zinc dibenzyldithiocarbamate, zinc dimethyldithiocarbamate (PZ), zinc diethyldithiocarbamate (ZDC), zinc dibutyldithiocarbamate (BZ), and zinc ethylphenyldithiocarbamate.

[0100] In one embodiment, the accelerator is composed of 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:(0.2-0.3).

[0101] In one embodiment, the antioxidant is at least one of an amine antioxidant, a phenol antioxidant, and 2-thiol benzimidazole. The amine antioxidant is selected from octylated diphenylamine, dioctylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonamide)diphenylamine, N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, N- At least one of phenyl-N'-(3-formyloxy-2-hydroxypropyl) p-phenylenediamine, N,N'-bis(1-methylheptyl) p-phenylenediamine, N,N'-bis(1,4-dimethylpentyl) p-phenylenediamine, N,N'-bis(1-ethyl-3-methylpentyl) p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl p-phenylenediamine, phenylhexyl p-phenylenediamine, phenyl-α-naphthylamine, and phenyl-β-naphthylamine. The phenol antioxidant is selected from at least one of 2,6-di-tert-butyl-4-methylphenol, 2,2'-thiobis(4-methyl-6-tert-butylphenol), and 2,4-di(n-octylthiomethylene)-6-methylphenol.

[0102] 4,4'-Bis(α,α-dimethylbenzyl)diphenylamine

[0103] 4,4'-Bis(α,α-dimethylbenzyl)diphenylamine is highly efficient, non-toxic and low-volatile. It can provide excellent protection even at high temperatures. It is safe, non-toxic, pollution-free, has stable process and good aging resistance for women's close-fitting mold cup products. It is the most suitable amine antioxidant for close-fitting latex cotton.

[0104] In one embodiment, the activator is zinc oxide.

[0105] In one embodiment, the foaming agent is potassium oleate.

[0106] In one embodiment, in step S02, the surface of the carrier is sprayed with an anti-adhesion substance. The anti-adhesion substance is Teflon, silicone or a release agent. The purpose is to prevent the latex foam from adhering to the stainless steel plate or conveyor belt in the subsequent solidification process after spraying, resulting in waste or inability to move to the next process.

[0107] In one embodiment, the carrier in step S02 is a stainless steel plate or a conveyor belt of an assembly line. The stainless steel plate has a length of 250-350 mm and a width of 150-250 mm.

[0108] In one embodiment, the thickness of the latex foam sprayed on the carrier in step S02 is 2-20 mm, preferably 3-10 mm.

[0109] In one embodiment, the gelling agent in step S03 includes organopolysiloxane, ammonium sulfate, ammonium acetate, ammonium acetate, and polyethylene glycol ether substances.

[0110] In one embodiment, the amount of the gelling agent added in step S03 is 2.8-3.6% of the weight of the raw latex; the gelling agent in step S03 includes organopolysiloxane, ammonium sulfate, ammonium acetate, ammonium acetate, polyethylene glycol isooctylphenyl ether, and arylethylphenyl polyethylene glycol ether.

[0111] In one embodiment, the gelling agent in step S03 includes organopolysiloxane, polyethylene glycol p-isooctylphenyl ether, and arylethylphenyl polyethylene glycol ether.

[0112] In one embodiment, the gelling agent in step S03 is organopolysiloxane.

[0113] In many tests, the applicant unexpectedly found that the products made of Coagulant WS, an organopolysiloxane produced by Lanxess Technology Co., Ltd. of Germany, met the process requirements. The organopolysiloxane preparation was used as the gelling material, and after curing, it was subjected to high pressure and high temperature curing process, replacing the existing sodium fluorosilicate gelling. The organopolysiloxane was a yellow liquid, and the molding effect and product quality could be improved. The possible reason is that the selection of the thermosensitive agent directly affects the gelling effect and the molding effect. Ammonium chloride, ammonium acetate and ammonium nitrate gelled too fast, and were unstable for latex with high fatty acids. At the same time, the combination of the gelling and molding effects of ammonium sulfate was not particularly suitable for large-scale production. The organopolysiloxane preparation has good processing stability, and its gelled products do not contain inorganic salts and organic metal salts, have a low gelling temperature, and are better than inorganic thermosensitive agents in aging resistance, gelling texture and hygiene.

[0114] In one embodiment, the gelling agent in step S03 is composed of organopolysiloxane and arylethylphenyl polyethylene glycol ether in a mass ratio of 1:(0.1-0.2).

[0115] The applicant unexpectedly discovered that when an organopolysiloxane preparation is used in combination with aryl ethyl phenyl polyglycol ether (Emulvin WA, Lanxess, Germany), it acts as a latex stabilizer below 25°C, has a good production control effect for large-scale production, has a heat-sensitive effect above 33°C, and a uniform and delicate latex foaming solid can be obtained at 32°C-70°C.

[0116] In one embodiment, the gelling agent in step S03 is composed of organopolysiloxane, arylethylphenyl polyethylene glycol ether, and polyethylene glycol-p-isooctylphenyl ether in a mass ratio of 1: (0.1-0.2): (0.04-0.06).

[0117] The applicant has found that the use of a gelling agent composed of an organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether can further prevent the edge rot problem during use and improve the air permeability and aging resistance. This may be because the addition of polyethylene glycol p-isooctyl phenyl ether, together with aryl ethyl phenyl polyethylene glycol ether, can reduce surface tension, reduce the binding force between molecules, achieve a better foaming effect, and effectively improve the pore volume and stability of the latex foaming solidified product. The inventors found in subsequent studies that when the mass ratio of organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether is 1: (0.1-0.2): (0.04-0.06), the effect is best. The inventors speculate that this may be because the hydrophobic carbon chains of the two are different at this ratio, and the emulsification and dispersion effect is better through synergistic interaction, which further reduces the gap between the polar heads and forms a more uniform and stable foam volume. In addition, aryl ethyl phenyl polyethylene glycol ether and polyethylene glycol p-isooctyl phenyl ether can promote the extension of the molecular structure of organic polysiloxane, improve the uniform dispersion effect of each component in the system, make the latex foaming solid more uniform and delicate, quickly and evenly coagulate the latex, which is beneficial to the subsequent cross-linking and vulcanization of the latex foam, and has good mechanical properties, air permeability and aging resistance.

[0118] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0119] S04: transferring the latex solidified product into a cup mold of a vulcanizing machine;

[0120] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0121] S06: hot water leaching and drying.

[0122] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0123] S01: mixing the raw latex and the dispersion, stirring and foaming to obtain latex foam;

[0124] S02: spraying latex foam onto a carrier;

[0125] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 65-75° C. for 5-15 minutes to obtain a latex solid;

[0126] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0127] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0128] S06: hot water leaching and drying.

[0129] In one embodiment, the cup mold used in step S04 is a mold commonly used in the cup mold industry for existing polyurethane sponge hot pressing.

[0130] In one embodiment, in step S05, the temperature of the vulcanizer is heated to 90-115°C and the pressure is adjusted to 180-220 kg / cm 3 .

[0131] like Figure 1 As shown, the vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 105-115°C, driving the temperature of the upper and lower molds to 105-115°C, preferably 110°C, and the mold material is aluminum. The cylinder pressure is 180-220kg / cm 3 , preferably 200kg / cm 3 The applicant found in the test process that the pressure of the cylinder is determined by the density and thickness of the edge. If the pressure is insufficient, the density and thickness of the edge will not meet the requirements. If the pressure is too high, the density will increase, but the thickness will become thinner, and the force will still decrease. Therefore, it is necessary to adjust the pressure of the cylinder to 200kg / cm according to the product requirements. 3 When the pressure drops, adjust the cylinder pressure specifically.

[0132] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is heated and vulcanized while being strongly shaped by the pressure. During this period, the pressure needs to be maintained at 180-220kg / cm 3 The temperature is kept at about 105-115℃ for about 10 minutes. The specific time is determined by the thickness and density of the product.

[0133] After the latex solidified material is vulcanized, a pressed edge latex mold cup product can be obtained. After leaching, drying and drying, a mold cup blank of a pressed edge latex mold cup is obtained, and after cutting with a mold cup knife or scissors, a pressed edge latex mold cup product is completed.

[0134] In one embodiment, the hot water leaching in step S06 is performed by soaking and leaching in 50-80° C. hot water for 1-5 minutes.

[0135] In one embodiment, the drying in step S06 is spin drying and / or drying.

[0136] The invention provides a process for preparing an edge-pressed latex mold cup without using sodium fluorosilicate as a gelling agent.

[0137] A pressed edge latex mold cup is prepared by adopting the method for preparing the pressed edge latex mold cup as described above.

[0138] like Figure 2 As shown, a latex mold cup with edge pressing prepared by edge pressing process comprises a natural latex foam body 21, a crease part 22, an edge pressing part 23 and a surrounding edge pressing part 24. The natural latex foam body 21 is the main body of the mold cup, and its thickness, curvature and overall shape determine the effect of the cup shape; the crease part 22 locates the boundary of the overall mold cup; the edge pressing part 23 cooperates with the crease part 22 to accurately locate the placed steel ring or strapping strip, and the effect is that it is fixed to the edge pressing part 23 by sewing or gluing, so that the force is more concentrated on the chest; the surrounding edge pressing part 24 is the four sides of the mold cup, and the thickness of the edge pressing part 23 and the surrounding edge pressing part 24 is less than 1mm. Through sewing positioning, it can effectively receive the lifting and gathering force, thereby solving the problem of sewing positioning of the latex mold cup.

[0139] An application of the edge-pressed latex mold cup in a natural latex bra.

[0140] The edge-pressed latex mold cup is fixed in the cup by sewing, gluing, inserting and the like to obtain a edge-pressed latex mold cup bra.

[0141] like Figure 3 As shown, a natural latex bra comprises the pressed-edge latex mold cup 35 as described above, including a left cup 31 and a right cup 32 consisting of an upper and lower bowl, and a back ratio and other accessories 33 for connecting the left cup 31 and the right cup 32, and two shoulder straps 34 connected to the two cups and the back ratio 33. The latex mold cups in the left cup 31 and the right cup 32 (or the combination of 31 and 32) are all pressed-edge latex mold cups.

[0142] The edge-pressed latex mold cup provided by the present invention adopts all-healthy additives and does not contain toxic substances such as sodium fluorosilicate. The product is healthier and more suitable for skin-friendly use, especially for delicate breast skin of women. It has a very high plastic deformation retention rate, and has good elasticity and strength. The bra made from it is easy to contain and support the breasts to adapt to breast shaking, conform to the strain and slippage of the skin, and is beneficial to shaping and correcting the breast shape of women. The edge-pressed natural latex mold cup of the present invention has good mechanical properties, and has excellent mechanical properties such as a good steel ring-free supporting part, a gathered force-bearing part, a supporting force-bearing part and a lifting force-bearing part. Secondly, the present invention creates a new process method, and obtains latex foam sponges of different densities from the same latex foaming material, which is not limited to the underwear industry, and more foaming products can be processed more simply because of this process.

[0143] The present invention is specifically described below by way of examples. In addition, unless otherwise specified, all raw materials used are commercially available.

[0144] In the examples, the styrene-butadiene rubber was provided by PetroChina Lanzhou Petrochemical Company, with the grade of SBR1502.

[0145] The nitrogen content of the natural rubber in the embodiment is 0.5 wt %, provided by Hainan Natural Rubber Industry Group Co., Ltd., and the product name is SCRWF.

[0146] The zinc oxide in the embodiment is an indirect method zinc oxide provided by Shijiazhuang Youchang Chemical Technology Co., Ltd., model: 99.7, product grade: superior grade, sieve residue (45 micron mesh) ≤ 0.1wt%.

[0147] The organopolysiloxane in the examples is Coagulant WS from LANXESS, Germany.

[0148] In the embodiment, the arylethylphenyl polyethylene glycol ether is Emulvin WA from LANXESS, Germany.

[0149] In the examples, polyethylene glycol p-isooctylphenyl ether was provided by Jiangsu Haian Petrochemical Plant, model number: Triton X-100.

[0150] Example

[0151] Example 1

[0152] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0153] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0154] S02: spraying latex foam onto a carrier;

[0155] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0156] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0157] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0158] S06: hot water leaching and drying.

[0159] In step S01, the raw material latex is natural rubber.

[0160] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0161] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0162] The vulcanizing agent is sulfur.

[0163] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0164] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0165] The activator is zinc oxide.

[0166] The foaming agent is potassium oleate.

[0167] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0168] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0169] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0170] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0171] In the step S03, the gelling agent is organopolysiloxane.

[0172] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0173] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 200kg / cm 3 .

[0174] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the temperature of the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 200kg / cm 3 .

[0175] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 200kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0176] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0177] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0178] Example 2

[0179] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0180] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0181] S02: spraying latex foam onto a carrier;

[0182] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0183] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0184] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0185] S06: hot water leaching and drying.

[0186] In step S01, the raw material latex is natural rubber.

[0187] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0188] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0189] The vulcanizing agent is sulfur.

[0190] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0191] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0192] The activator is zinc oxide.

[0193] The foaming agent is potassium oleate.

[0194] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0195] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0196] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0197] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0198] In the step S03, the gelling agent is obtained by mixing organic polysiloxane and aryl ethyl phenyl polyethylene glycol ether in a mass ratio of 1:0.15.

[0199] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0200] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 200kg / cm 3 .

[0201] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the temperature of the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 200kg / cm 3 .

[0202] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 200kg / cm3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0203] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0204] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0205] Example 3

[0206] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0207] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0208] S02: spraying latex foam onto a carrier;

[0209] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0210] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0211] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0212] S06: hot water leaching and drying.

[0213] In step S01, the raw material latex is natural rubber.

[0214] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0215] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0216] The vulcanizing agent is sulfur.

[0217] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0218] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0219] The activator is zinc oxide.

[0220] The foaming agent is potassium oleate.

[0221] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0222] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0223] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0224] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0225] In the step S03, the gelling agent is obtained by mixing organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether in a mass ratio of 1:0.15:0.05.

[0226] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0227] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 200kg / cm 3 .

[0228] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the temperature of the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 200kg / cm 3 .

[0229] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 200kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0230] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0231] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0232] Example 4

[0233] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0234] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0235] S02: spraying latex foam onto a carrier;

[0236] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0237] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0238] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0239] S06: hot water leaching and drying.

[0240] In step S01, the raw latex is obtained by mixing 70 wt % of natural rubber and 30 wt % of styrene-butadiene rubber.

[0241] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0242] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0243] The vulcanizing agent is sulfur.

[0244] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0245] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0246] The activator is zinc oxide.

[0247] The foaming agent is potassium oleate.

[0248] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0249] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0250] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0251] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0252] In the step S03, the gelling agent is obtained by mixing organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether in a mass ratio of 1:0.15:0.05.

[0253] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0254] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 200kg / cm 3 .

[0255] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the temperature of the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 200kg / cm 3 .

[0256] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 200kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0257] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0258] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0259] Comparative Example 1

[0260] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0261] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0262] S02: spraying latex foam onto a carrier;

[0263] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0264] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0265] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0266] S06: hot water leaching and drying.

[0267] In step S01, the raw material latex is natural rubber.

[0268] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0269] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0270] The vulcanizing agent is sulfur.

[0271] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0272] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0273] The activator is zinc oxide.

[0274] The foaming agent is potassium oleate.

[0275] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0276] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0277] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0278] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0279] In step S03, the gelling agent is sodium fluorosilicate.

[0280] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0281] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 200kg / cm 3 .

[0282] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the temperature of the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 200kg / cm 3.

[0283] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 200kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0284] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0285] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0286] Comparative Example 2

[0287] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0288] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0289] S02: spraying latex foam onto a carrier;

[0290] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0291] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0292] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0293] S06: hot water leaching and drying.

[0294] In step S01, the raw material latex is natural rubber.

[0295] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0296] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0297] The vulcanizing agent is sulfur.

[0298] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0299] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0300] The activator is zinc oxide.

[0301] The foaming agent is potassium oleate.

[0302] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0303] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0304] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0305] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0306] In the step S03, the gelling agent is obtained by mixing organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether in a mass ratio of 1:0.15:0.15.

[0307] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0308] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 200kg / cm 3 .

[0309] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the temperature of the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 200kg / cm 3 .

[0310] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 200kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0311] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0312] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0313] Comparative Example 3

[0314] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0315] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0316] S02: spraying latex foam onto a carrier;

[0317] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0318] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0319] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0320] S06: hot water leaching and drying.

[0321] In step S01, the raw material latex is natural rubber.

[0322] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0323] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0324] The vulcanizing agent is sulfur.

[0325] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0326] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0327] The activator is zinc oxide.

[0328] The foaming agent is potassium oleate.

[0329] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0330] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0331] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0332] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0333] In the step S03, the gelling agent is obtained by mixing organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether in a mass ratio of 1:0.15:0.05.

[0334] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0335] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 100kg / cm 3 .

[0336] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 100kg / cm 3 .

[0337] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 100kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0338] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0339] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0340] Comparative Example 4

[0341] A method for preparing a pressed edge latex mold cup comprises the following steps:

[0342] S01: mixing the raw latex and the dispersion, and frothing them with mechanical stirring at a speed of 900 r / min for 10 min to obtain latex foam;

[0343] S02: spraying latex foam onto a carrier;

[0344] S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 70° C. for 10 minutes to obtain a latex solid;

[0345] S04: transferring the latex solidified material into a cup mold of a vulcanizing machine;

[0346] S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid;

[0347] S06: hot water leaching and drying.

[0348] In step S01, the raw material latex is natural rubber.

[0349] The mass ratio of the raw latex to the dispersion in step S01 is 9:1.

[0350] In step S01, the dispersion includes 2 parts by weight of a vulcanizing agent, 1 part by weight of an accelerator, 2.5 parts by weight of an antioxidant, 1.2 parts by weight of an activator, and 1.5 parts by weight of a foaming agent. The dispersion is obtained by mixing the raw materials.

[0351] The vulcanizing agent is sulfur.

[0352] The accelerator is obtained by mixing 2-mercaptobenzothiazole and zinc dibenzyldithiocarbamate in a mass ratio of 1:0.25.

[0353] The antioxidant is 4,4'-bis(α,α-dimethylbenzyl)diphenylamine.

[0354] The activator is zinc oxide.

[0355] The foaming agent is potassium oleate.

[0356] In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance, and the anti-adhesion substance is Teflon.

[0357] In step S02, the carrier is a stainless steel plate, and the length of the stainless steel plate is 300 mm and the width is 200 mm.

[0358] In the step S02, the thickness of the latex foam sprayed on the carrier is 5 mm.

[0359] The amount of the gelling agent added in step S03 is 3.2% of the weight of the raw latex.

[0360] In the step S03, the gelling agent is obtained by mixing organic polysiloxane, aryl ethyl phenyl polyethylene glycol ether, and polyethylene glycol p-isooctyl phenyl ether in a mass ratio of 1:0.15:0.05.

[0361] The cup mold used in step S04 is a mold commonly used in the cup mold industry for hot pressing of existing polyurethane sponges.

[0362] In step S05, the temperature of the vulcanizer is heated to 110°C and the pressure is adjusted to 300kg / cm 3 .

[0363] The vulcanizer in step S05 is composed of an upper mold 1, a lower mold 2, an upper heating plate 4, a lower heating plate 5 and a pressure cylinder 3. The mold heating plate is heated to 110°C, driving the upper and lower molds to 110°C. The mold material is aluminum. The cylinder pressure is 300kg / cm 3 .

[0364] Move the latex solidified material into Figure 1 In the lower mold 2 of the vulcanizer shown in the figure, the pressure cylinder 3 drives the upper mold 1 to close the mold and pressurize and heat it. During this process, the latex solidified material is strongly shaped by the pressure while also being heated and vulcanized. During this period, the pressure needs to be maintained at 300kg / cm 3 , the temperature was maintained at 110°C and the holding time was 10 minutes.

[0365] The hot water leaching in step S06 is performed by soaking and leaching in 70° C. hot water for 3 minutes.

[0366] In step S06, the drying is performed by first spinning and then drying; the drying temperature is 50° C. and the drying time is 5 hours.

[0367] Performance Evaluation

[0368] The latex solidified product prepared in step S03 of Example 1-3 and Comparative Example 1-2 was subjected to conventional molding and hot vulcanization processes to obtain a foamed latex precision product; the molding was a compression molding method, and the molding machine pressure used in the compression molding was 0.6 MPa; the hot vulcanization temperature was 110° C. The foamed latex precision product was subjected to air permeability test and aging resistance test. The specific test results are shown in Table 1.

[0369] Air permeability test

[0370] According to the standard of GB / T 7755-2003 / ISO2782:1995 "Determination of air permeability of vulcanized rubber or thermoplastic rubber", the air permeability of the edge-pressed latex mold cup prepared by the method provided in the examples and comparative examples of the present application was tested (unit: cm 3 / cm 2 Each sample was tested three times in parallel and the average value was taken.

[0371] Aging resistance test

[0372] The test was carried out in accordance with GB / T 3512-2001 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber", and the test conditions were 90℃×72h. Each sample was tested three times in parallel and the average value was taken.

[0373] Performance evaluation

[0374] The edge-pressed latex mold cups provided in Examples 1-3 and Comparative Examples 1-4 of the present invention were placed in bra cups, and steel rings were placed at the edge-pressed outlets and sewn to prepare natural latex bras. The performance was evaluated based on whether the edge was prone to rotten edges during wearing and washing, and a score of 1 to 10 was given, where 10 points were the best performance and 1 point was the worse performance. The specific test results are shown in Table 1.

[0375] Table 1: Test results

[0376]

[0377] Note: “ / ” in the table means that the test was not performed.

[0378] The above is only a preferred embodiment of the present invention and is not intended to limit the invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a pressed edge latex mold cup, characterized in that: The following steps are involved: S01: mixing the raw latex and the dispersion, stirring and foaming to obtain latex foam; S02: spraying latex foam onto a carrier; S03: adding a gelling agent to the latex foam sprayed on the carrier, and then keeping the temperature at 65-75° C. for 5-15 minutes to obtain a latex solid; S04: transferring the latex solidified material into a cup mold of a vulcanizing machine; S05: The vulcanizer heats and presses the latex solid to press, shape and vulcanize the latex solid; S06: hot water leaching, drying; The amount of the gelling agent added in step S03 is 2.8-3.6% of the weight of the raw latex; In the step S03, the gelling agent is composed of organopolysiloxane, Emulvin WA from LANXESS, Germany, and polyethylene glycol p-isooctylphenyl ether in a mass ratio of 1: (0.1-0.2): (0.04-0.06); In step S05, the temperature of the vulcanizer is heated to 90-115°C and the pressure is adjusted to 180-220 kg / cm 2 ; The hot water leaching in step S06 is performed by soaking and leaching in 50-80° C. hot water for 1-5 minutes; In step S01, the raw material latex is natural rubber and / or synthetic rubber; The nitrogen content in the natural rubber is 0.1-0.6 wt %.

2. The method for preparing the edge-pressed latex mold cup according to claim 1, characterized in that: The dispersion in step S01 includes a vulcanizing agent, an accelerator, an antioxidant, an activator, and a foaming agent.

3. The method for preparing the edge-pressed latex mold cup according to claim 2, characterized in that: In the step S02, the surface of the carrier is sprayed with an anti-adhesion substance; in the step S02, the carrier is a stainless steel plate or an assembly line conveyor belt.

4. A method for preparing a pressed edge latex mold cup according to claim 3, wherein the pressed edge latex mold cup is used in a natural rubber latex bra.

Citation Information

Patent Citations

  • Pure natural latex mould cup and preparation process thereof

    CN109627486A

  • All-in-one natural latex bra cups, and preparation method thereof

    CN109880191A

  • Edge-pressing latex mold cup and edge-pressing latex mold cup bra

    CN210329386U