Quantum dots, methods for making the same, and compositions, composites, and electronic devices comprising the same

By preparing cadmium-free III-V group compound quantum dots and controlling their core-shell structure and synthesis process, the problems of insufficient color reproduction and luminous efficiency of existing cadmium quantum dots in display devices have been solved, achieving high-efficiency color reproduction and narrow emission peaks, making them suitable for next-generation display devices.

CN110746958BActive Publication Date: 2024-10-01SAMSUNG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910665612.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-23
Filing Date
2019-07-23
Publication Date
2024-10-01
Estimated Expiration
2039-07-23

AI Technical Summary

Technical Problem

Existing cadmium-based quantum dots, when applied to display devices, struggle to simultaneously achieve the desired color reproduction and improved electroluminescence properties, especially under the next-generation BT2020 standard, where issues arise regarding insufficient color mixing and luminous efficiency.

Method used

By using cadmium-free III-V compound quantum dots and controlling the composition and thickness of the core and shell, combined with appropriate synthesis methods, including multiple additions of group V element precursors and additives, quantum dots with low defects, narrow emission peaks and high quantum efficiency were prepared.

Benefits of technology

It achieves improved color reproducibility and color purity in display devices without color filters, reaching or exceeding 80% of the BT2020 standard in color reproducibility, while maintaining high quantum efficiency and narrow emission peak half-width.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110746958B_ABST
    Figure CN110746958B_ABST
Patent Text Reader

Abstract

Quantum dots, methods for making the same, and compositions, composites, and electronic devices comprising the same, the quantum dots comprising a semiconductor nanocrystal core and a semiconductor nanocrystal shell disposed on the core, the quantum dots excluding cadmium, wherein the core comprises a III-V group compound, the quantum dots having a maximum photoluminescence peak in the green light wavelength region, a full width at half maximum (FWHM) of the maximum photoluminescence peak of less than about 50 nanometers (nm), and a difference between the wavelength of the maximum photoluminescence peak and the first absorption peak wavelength of the quantum dots of less than or equal to about 25 nanometers.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2018-0085495 filed in the Korean Intellectual Property Office on Jul. 23, 2018, and all rights arising therefrom, the entire contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] Disclosed are quantum dots, methods for making the same, and composites and electronic devices comprising the same. Background Art

[0004] Quantum dots (i.e., nanometer-sized semiconductor nanocrystals) can have different band gaps by varying the size and composition of the nanocrystals, and can therefore emit light of various photoluminescence wavelengths. Quantum dots can exhibit electroluminescent properties. The photoluminescent properties of quantum dots can be applied in a variety of fields. The development of quantum dots that can exhibit improved electroluminescent properties and do not include heavy metals (e.g., cadmium, lead, etc.) is desirable. Summary of the invention

[0005] Embodiments provide quantum dots or clusters of quantum dots that can exhibit improved electroluminescent properties.

[0006] Embodiments provide methods of manufacturing the quantum dots.

[0007] An embodiment provides a composition including the quantum dots.

[0008] An embodiment provides a quantum dot-polymer composite including the quantum dots.

[0009] An embodiment provides an electronic device including the quantum dots.

[0010] In one embodiment, a quantum dot includes a semiconductor nanocrystal core and a semiconductor nanocrystal shell disposed on the core, and does not include cadmium. In the quantum dot, the core includes a III-V compound including a III metal and a V element (e.g., a compound including indium and phosphorus), the quantum dot has a maximum photoluminescence peak in a green light wavelength region, a full width at half maximum (FWHM) of the maximum photoluminescence peak is less than about 50 nanometers (nm), and a difference between the wavelength of the maximum photoluminescence peak and the first absorption peak wavelength of the quantum dot (hereinafter, also referred to as Stokes shift) is less than or equal to about 25 nm.

[0011] The green light wavelength region may be greater than or equal to about 500 nm and less than or equal to about 560 nm.

[0012] The full width at half maximum (FWHM) of the maximum photoluminescence peak may be less than or equal to about 35 nm.

[0013] The FWHM of the maximum photoluminescence peak may be less than or equal to about 34 nm.

[0014] The FWHM of the maximum photoluminescence peak may be less than or equal to about 33 nm.

[0015] The quantum dots may include indium and zinc.

[0016] The quantum dots may have a size greater than or equal to about 1.5 nm.

[0017] The quantum dots may have a quantum efficiency (quantum yield) of greater than or equal to about 80%.

[0018] The quantum dot may further include an additive (eg, in the core) including a Group IV element, As, Sb, Bi, Te, or a combination thereof. The Group IV element may include tin (Sn).

[0019] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal (eg, indium) may be less than or equal to about 0.1 mole.

[0020] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.08 mole.

[0021] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.05 mole.

[0022] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.03 mole.

[0023] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.025 mole.

[0024] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.02 mole.

[0025] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.01 mole.

[0026] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be less than or equal to about 0.005 mole.

[0027] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be greater than or equal to about 0.0001.

[0028] In the quantum dot, a molar amount of the additive relative to 1 mole of the Group III metal may be greater than or equal to about 0.001.

[0029] The shell may include a first semiconductor nanocrystalline shell including zinc and selenium and a second semiconductor nanocrystalline shell disposed on the first semiconductor nanocrystalline shell, and the second semiconductor nanocrystalline shell may include zinc and sulfur.

[0030] The first semiconductor nanocrystal shell may be disposed directly on a surface of the semiconductor nanocrystal core and the first semiconductor nanocrystal shell may not include sulfur.

[0031] The first semiconductor nanocrystalline shell may have a thickness greater than or equal to about 1 monolayer, greater than or equal to about 2 monolayers, or greater than or equal to 3 monolayers. The first semiconductor nanocrystalline shell may have a thickness less than or equal to about 10 monolayers.

[0032] In embodiments, the first semiconductor nanocrystal shell may have a thickness of less than or equal to about 1 monolayer, or may have a thickness of less than or equal to about 0.5 monolayer.

[0033] The first semiconductor nanocrystal shell may have a thickness of less than or equal to about 1 nm, such as less than or equal to about 0.9 nm, less than or equal to about 0.8 nm, less than or equal to about 0.7 nm, or less than or equal to about 0.65 nm.

[0034] The second semiconductor nanocrystal shell may be the outermost layer of the quantum dot.

[0035] The second semiconductor nanocrystalline shell may be disposed directly on the first semiconductor nanocrystalline shell.

[0036] The second semiconductor nanocrystal shell may include ZnSeS, ZnS, or a combination thereof.

[0037] The second semiconductor nanocrystal shell may have a varying composition in a radial direction.

[0038] The second semiconductor nanocrystal shell may have a concentration gradient of sulfur that increases toward a surface of the quantum dot.

[0039] The second semiconductor nanocrystal shell may have a thickness of less than or equal to about 1 nm, such as less than or equal to about 0.9 nm, less than or equal to about 0.8 nm, less than or equal to about 0.7 nm, or less than or equal to about 0.65 nm.

[0040] The core may include indium, phosphorus, and optionally zinc, and the shell may include zinc, sulfur, and selenium.

[0041] In the quantum dots, a molar ratio of sulfur and selenium to indium may be greater than or equal to about 20: 1 and less than or equal to about 36: 1. In the quantum dots, a molar ratio of phosphorus to indium may be greater than or equal to about 0.6: 1 and less than or equal to about 0.9: 1. In the quantum dots, a molar ratio of zinc to indium may be greater than or equal to about 25: 1 and less than or equal to about 40: 1.

[0042] A difference between a wavelength of the maximum photoluminescence peak and a first absorption peak wavelength of the quantum dots may be less than or equal to about 22 nm.

[0043] A difference between a wavelength of the maximum photoluminescence peak and a first absorption peak wavelength of the quantum dots may be less than or equal to about 20 nm.

[0044] In the photoluminescence spectrum of the quantum dot, a ratio of a tail area of ​​a photoluminescence spectrum curve to a total area may be less than or equal to about 10%.

[0045] In the photoluminescence spectrum of the quantum dot, a ratio of an intensity at a tail start wavelength (eg, about 580 nm) to an intensity at a maximum photoluminescence peak wavelength may be less than or equal to about 0.12:1.

[0046] In the photoluminescence spectrum of the quantum dot, a ratio of an intensity at a tail start wavelength to an intensity at a maximum photoluminescence peak wavelength may be less than or equal to about 0.11:1.

[0047] In the photoluminescence spectrum of the quantum dot, a ratio of an intensity at a tail start wavelength to an intensity at a maximum photoluminescence peak wavelength may be less than or equal to about 0.1:1.

[0048] In the photoluminescence spectrum of the quantum dot, a ratio of an intensity at a tail start wavelength to an intensity at a maximum photoluminescence peak wavelength may be less than or equal to about 0.095:1.

[0049] In the photoluminescence spectrum of the quantum dot, a ratio of an intensity at a tail initial wavelength to an intensity at a maximum photoluminescence peak wavelength may be less than or equal to about 0.09:1.

[0050] In an embodiment, a method of making the above-mentioned quantum dots comprises,

[0051] obtaining (e.g., preparing) a semiconductor nanocrystal core comprising a Group III-V compound comprising a Group III metal and a Group V element;

[0052] preparing a first solution including a shell metal precursor and an organic ligand;

[0053] adding the semiconductor nanocrystal cores to the first solution at a first temperature; and

[0054] heating the first solution including the semiconductor nanocrystal core to a second temperature and adding a shell non-metal precursor to the first solution to form a semiconductor nanocrystal shell on the surface of the semiconductor nanocrystal core and to produce the quantum dot,

[0055] Wherein the first temperature is less than or equal to about 150°C, and the second temperature is greater than or equal to about 250°C, for example, greater than or equal to about 260°C, greater than or equal to about 270°C, greater than or equal to about 280°C, or greater than or equal to about 290°C and less than or equal to about 350°C.

[0056] The semiconductor nanocrystal core may further include an additive including a Group IV element, As, Sb, Bi, Te, or a combination thereof.

[0057] The Group IV element may include tin.

[0058] The first temperature may be less than or equal to about 120°C.

[0059] The second temperature may be greater than or equal to about 300°C and less than or equal to about 330°C.

[0060] The formation of the semiconductor nanocrystal shell may include adding the shell non-metal precursor and optional shell metal precursor to the first solution at least twice.

[0061] During the preparation of the semiconductor nanocrystal core and / or the formation of the shell, a Group V element precursor (eg, a phosphorus precursor) may be added at least twice (eg, injected in a separate manner).

[0062] The method may include adding additional precursors to the first solution during the formation of the semiconductor nanocrystal shell, the preparation of the semiconductor nanocrystal core, or a combination thereof.

[0063] The additional precursor may include ammonium fluoride, a precursor comprising the above-mentioned additives, or a combination thereof.

[0064] The method may further include adding ammonium fluoride, a Group IV element, or a combination thereof to the first solution during formation of the semiconductor nanocrystal shell.

[0065] The amount of the additional precursor may be greater than or equal to about 0.001 mol and less than or equal to about 0.1 mol per 1 mol of the Group III metal.

[0066] In an embodiment, the quantum dot-polymer composite comprises: a polymer matrix (matrix); and a plurality of quantum dots dispersed in the polymer matrix,

[0067] The plurality of quantum dots may include the aforementioned quantum dots (or a group thereof).

[0068] The polymer matrix may include a cross-linked polymer, a binder polymer having carboxylic acid groups, or a combination thereof.

[0069] The cross-linked polymer may include a polymerization product of a photopolymerizable monomer including a carbon-carbon double bond, a polymerization product of the photopolymerizable monomer and a polythiol compound having at least two thiol groups at a terminal, or a combination thereof.

[0070] The quantum dot-polymer composite may further include metal oxide fine particles in the polymer matrix.

[0071] The quantum dot-polymer composite may be in the form of a film having a thickness greater than or equal to about 1 micrometer (μm) and less than or equal to about 200 μm.

[0072] The quantum dot polymer composite may be configured to emit light having a photoluminescence peak half-width less than or equal to about 38 nm.

[0073] The photoluminescence peak half width may be less than or equal to about 37 nm.

[0074] The photoluminescence peak half width may be less than or equal to about 36 nm.

[0075] The photoluminescence peak half width may be less than or equal to about 35 nm.

[0076] The photoluminescence peak half width may be less than or equal to about 34 nm.

[0077] The quantum dot polymer composite may be configured to emit light having a Cy greater than or equal to about 0.23 and less than or equal to about 0.24 in color coordinates.

[0078] The quantum dot polymer composite may be configured to emit light having a Cx greater than or equal to about 0.18 and less than or equal to about 0.19 in color coordinates.

[0079] In an embodiment, a display device includes a light source and a photoluminescent element, wherein the photoluminescent element includes the above-mentioned quantum dots or the above-mentioned quantum dot-polymer composite, and the light source is configured to provide incident light to the photoluminescent element.

[0080] The incident light may have a photoluminescence peak wavelength of about 440 nm to about 460 nm.

[0081] The photoluminescent element may include a sheet of the quantum dot-polymer composite.

[0082] The display device may further include a liquid crystal panel, and

[0083] The sheet of the quantum dot polymer composite may be disposed between the light source and the liquid crystal panel.

[0084] The photoluminescent element is a stack structure including a substrate and a light-emitting layer disposed on the substrate, wherein the light-emitting layer includes a pattern of the quantum dot polymer composite and the pattern includes at least one repeating segment emitting light of a predetermined wavelength.

[0085] The display device may be configured to have a color reproducibility greater than or equal to about 80% under the standard of BT2020.

[0086] The display device may be configured to have a color reproducibility greater than or equal to about 85% under the standard of BT2020. The display device may be configured to have a color reproducibility greater than or equal to about 88% under the standard of BT2020. The display device may be configured to have a color reproducibility greater than or equal to about 90% under the standard of BT2020.

[0087] The display device may not include a color filter (eg, blocking red light and / or green light).

[0088] The pattern may include a first segment that emits a first type of light and a second segment that emits a second type of light having a different central wavelength than the first type of light.

[0089] The light source may include a plurality of light emitting cells corresponding to each of the first segment and the second segment, wherein a first electrode and a second electrode face the light emitting cells and an electroluminescent layer is disposed between the first electrode and the second electrode.

[0090] The display device may further include a lower substrate, a polarizer disposed under the lower substrate, and a liquid crystal layer disposed between the stack structure and the lower substrate, wherein the stack structure is disposed so that the light emitting layer faces the liquid crystal layer.

[0091] The display device may further include a polarizer between the liquid crystal layer and the light emitting layer.

[0092] The light source may include a light emitting diode (LED) and optionally a light guide.

[0093] Quantum dots according to embodiments may emit green light with improved electroluminescent properties. Quantum dots according to embodiments may be used in a variety of display devices and biomarkers (e.g., biosensors, bioimaging, etc.), photodetectors, solar cells, hybrid composite materials, etc. A display device including quantum dots according to embodiments may exhibit improved display quality (e.g., improved color reproducibility under the next generation color standard BT2020 benchmark). BRIEF DESCRIPTION OF THE DRAWINGS

[0094] Figure 1A is an exploded view of a display device according to an embodiment.

[0095] Figure 1B is a cross-sectional view of a display device according to an embodiment.

[0096] Figure 2 A process of manufacturing a quantum dot-polymer composite pattern using a composition according to an embodiment is shown.

[0097] Figure 3A and 3B is a schematic cross-sectional view of a display device according to an embodiment.

[0098] Figure 4 is a cross-sectional view of a display device according to an embodiment.

[0099] Figure 5 is a graph of absorption / photoluminescence (PL) intensity (arbitrary units (au)) versus wavelength (nm), showing the photoluminescence spectrum and ultraviolet-visible (UV-Vis) spectrum of the quantum dots synthesized in Example 1.

[0100] Figure 6 is a graph of absorption / PL intensity (au) versus wavelength (nm), showing the photoluminescence spectrum and UV-Vis spectrum of the quantum dots synthesized in Example 2.

[0101] Figure 7 : is a graph of PL intensity (Int.) (normalized (norm.)) versus wavelength (nm), which shows the photoluminescence spectra of the quantum dots of Example 2 and Comparative Example 1.

[0102] Figure 8 FIG. 5 is a graph showing the color reproducibility simulation results of the quantum dot-polymer composite of the example under the BT2020 standard. DETAILED DESCRIPTION

[0103] With reference to the following example embodiments together with the accompanying drawings attached hereto, the advantages and characteristics of the present disclosure, and the methods for realizing the same will become clear. However, the embodiments should not be construed as being limited to the embodiments set forth herein. If not otherwise defined, all terms (including technical and scientific terms) in this specification may be defined as commonly understood by those skilled in the art. The terms defined in the common dictionary may not be interpreted ideally or exaggeratedly, unless clearly defined. In addition, unless explicitly described to the contrary, the wording "including (comprising)" is understood to imply the inclusion of the stated elements, but does not exclude any other elements.

[0104] Furthermore, the singular includes the plural unless otherwise mentioned.

[0105] Like reference numerals refer to like elements throughout.

[0106] It will be understood that when an element is referred to as being “on” another element, it can be directly in contact with the other element or intervening elements may exist therebetween. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements.

[0107] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings herein, the "first element", "component", "region", "layer" or "part" discussed below may be referred to as a second element, component, region, layer or part.

[0108] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0109] In addition, relative terms such as "lower" or "bottom" and "upper" or "top" may be used herein to describe the relationship of one element to another element as shown in the figure. It will be understood that in addition to the orientations depicted in the figures, relative terms are also intended to cover different orientations of the device. For example, if the device in one of the figures is turned over, the element described as being on the "lower" side of the other element will be oriented on the "upper" side of the other element. Therefore, depending on the specific orientation of the figure, the exemplary term "lower" can cover both "lower" and "upper" orientations. Similarly, if the device in one of the figures is turned over, the element described as "below" or "below" the other element will be oriented "above" the other element. Therefore, the exemplary terms "below..." or "below..." can cover both "above..." and "below..." orientations.

[0110] As used herein, "about" includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" may mean that the deviation from the stated value is within one or more standard deviations, or within ±10% or 5%.

[0111] Exemplary embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. Thus, deviations from the shapes of the figures as a result of, for example, manufacturing techniques and / or tolerances are expected. Thus, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as shown herein, but rather include deviations in shape resulting from, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. In addition, the illustrated sharp corners may be rounded. Thus, the regions shown in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions, and are not intended to limit the scope of the claims.

[0112] As used herein, when no definition is otherwise provided, "substituted" refers to a compound or group in which a hydrogen is replaced by a C1-C30 alkyl, C2-C30 alkenyl, C2-C30 alkynyl, C6-C30 aryl, C7-C30 alkaryl, C1-C30 alkoxy, C1-C30 heteroalkyl, C3-C40 heteroaryl, C3-C30 heteroalkaryl, C3-C30 cycloalkyl, C3-C15 cycloalkenyl, C6-C30 cycloalkynyl, C2-C30 heterocycloalkyl, halogen (-F, -Cl, -Br, or -I), hydroxyl (-OH), nitro (-NO), or 2 ), thiocyanate (-SCN), cyano (-CN), amino (-NRR', wherein R and R' are independently hydrogen or C1-C6 alkyl), azido (-N 3 ), amidino (-C(=NH)NH 2 ), hydrazino (-NHNH 2 ), hydrazone (=N(NH 2 )), aldehyde group (-C(=O)H), carbamoyl group (-C(O)NH 2 ), thiol group (-SH), ester group (-C(=O)OR, wherein R is C1-C6 alkyl or C6-C12 aryl), carboxyl group (-COOH) or its salt (-C(=O)OM, wherein M is an organic or inorganic cation), sulfonic acid group (-SO 3 H) or its salt (-SO 3 M, where M is an organic or inorganic cation), a phosphate group (-PO3 H 2 ) or its salt (-PO 3 MH or -PO 3 M 2 , wherein M is an organic or inorganic cation), or a combination thereof.

[0113] As used herein, when no definition is otherwise provided, the term "hetero" refers to a heteroatom including one to three, wherein the heteroatom may be N, O, S, Si, or P.

[0114] As used herein, when a definition is not otherwise provided, "aliphatic" refers to a C1-C30 linear or branched alkyl, alkenyl or alkynyl group.

[0115] As used herein, when a definition is not otherwise provided, "aromatic" refers to a C6-C30 aryl group or a C2-C30 heteroaryl group.

[0116] As used herein, when a definition is not otherwise provided, "heteroaryl" refers to an aromatic group that includes at least one heteroatom covalently bonded to one or more carbon atoms of an aromatic ring.

[0117] As used herein, when no definition is otherwise provided, “alicyclic” may refer to a C3-C30 cycloalkyl group, a C3-C30 cycloalkenyl group, or a C3-C30 cycloalkynyl group.

[0118] As used herein, when no definition is otherwise provided, "(meth)acrylate" refers to acrylate, methacrylate, or a combination thereof.

[0119] As used herein, when no definition is provided in addition, "hydrophobic moiety" refers to a moiety that provides a tendency for the corresponding compound to agglomerate in an aqueous solution and repel water. For example, the hydrophobic moiety may include an aliphatic hydrocarbon group (alkyl, alkenyl, alkynyl, etc.) with a carbon number of 1 or more (e.g., 2 or more, 3 or more, 4 or more, or 5 or more), an aromatic hydrocarbon group (phenyl, naphthyl, alkaryl, etc.) with a carbon number of 6 or more, or an alicyclic hydrocarbon group (cyclohexyl, norbornene group, norbornane group, tricyclodecane group, etc.) with a carbon number of 5 or more.

[0120] As used herein, "dispersion" refers to a dispersion in which the dispersed phase is solid and the continuous phase comprises a liquid. For example, "dispersion" may refer to a colloidal dispersion in which the dispersed phase has a size greater than or equal to about 1 nm, such as greater than or equal to about 2 nm, greater than or equal to about 3 nm, or greater than or equal to about 4 nm and a few microns (μm) or less (e.g., less than or equal to about 2 μm, less than or equal to about 1 μm, or less than or equal to about 0.5 μm).

[0121] As used herein, the term "Group" refers to a Group of the Periodic Table.

[0122] As used herein, “Group I” refers to Group IA and Group IB, and examples may include Li, Na, K, Rb, and Cs, but are not limited thereto.

[0123] As used herein, “Group II” refers to Group IIA and Group IIB, and examples of Group II metals may be Cd, Zn, Hg, and Mg, but are not limited thereto.

[0124] As used herein, “Group III” refers to Group IIIA and Group IIIB, and examples of Group III metals may be Al, In, Ga, and Tl, but are not limited thereto.

[0125] As used herein, "Group IV" refers to Group IVA and Group IVB, and examples of Group IV metals may be Si, Ge, and Sn, but are not limited thereto. As used herein, the term "metal" may include semimetals such as Si.

[0126] As used herein, “Group V” refers to Group VA, and examples may include nitrogen, phosphorus, arsenic, antimony, and bismuth, but are not limited thereto.

[0127] As used herein, "Group VI" refers to Group VIA, and examples may include sulfur, selenium, and tellurium, but are not limited thereto.

[0128] As used herein, "tail" refers to the portion of the photoluminescence spectrum curve that exists in the following wavelength region: at least 40 nm (e.g., at least 41 nm, at least 42 nm, at least 43 nm, at least 44 nm, at least 45 nm, at least 46 nm, at least 47 nm, at least 48 nm, at least 49 nm, or at least 50 nm) greater than the maximum photoluminescence peak wavelength. The tail start wavelength is the wavelength at which the tail begins.

[0129] As used herein, "monolayer" is a unit of measure for shell thickness. A monolayer can be calculated as the closest distance between relevant lattice planes (e.g., the distance between adjacent lattice planes in the

[111] direction) from the bulk (bulk crystal) structure (cubic lattice structure) of a given shell material (e.g., ZnS, ZnSe). For example, in the case of cubic ZnSe and ZnS, one monolayer can correspond to 0.328 nm and 0.31 nm thickness, respectively.

[0130] Semiconductor nanocrystal particles (also referred to as quantum dots) are crystalline materials with a size of several nanometers. Semiconductor nanocrystal particles can have a large surface area per unit volume due to very small size, and can present different properties from bulk materials with the same composition due to quantum confinement effects. Quantum dots can absorb light from an excitation source to be excited, and can emit energy corresponding to the energy band gap of the quantum dots. Quantum dots have potential applicability for a variety of devices (e.g., electronic devices) due to their unique photoluminescent properties. Quantum dots with properties that can currently be applied to electronic devices, etc. are mainly based on cadmium quantum dots. However, cadmium can cause serious environmental / health problems and is therefore a restricted element. Non-cadmium-based (cadmium-free) quantum dots are nanocrystals based on III-V groups. However, compared with those based on cadmium quantum dots, non-cadmium-based quantum dots can have insufficient photoluminescent properties (e.g., half width (FWHM) and luminous efficiency).

[0131] The quantum dot according to the embodiment includes a semiconductor nanocrystal core and a semiconductor nanocrystal shell disposed on the core, and does not include cadmium. The core includes a III-V compound, the quantum dot has a maximum photoluminescence peak in a green light wavelength region, and a half width (FWHM) of the maximum photoluminescence peak is less than or equal to about 50nm. The quantum dot has a difference (hereinafter referred to as Stokes shift) between the wavelength of the maximum photoluminescence peak and the first absorption peak wavelength of less than or equal to about 25nm. The quantum dot according to the embodiment may include indium and zinc.

[0132] The green light wavelength region may be greater than or equal to about 500 nm, for example, greater than or equal to about 510 nm, greater than or equal to about 520 nm, or greater than or equal to about 530 nm. The green light wavelength region may be less than or equal to about 560 nm, for example, less than or equal to about 550 nm, or less than or equal to about 540 nm. The first absorption peak may be greater than or equal to about 490 nm, for example, greater than or equal to about 495 nm, or greater than or equal to about 500 nm. The first absorption peak may be less than or equal to the wavelength of the maximum photoluminescence peak. For example, the first absorption peak may be less than or equal to about 550 nm, less than or equal to about 540 nm, or less than or equal to about 530 nm.

[0133] Here, the "first absorption peak (first excitation absorption peak)" refers to a main peak that first appears from a lower energy region in the UV-Vis absorption spectrum.

[0134] Non-cadmium quantum dots (e.g., based on III-V compounds including indium (In) and phosphorus (P)) have more traps and are more difficult to grow uniformly, and therefore have a wider half-width (FWHM) than cadmium quantum dots such as CdSe. In addition, since the core including indium (In) and phosphorus (P) can be easily oxidized on the surface, non-cadmium quantum dots cannot simultaneously present the desired values ​​of quantum efficiency and half-width (FWHM) even after the core is coated with a shell. Therefore, when applied to a display device (e.g., used in a display device), non-cadmium quantum dots may have difficulty in presenting the desired color reproducibility (e.g., under the next generation BT2020).

[0135] In quantum dots, Stokes shift refers to the difference between absorption energy and photoluminescence energy. Stokes shift can be represented by the difference between the first absorption peak wavelength (nm) (or energy, microelectron volts (meV)) in the UV-Vis absorption spectrum and the maximum photoluminescence peak wavelength (energy) in the photoluminescence spectrum. Without wishing to be bound by any theory, it is believed that the Stokes shift may depend on the size and / or composition of the quantum dot particles (e.g., the presence or absence of additional elements). Without wishing to be bound by any theory, it is believed that the surface state of the quantum dot may also have an effect on the Stokes shift. For example, the Stokes shift of a quantum dot may represent the composition, surface state, or a combination thereof of the quantum dot.

[0136] The size, composition, and surface of each individual quantum dot may have an effect on the Stokes shift of its group. The inventors have found that the Stokes shift of core / shell quantum dots may have a direct effect on the color reproducibility of a device including the quantum dots. Quantum dots according to embodiments (e.g., when the quantum dots form a group) may show a relatively low value of the Stokes shift, and when applied to a display device (e.g., used in a display device), the quantum dots of embodiments may exhibit improved color reproducibility.

[0137] The inventors have found that the Stokes shift may be related to defects in quantum dots, (average) particle size, size distribution, or a combination thereof, and that the Stokes shift may provide an indication of the effect that defects in quantum dots have on their luminescent properties, assuming no substantial change in the size and distribution of the quantum dots. According to the inventors' studies, the luminescent properties (e.g., FWHM and luminous efficiency) of quantum dots emitting green light may be more susceptible to the presence of defects in quantum dots than those emitting red light. In addition, defects in quantum dots may lead to an increase in trap emission, causing an increase in the longer wavelength tail in their photoluminescence spectrum. When the quantum dots are used as luminescent materials in a display device, the increase in the longer wavelength tail of the photoluminescence (PL) peak of the quantum dots may lead to problems with mixed light in the red and green wavelength regions, which may have a (e.g., severe) adverse effect on the color reproducibility of the device.

[0138] The quantum dots of the embodiments can be prepared by the methods described in detail below (e.g., including an environment rich in group III metals, controlled addition (e.g., injection) of group V element precursors, and addition of the above-mentioned additives). The inventors have found that in a reaction system for synthesizing a core based on a group III-V compound (e.g., a quantum dot based on indium phosphide), the amount of the group V element precursor can vary uncontrollably and dramatically (e.g., depleted), which can significantly contribute to an increase in the number of defects in the resulting quantum dots.

[0139] Without wishing to be bound by any theory, the method described later can help control the amount of the group V element in the reaction system for the core, and thus the resulting quantum dots can have a reduced (e.g., reduced) number of defects. In addition, during the synthesis of the core, the shell, or a combination thereof, adding (e.g., injecting) the additive in an amount as described below can bring about enhanced luminescent properties (e.g., Stokes shift, PL quantum yield (QY), or FWHM) without causing significant changes in the luminescent wavelength (e.g., band gap) of the (green-emitting) quantum dots.

[0140] In the method to be described later, in addition to its nucleation period, the V group element precursor (e.g., phosphorus precursor) may be further added at an appropriate time of the synthesis of the core, whereby a rapid and sharp change in the amount of the precursor may be suppressed and the resulting quantum dot may show a reduced (e.g., decreased) Stokes shift. In addition, the above-mentioned additive included in the quantum dot (e.g., the core) may have an electronegativity greater than or equal to that of a IV group element such as tin (e.g., 1.96 for Sn) and less than or equal to the large electronegativity of a given V group element (e.g., 2.19 for phosphorus), and may also contribute to the reduction of the Stokes shift.

[0141] In summary, without wishing to be bound by any theory, it is believed that the manufacturing environment to be described subsequently may be related to (e.g., affect) the properties of the quantum dots (e.g., reduce or reduce the number of defects on the surface of the quantum dots), which in turn may contribute to the reduced level of, e.g., reduced Stokes shift (which may otherwise not be achieved by non-cadmium quantum dots). In addition, the quantum dots of the embodiments may have a reduced (e.g., shorter) tail in the photoluminescence spectrum of the quantum dots (e.g., in the longer wavelength region) and a reduced, e.g., reduced FWHM and an improved quantum efficiency. For quantum dots emitting green light, the reduced (e.g., shorter) tail of the longer wavelength region of the PL peak may effectively suppress light mixing with red light emission of the device, and when applied in the device, the quantum dots of the embodiments and the quantum dot polymer composites including the same may exhibit improved color reproducibility.

[0142] In an embodiment, the quantum dot may have a Stokes shift of less than or equal to about 25 nm, less than or equal to about 25 nm, less than or equal to about 23 nm, less than or equal to about 22 nm, less than or equal to about 21 nm, less than or equal to about 20 nm, or less than or equal to about 19 nm. The Stokes shift may be greater than or equal to about 5 nm, greater than or equal to about 6 nm, greater than or equal to about 7 nm, greater than or equal to about 8 nm, greater than or equal to about 9 nm, or greater than or equal to about 10 nm.

[0143] In terms of energy levels, the quantum dots may have a Stokes shift of less than or equal to about 0.15 eV, less than or equal to about 0.145 eV, less than or equal to about 0.14 eV, less than or equal to about 0.135 eV, less than or equal to about 0.13 eV, less than or equal to about 0.125 eV, less than or equal to about 0.12 eV, less than or equal to about 0.115 eV, less than or equal to about 0.11 eV, less than or equal to about 0.105 eV, less than or equal to about 0.1 eV, less than or equal to about 0.095 eV, less than or equal to about 0.09 eV, or less than or equal to about 0.085 eV.

[0144] In embodiments, the quantum dots may exhibit enhanced optical properties.

[0145] In embodiments, the maximum photoluminescence peak of the quantum dots may have a FWHM of less than or equal to about 35 nm, less than or equal to about 34 nm, 33 nm, less than or equal to about 32 nm, or less than or equal to about 31 nm.

[0146] In embodiments, the quantum yield of the quantum dots may be greater than or equal to about 80%, greater than or equal to about 81%, greater than or equal to about 83%, greater than or equal to about 84%, greater than or equal to about 85%, or greater than or equal to about 86%.

[0147] The quantum dots may be included in (organic) solutions or complexes (eg when they are subjected to optical property analysis). The solution including the quantum dots may have an optical density or absorbance (absorbance) of greater than or equal to about 5%, greater than or equal to about 10%, greater than or equal to about 15%, greater than or equal to about 20%, greater than or equal to about 25%, greater than or equal to about 30%, greater than or equal to about 35%, greater than or equal to about 40%, greater than or equal to about 45%, greater than or equal to about 50%, greater than or equal to about 55%, greater than or equal to about 60%, greater than or equal to about 65%, greater than or equal to about 70%, greater than or equal to about 75%, greater than or equal to about 80%, or greater than or equal to about 85% and less than or equal to about 100%, less than or equal to about 90%, less than or equal to about 80%, less than or equal to about 70%, less than or equal to about 60%, less than or equal to about 50%, less than or equal to about 40%, less than or equal to about 30%, less than or equal to about 20%, or less than or equal to about 10%.

[0148] In the photoluminescence spectrum of the quantum dots, the ratio of the (predetermined) tail area of ​​the PL peak curve to the total area may be less than or equal to about 10%, less than or equal to about 9%, less than or equal to about 8%, less than or equal to about 7%, less than or equal to about 6%, less than or equal to about 5%, or less than or equal to about 4%.

[0149] In the photoluminescence spectrum of the quantum dots, the ratio of the intensity at the tail start wavelength to the intensity of the maximum PL peak may be less than or equal to about 0.12, for example, less than or equal to about 0.11, less than or equal to about 0.1, less than or equal to about 0.9, less than or equal to about 0.8, less than or equal to about 0.7, less than or equal to about 0.6, or less than or equal to about 0.5.

[0150] When they are applied to display devices (in the form of composite films or single layers), even without the help of color filters (e.g., blocking blue light, green light and / or red light), quantum dots having the above properties can exhibit enhanced Stokes shift and narrowed FWHM, thereby achieving increased brightness (without the loss of its brightness due to the presence of color filters). In addition, when applied to displays, the quantum dots can show improved color purity and prevent color mixing, so that in the absence of color filters, they can achieve an enhanced color gamut of greater than or equal to about 80%, greater than or equal to about 85%, greater than or equal to about 89%, or greater than or equal to about 90%.

[0151] In an embodiment, the semiconductor nanocrystal core may include indium. The semiconductor nanocrystal core may include phosphorus. The semiconductor nanocrystal core may include InP, InAs, GaP, GaAs, or a combination thereof. In an embodiment, the quantum dot may include a semiconductor nanocrystal core comprising indium phosphide (e.g., InP). The semiconductor nanocrystal core may further include zinc.

[0152] When the core includes zinc, the amount of zinc may be greater than 0, greater than or equal to about 0.001 mole, greater than or equal to about 0.005 mole, greater than or equal to about 0.01 mole, greater than or equal to about 0.05 mole, greater than or equal to about 0.1 mole, greater than or equal to about 0.5 mole, or greater than or equal to about 1 mole and less than or equal to about 5 moles, less than or equal to about 3 moles, less than or equal to about 1 mole, less than or equal to about 0.9 mole, less than or equal to about 0.7 mole, less than or equal to about 0.5 mole, less than or equal to about 0.3 mole, or less than or equal to about 0.1 mole, based on 1 mole of indium.

[0153] The semiconductor nanocrystal core may further include a Group IV element. The Group IV element may include tin (Sn).

[0154] In the quantum dot according to the embodiment, the amount of the Group IV element may be greater than or equal to about 0.00001 mol, greater than or equal to about 0.00005 mol, greater than or equal to about 0.0001 mol, greater than or equal to about 0.0005 mol, greater than or equal to about 0.001 mol, greater than or equal to about 0.0015 mol, greater than or equal to about 0.002 mol, greater than or equal to about 0.003 mol, greater than or equal to about 0.004 mol, greater than or equal to about 0.005 mol, greater than or equal to about 0.006 mol, greater than or equal to about 0.007 mol, greater than or equal to about 0.008 mol, greater than or equal to about 0.009 mol, greater than or equal to about 0.01 mol, or greater than or equal to about 0.1 mol and less than or equal to about 1 mol, less than or equal to about 0.9 mol, less than or equal to about 0.8 mol, less than or equal to about 0.7 mol, less than or equal to about 0.6 mol, Less than or equal to about 0.5 mole, less than or equal to about 0.4 mole, less than or equal to about 0.3 mole, less than or equal to about 0.2 mole, less than or equal to about 0.1 mole, less than or equal to about 0.09 mole, less than or equal to about 0.08 mole, less than or equal to about 0.07 mole, less than or equal to about 0.06 mole, less than or equal to about 0.05 mole, less than or equal to about 0.04 mole, less than or equal to about 0.03 mole, less than or equal to about 0. The presence and amount of the Group IV element can be confirmed by a suitable method such as X-ray photoelectron spectroscopy (XPS) or inductively coupled plasma atomic emission spectroscopy (ICP-AES).

[0155] The size of the core may be appropriately selected in consideration of the photoluminescence wavelength. For example, the size of the core may be greater than or equal to about 1 nm, such as greater than or equal to about 1.1 nm, greater than or equal to about 1.2 nm, greater than or equal to about 1.3 nm, greater than or equal to about 1.4 nm, greater than or equal to about 1.5 nm, greater than or equal to about 1.6 nm, greater than or equal to about 1.7 nm, greater than or equal to about 1.8 nm, greater than or equal to about 1.9 nm, or greater than or equal to about 2 nm. For example, the size of the core may be less than or equal to about 5 nm, such as less than or equal to about 4.5 nm, less than or equal to about 4 nm, less than or equal to about 3.5 nm, or less than or equal to about 3 nm.

[0156] The quantum dot according to the embodiment may have a core-multilayer shell structure. The semiconductor nanocrystal shell may include a first semiconductor nanocrystal shell including zinc and selenium. The shell may include a second semiconductor nanocrystal shell disposed on the first semiconductor nanocrystal shell and including zinc and sulfur. For example, the quantum dot may include a first shell directly on the core and including ZnSe, ZnSeS, or a combination thereof. The quantum dot may have a core-multilayer shell structure having a second shell directly on the first shell, having a composition different from the first shell, and including ZnS, ZnSeS, or a combination thereof.

[0157] The first semiconductor nanocrystal shell may include ZnSe. The first semiconductor nanocrystal shell may not include sulfur (S). For example, the first semiconductor nanocrystal shell may not include ZnSeS. In an embodiment, the semiconductor nanocrystal shell may include ZnSeS. The first semiconductor nanocrystal shell may be directly disposed on the semiconductor nanocrystal core. The first semiconductor nanocrystal shell may have a thickness greater than or equal to about 1 monolayer (ML), greater than or equal to about 1.5ML, greater than or equal to about 2ML, greater than or equal to about 2.5ML, greater than or equal to about 3ML, or greater than or equal to about 4ML. The first semiconductor nanocrystal shell may have a thickness less than or equal to about 10ML, for example, less than or equal to about 9ML, less than or equal to about 8ML, or less than or equal to about 7ML.

[0158] In one embodiment, the thickness of the first semiconductor nanocrystal shell may be greater than or equal to about 1 nm, greater than or equal to about 1.1 nm, greater than or equal to about 1.2 nm, greater than or equal to about 1.3 nm, greater than or equal to about 1.4 nm, or greater than or equal to about 1.5 nm. The thickness of the first semiconductor nanocrystal shell may be less than or equal to about 3.5 nm, less than or equal to about 3 nm, less than or equal to about 2.5 nm, less than or equal to about 2 nm, or less than or equal to about 1.5 nm.

[0159] In another embodiment, the thickness of the first semiconductor nanocrystal shell can be less than or equal to about 1 nm, such as less than or equal to about 0.9 nm, less than or equal to about 0.8 nm, less than or equal to about 0.7 nm, or less than or equal to about 0.65 nm.

[0160] Without being bound by any particular theory, it is believed that quantum dots according to embodiments include a first semiconductor nanocrystal shell having a relatively increased thickness, and the shell may contribute to achieving shell uniformity and improving optical properties of the quantum dots.

[0161] The second semiconductor nanocrystal shell may be the outermost layer of the quantum dot. The second semiconductor nanocrystal shell may be directly disposed on the first semiconductor nanocrystal shell. The second semiconductor nanocrystal shell may include ZnSeS, ZnS, or a combination thereof. The second semiconductor nanocrystal shell may have a composition that varies in the radial direction. The second semiconductor nanocrystal shell may have a concentration gradient of sulfur that increases toward the surface of the quantum dot. In one embodiment, the thickness of the second semiconductor nanocrystal shell may be greater than or equal to about 1 nm, such as greater than or equal to about 0.9 nm, greater than or equal to about 0.8 nm, greater than or equal to about 0.7 nm, or greater than or equal to about 0.65 nm. In another embodiment, the thickness of the second semiconductor nanocrystal shell may be less than or equal to about 1 nm, such as less than or equal to about 0.9 nm, less than or equal to about 0.8 nm, less than or equal to about 0.7 nm, or less than or equal to about 0.65 nm.

[0162] In the quantum dot according to the embodiment, the core may include indium, phosphorus, and optionally zinc, and the shell may include zinc, sulfur, and selenium.

[0163] In the quantum dots, the molar ratio of sulfur and selenium to indium may be greater than or equal to about 20:1, for example, greater than or equal to about 21:1, greater than or equal to about 22:1, greater than or equal to about 23:1, greater than or equal to about 24:1, greater than or equal to about 25:1, or greater than or equal to about 26:1 and less than or equal to about 36:1, less than or equal to about 35:1, less than or equal to about 34:1, less than or equal to about 33:1, less than or equal to about 32:1, less than or equal to about 31:1, less than or equal to about 30:1, or less than or equal to about 29:1.

[0164] In the quantum dots, the molar ratio of phosphorus to indium may be greater than or equal to about 0.6: 1, for example, greater than or equal to about 0.65: 1, or greater than or equal to about 0.7: 1. In the quantum dots, the molar ratio of phosphorus to indium may be less than or equal to about 1.5, less than or equal to about 1.4, less than or equal to about 1.3, less than or equal to about 1.2, less than or equal to about 1.1, less than or equal to about 1, less than or equal to about 0.9: 1, for example, less than or equal to about 0.87: 1, less than or equal to about 0.85: 1, less than or equal to about 0.8: 1, or less than or equal to about 0.78: 1.

[0165] In the quantum dots, the molar ratio of zinc to indium may be greater than or equal to about 25:1, greater than or equal to about 26:1, greater than or equal to about 27:1, greater than or equal to about 28:1, greater than or equal to about 29:1 and less than or equal to about 45:1, less than or equal to about 44:1, less than or equal to about 43:1, less than or equal to about 42:1, less than or equal to about 41:1, less than or equal to about 40:1, less than or equal to about 39:1, less than or equal to about 38:1, less than or equal to about 37:1, less than or equal to about 36:1, or less than or equal to about 35:1. In the quantum dots, the molar ratio of selenium to sulfur (Se / S) may be greater than or equal to about 0.80:1, for example, greater than or equal to about 0.85:1, or greater than or equal to about 0.89:1 and less than or equal to about 2:1, for example, less than or equal to about 1.5:1.

[0166] Without being bound by any particular theory, the quantum dots having the above composition and manufactured by the manufacturing method described later may exhibit a reduced Stokes shift.

[0167] The quantum dots may have an (average) size of about 2 nm or more, such as about 3 nm or more, about 3.5 nm or more, about 4 nm or more, about 4.5 nm or more, about 5 nm or more, about 5.5 nm or more, about 6 nm or more, about 6.5 nm or more, about 7 nm or more, about 7.5 nm or more, or about 8 nm or more. The quantum dots may have an (average) size of about 30 nm or less, such as about 20 nm or less, about 15 nm or less, about 10 nm or less, about 9 nm or less, about 8 nm or less, or about 7.5 nm or less. The size of the quantum dots may be a particle diameter.

[0168] The size of the quantum dot may be a diameter. For non-spherical shapes, the size of the quantum dot may be an equivalent diameter, which is calculated by a two-dimensional area confirmed by transmission electron microscopy analysis. The size of the quantum dot may be measured by averaging the major and minor axis dimensions. The shape of the quantum dot is not particularly limited, and may be, for example, a spherical, polyhedral, pyramidal, multi-pod (multi-legged), or cubic shape, nanotube, nanowire, nanofiber, nanosheet, or a combination thereof, but is not limited thereto. The quantum dot may include an organic ligand, an organic solvent, or a combination thereof that will be described later on the surface of the quantum dot. The organic ligand, the organic solvent, or a combination thereof may be bound to the surface of the quantum dot.

[0169] According to the quantum dots of the embodiment, it can be applied to the display device as a sheet or as a patterned film. In an embodiment, the sheet or the patterned film may include a quantum dot-polymer composite. For example, a display device including a color filter based on quantum dots can provide improved display quality in terms of color purity, brightness, etc. The inventors have found that the quantum dots according to the embodiment can show a reduced level of Stokes shift, and therefore, can present greatly improved color reproducibility. Therefore, the quantum dots according to the embodiment can present improved color reproducibility based on BT2020, the next generation standard for display devices.

[0170] An embodiment provides a method for manufacturing the above-mentioned quantum dots, comprising:

[0171] preparing a semiconductor nanocrystal core comprising a Group III-V compound comprising a Group III metal and a Group V element;

[0172] preparing a first solution including a shell metal precursor and an organic ligand;

[0173] At a first temperature, adding semiconductor nanocrystal cores comprising a Group III-V compound to the first solution, for example, injecting semiconductor nanocrystal cores comprising a Group III-V compound into the first solution; and

[0174] The first solution including the semiconductor nanocrystal core is heated to a second temperature and a shell non-metal precursor is added to the first solution, such as injected into the first solution, to form a semiconductor nanocrystal shell on the surface of the semiconductor nanocrystal core.

[0175] During the formation of the semiconductor nanocrystal core and / or the formation of the shell, a Group V precursor (eg, a phosphorus precursor) may be added at least twice (eg, injected in separate portions).

[0176] The first temperature is less than or equal to about 150° C. The second temperature may be greater than or equal to about 250° C., for example, greater than or equal to about 260° C., greater than or equal to about 270° C., greater than or equal to about 280° C., or greater than or equal to about 290° C. and less than or equal to 350° C., for example, less than or equal to about 340° C., or less than or equal to about 330° C.

[0177] The compositions of the quantum dots, the semiconductor nanocrystal core, and the semiconductor nanocrystal shell are the same as described above.

[0178] In an embodiment, the first temperature may be greater than or equal to about 50°C, such as greater than or equal to about 80°C, or greater than or equal to about 90°C. The first temperature may be less than or equal to about 140°C, such as less than or equal to about 130°C, less than or equal to about 120°C, or less than or equal to about 110°C. The second temperature may be greater than or equal to about 250°C, such as greater than or equal to about 260°C, greater than or equal to about 270°C, greater than or equal to about 280°C, greater than or equal to about 290°C, greater than or equal to about 300°C, or greater than or equal to about 310°C. The second temperature may be less than or equal to about 330°C, such as less than or equal to about 325°C.

[0179] In the method, the type and amount of the semiconductor nanocrystal core, the shell metal precursor, and the shell non-metal precursor can be selected in consideration of the composition and size of the desired final quantum dot. For example, when the core includes indium, phosphorus, and optional zinc, and the shell includes zinc, sulfur, and selenium, each of the amounts of the zinc-containing precursor, the selenium-containing precursor, and the sulfur-containing precursor relative to the core can be controlled so that the resulting quantum dot can have the above-mentioned ratio of zinc, selenium, and sulfur relative to indium, respectively.

[0180] The organic ligand may include RCOOH, RNH 2 , R 2 NH, R 3 N, RSH, RH 2 PO, R 2 HPO, R 3 PO, RH 2 P.R 2 HP, R 3 P, ROH, RCOOR, RPO(OH) 2 , RHPOOH, R 2 POOH, or a combination thereof, wherein R is the same or different and independently hydrogen, a C1-C40 (e.g., C3-C24) aliphatic hydrocarbon group (e.g., alkyl, alkenyl, or alkynyl), or a C6-C20 aromatic hydrocarbon group (e.g., aryl), wherein in the organic ligand, at least one R is not hydrogen). The organic ligand may be RCOOH and RNH 2 mixture.

[0181] The organic ligand can be coordinated, for example, bound to the surface of the obtained nanocrystal and can contribute to the dispersibility of the nanocrystal in the solution, affect the luminescence and electrical properties of the quantum dots, or a combination thereof. Examples of the organic ligand can include methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecanethiol, hexyl mercaptan, octyl mercaptan, benzyl mercaptan; methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine; formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid, or benzoic acid; phosphine or aminophosphine such as substituted or unsubstituted methylphosphine (e.g., trimethylphosphine, methyldiphenylphosphine, etc.), substituted or unsubstituted ethylphosphine (e.g., triethylphosphine, ethyldiphenylphosphine, etc.), substituted or unsubstituted propylphosphine, substituted or unsubstituted butylphosphine, substituted or unsubstituted substituted pentyl phosphine, or substituted or unsubstituted octyl phosphine (e.g., trioctyl phosphine (TOP)); phosphine oxides such as substituted or unsubstituted methyl phosphine oxide (e.g., trimethyl phosphine oxide, methyl diphenyl phosphine oxide, etc.), substituted or unsubstituted ethyl phosphine oxide (e.g., triethyl phosphine oxide, ethyl diphenyl phosphine oxide, etc.), substituted or unsubstituted propyl phosphine oxide, substituted or unsubstituted butyl phosphine oxide, or substituted or unsubstituted octyl phosphine oxide (e.g., trioctyl phosphine oxide (TOPO); diphenylphosphine or triphenylphosphine compounds, or oxide compounds thereof; phosphinic acid, etc., but are not limited thereto. One or more organic ligands may be used. In an embodiment, the organic ligand may be a mixture of a fatty acid and an aliphatic primary amine.

[0182] The solvent for forming the first solution can be appropriately selected. The solvent can be an organic solvent. The organic solvent can include C6-C22 primary amines such as hexadecylamine; C6-C22 secondary amines such as dioctylamine; C6-C40 tertiary amines such as trioctylamine; nitrogen-containing heterocyclic compounds such as pyridine; C6-C40 aliphatic hydrocarbons (such as alkanes, alkenes, alkynes, etc.) such as hexadecane, octadecane, octadecene, or squalane; C6-C30 aromatic hydrocarbons such as phenyldodecane, phenyltetradecane, or phenylhexadecane; phosphine substituted by C6-C22 alkyl such as trioctylphosphine; phosphine oxide substituted by C6-C22 alkyl such as trioctylphosphine oxide; C12-C22 aromatic ethers such as phenyl ether or benzyl ether; or a combination thereof. The type and amount of the solvent can be appropriately selected considering the precursor and the organic ligand.

[0183] The first solution may be heated at a predetermined temperature, for example, greater than or equal to about 100° C. and less than or equal to about 150° C., under vacuum, an inert atmosphere, or a combination thereof.

[0184] The core according to an embodiment can be formed by a thermal addition, such as a hot injection method, in which a Group V element precursor (e.g., a phosphorus precursor) is added, such as injected, into a solution including a metal precursor, such as an indium precursor, and an optional ligand, and an optional zinc precursor, which is heated at a high temperature (e.g., greater than or equal to about 200°C).

[0185] The implantation of the Group V element precursor (eg, phosphorus precursor) may be performed at least twice (eg, in a divided manner) (eg, upon nucleation of the core and thereafter at a suitable interval). In embodiments, the implantation time and / or the amount implanted may be appropriately controlled.

[0186] In an embodiment, the core may be prepared in a heating (temperature ramping) process in which the reactants are first mixed and dissolved and then heated together.

[0187] The same or different amounts of the group V precursor (e.g., phosphorus precursor) may be added to the heated solution multiple times (e.g., at least twice, such as at the beginning and later parts of the reaction), such as injected into the heated solution. For example, when the group V element precursor is added twice, the ratio between the amounts added each time may be 1:0.1 to 1:10.

[0188] The phosphorus precursor may include at least two (eg, three, four, or more) different phosphorus compounds.

[0189] The phosphorus precursor may include white phosphorus; red phosphorus; a mono-, di- or tri-substituted or unsubstituted alkyl phosphine, such as a tri(alkylsilyl)phosphine (e.g., tri(trialkylsilyl)phosphine), tricyclohexylphosphine, cyclohexyldimethylphosphine, diethylhexylphosphine, dimethylethylphosphine, diethylmethylphosphine, diethylcarboxymethylphosphine, dialkylaminoalkylphosphine, diarylphosphine, dialkylphosphine, trialkylphosphine, triarylphosphine (e.g., triphenylphosphine), or a combination thereof.

[0190] The metal (e.g., indium) precursor may be in the form of a metal (e.g., metal powder), an alkylated metal compound, a metal alkoxide, a metal carboxylate, a metal nitrate, a metal perchlorate, a metal sulfate, a metal acetylacetonate, a metal halide, a metal cyanide, a metal hydroxide, a metal oxide, a metal peroxide, or a combination thereof. In an embodiment, the metal (e.g., indium) precursor may be present in excess of the Group V element (e.g., phosphorus) precursor.

[0191] When the core further includes the above-mentioned additive (e.g., a Group 4 element such as Sn (tin), As, Sb, Bi, or Te), a precursor of the additive may be further added at a suitable time during the core synthesis (e.g., a nucleation step, a later part, or in the middle). The precursor for the additive may be in the form of a suitable compound. The precursor may be a carboxylate, or an alkyl halide, etc. The precursor for the additive may be a tin carboxylate (e.g., tin acetate), an alkyl tin chloride (e.g., dialkyl tin dichloride), etc.

[0192] In embodiments, the addition of the above-mentioned additives can help to keep (e.g., maintain) the amount of the Group V element precursor at a controlled level during the core synthesis without causing a significant change in the emission wavelength of the quantum dots, and reduce the number of defects in the prepared core (and subsequently formed shell).

[0193] The amount of the precursor for the additive may be appropriately controlled. In an embodiment, the amount of the additive precursor may be greater than or equal to about 0.001 mole, such as greater than or equal to about 0.005 mole, or greater than or equal to about 0.01 mole and less than or equal to about 0.1 mole, less than or equal to about 0.09 mole, less than or equal to about 0.08 mole, less than or equal to about 0.07 mole, less than or equal to about 0.06 mole, less than or equal to about 0.05 mole, less than or equal to about 0.04 mole, less than or equal to about 0.03 mole, less than or equal to about 0.02 mole, or less than or equal to about 0.01 mole, relative to 1 mole of the Group III metal. Within the above range, the desired Stokes shift value can be achieved without any substantial reduction in the luminous efficiency of the quantum dots.

[0194] The shell metal precursor may be a zinc-containing precursor. The zinc-containing precursor is not particularly limited and may be appropriately selected. For example, the zinc-containing precursor may be Zn metal powder, alkylated Zn compounds, alcohol Zn, carboxylic acid Zn, Zn nitrate, Zn perchlorate, Zn sulfate, Zn acetylacetonate, Zn halides, Zn cyanides, Zn hydroxides, Zn oxides, Zn peroxides, zinc carbonate, or a combination thereof. Examples of the shell metal precursor may be dimethyl zinc, diethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, etc. One or more shell metal precursors may be used.

[0195] The shell non-metal precursor may include a selenium-containing precursor and a sulfur-containing precursor.

[0196] The type of the selenium-containing precursor is not particularly limited and can be appropriately selected. For example, the selenium-containing precursor includes selenium-trioctylphosphine (Se-TOP), selenium-tributylphosphine (Se-TBP), selenium-triphenylphosphine (Se-TPP), or a combination thereof, but is not limited thereto.

[0197] The sulfur-containing precursor is not particularly limited and can be appropriately selected. The sulfur-containing precursor can be hexyl mercaptan, octyl mercaptan, decanyl mercaptan, dodecanol, hexathiol, mercaptopropyl silane, sulfur-trioctyl phosphine (S-TOP), sulfur-tributyl phosphine (S-TBP), sulfur-triphenylphosphine (S-TPP), sulfur-trioctylamine (S-TOA), trimethylsilyl sulfide, ammonium sulfide, sodium sulfide or its combination. The sulfur-containing precursor can be added, for example, injected into the first solution once or more times (for example, twice or more times). The formation of the semiconductor nanocrystal shell can include further adding the shell non-metal precursor and optional shell metal precursor to the first solution, for example, injecting the shell non-metal precursor and optional shell metal precursor into the first solution at least once, at least twice, at least three times, at least four times, at least five times or more times.

[0198] In the shell formation, by adjusting the order and amount of addition (e.g., injection) of the shell non-metal precursor to the first solution, the semiconductor nanocrystal shell of the final quantum dot can be formed to have a desired composition (e.g., the first and second shells described above). In an embodiment, the formation of the semiconductor nanocrystal shell may include: forming a first semiconductor nanocrystal shell on the semiconductor nanocrystal core by reacting a zinc-containing precursor and a selenium-containing precursor at a first reaction temperature for greater than or equal to about 40 minutes; and forming a second semiconductor nanocrystal shell on the first semiconductor nanocrystal shell by reacting a zinc-containing precursor and a sulfur-containing precursor at a second reaction temperature in the presence of particles having the first semiconductor nanocrystal shell in an organic solvent and an organic ligand.

[0199] In the shell formation, the core addition (e.g., core injection) temperature (e.g., first temperature) may be appropriately controlled as above. For example, the core may be added, e.g., injected into the first solution, at a temperature of about 80° C. or more, about 90° C. or more, about 100° C. or more, about 110° C. or more, about 120° C. or more, about 130° C. or more, or about 140° C. or more. The core may be added, e.g., injected into the first solution, at a temperature of about 150° C. or less, about 140° C. or less, about 130° C. or less, about 120° C. or less, or about 110° C. or less.

[0200] The temperature for the shell formation (e.g., the second reaction temperature) may be appropriately selected. For example, the temperature for the shell formation may be greater than or equal to about 250° C., such as greater than or equal to about 260° C., greater than or equal to about 270° C., greater than or equal to about 280° C., greater than or equal to about 290° C., greater than or equal to about 300° C., greater than or equal to about 310° C., or greater than or equal to about 315° C. After the heating of the solution is completed or while the first solution is heated to the reaction temperature, the shell non-metal precursor and optionally the shell metal precursor added thereto are added, such as injected into the first solution.

[0201] The reaction time for the shell formation (eg, the first shell, the second shell, or a combination thereof) can be appropriately adjusted, but is not particularly limited. The thickness of the first / second semiconductor nanocrystal shell can be adjusted by reacting at the shell formation reaction temperature for a predetermined reaction time.

[0202] In the method according to the embodiment, the content of the shell metal / non-metal precursor of the group III metal (e.g., indium) included in the core in the reaction system can be selected. For example, when a ZnSe shell is formed on a core containing indium, the amount of the selenium precursor relative to the amount of indium can be adjusted to form a first semiconductor nanocrystal shell with a predetermined thickness with a predetermined reaction time. For example, selenium can be used in a range of greater than or equal to about 5.5 moles and less than or equal to about 10 moles of indium in the reaction system according to about 1 mole. The amount of the sulfur precursor relative to indium can be adjusted to form a second semiconductor nanocrystal shell with a predetermined thickness and composition with a predetermined reaction time. In an embodiment, sulfur is used in an amount greater than or equal to about 25 moles and less than or equal to about 45 moles of indium per 1 mole.

[0203] The method may not include reducing the temperature of the reaction solution including particles having the first semiconductor nanocrystal shell to less than or equal to about 50° C. (eg, less than or equal to about 30° C. or room temperature).

[0204] The method may further include adding an additive comprising ammonium fluoride, a group IV element, or a combination thereof to the first solution during the formation of the semiconductor nanocrystal shell, such as injecting ammonium fluoride, a group IV element, or a combination thereof into the first solution. The mode of adding the additive (e.g., the time for adding) is not particularly limited. The additive may be added individually or in a mixture with other precursors (e.g., sulfur and / or selenium precursors).

[0205] The amount of the additive (e.g., ammonium fluoride) may be appropriately selected. Based on 1 mole of the Group III metal (e.g., indium), the amount of the additive (e.g., ammonium fluoride) may be greater than or equal to about 0.0001 mole, greater than or equal to about 0.0005 mole, greater than or equal to about 0.001 mole, greater than or equal to about 0.005 mole, greater than or equal to about 0.01 mole, greater than or equal to about 0.05 mole, greater than or equal to about 0.1 mole, greater than or equal to about 0.5 mole, or greater than or equal to about 1 mole and less than or equal to about 5 moles, less than or equal to about 4 moles, less than or equal to about 3 moles, less than or equal to about 2 moles, less than or equal to about 1 mole, less than or equal to about 0.5 mole, or less than or equal to about 0.1 mole.

[0206] When adding non-solvent to the final reaction solution obtained, the nanocrystal of organic ligand coordination can be separated (e.g., precipitated). The non-solvent can be a polar solvent miscible with the solvent used in the reaction, and the nanocrystal is non-dispersible therein. The non-solvent can be selected depending on the solvent used in the reaction, and can be, for example, acetone, ethanol, butanol, isopropanol, ethylene glycol, water, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), diethyl ether, formaldehyde, acetaldehyde, a solvent with a solubility parameter similar to the aforementioned non-solvent, or a combination thereof. The separation can be carried out by centrifugation, precipitation, chromatography, or distillation. If necessary, the separated nanocrystal can be added to a washing solvent and washed. The washing solvent is not particularly limited and can have a solubility parameter similar to the solubility parameter of the ligand, and can, for example, include hexane, heptane, octane, chloroform, toluene, benzene, etc.

[0207] In an embodiment, the quantum dot composition includes the above-mentioned quantum dots, a dispersant or a binder polymer (e.g., including a carboxylic acid group) optionally used to ensure the dispersion of the quantum dots, a polymerizable monomer (e.g., a photopolymerizable monomer) including a carbon-carbon double bond, and an initiator (e.g., a photoinitiator or a thermal initiator). The composition may further include an organic solvent.

[0208] The composition according to the embodiment can be used to manufacture the pattern of quantum dot-polymer complex. The composition according to the embodiment can be a photoresist composition containing quantum dots to which a photolithography method can be applied. The composition according to the embodiment can be an ink composition that can provide a pattern by printing (e.g., a droplet discharge method such as inkjet printing). The composition according to the embodiment may not include a conjugated polymer (except for the cardo adhesive that will be described later). The composition according to the embodiment may include a conjugated polymer. Here, the conjugated polymer may refer to a polymer having a conjugated double bond in the main chain of the polymer (e.g., polyphenylene vinylene, etc.).

[0209] In the composition, the quantum dots are the same as described above. In the composition, the amount of the quantum dots can be appropriately selected considering the final use and composition of the composition. In an embodiment, based on the solid content (solid content) of the composition, the amount of the quantum dots may be greater than or equal to about 1 weight percent (wt%), for example, greater than or equal to about 2 weight %, greater than or equal to about 3 weight %, greater than or equal to about 4 weight %, greater than or equal to about 5 weight %, greater than or equal to about 6 weight %, greater than or equal to about 7 weight %, greater than or equal to about 8 weight %, greater than or equal to about 9 weight %, greater than or equal to about 10 weight %, greater than or equal to about 15 weight %, greater than or equal to about 20 weight %, greater than or equal to about 25 weight %, greater than or equal to about 30 weight %, greater than or equal to about 35 weight %, or greater than or equal to about 40 weight %. Based on the solid content (solid content), the amount of the quantum dots may be less than or equal to about 70 wt %, for example, less than or equal to about 65 wt %, less than or equal to about 60 wt %, less than or equal to about 55 wt %, or less than or equal to about 50 wt %.

[0210] In the composition according to the embodiment, the dispersant is a compound capable of dispersing the quantum dots. The dispersant may include a binder polymer containing a carboxylic acid group (hereinafter, may also be referred to as a carboxylic acid polymer or a binder containing a carboxyl group). The binder polymer may be an insulating polymer. The binder polymer may include: a copolymer of a monomer mixture, the monomer mixture including a first monomer including a carboxylic acid group and a carbon-carbon double bond, a second monomer including a carbon-carbon double bond and a hydrophobic portion and excluding a carboxylic acid group, and optionally including a third monomer including a carbon-carbon double bond and a hydrophilic portion and excluding a carboxylic acid group;

[0211] A polyaromatic ring-containing polymer having a skeleton structure in which two aromatic rings are bonded to a quaternary carbon atom which is a constituent atom of another cyclic portion in the main chain and including a carboxylic acid group (—COOH); or

[0212] Its combination.

[0213] Examples of the first monomer may include carboxylic acid vinyl ester compounds such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, fumaric acid, 3-butenoic acid, etc., but are not limited thereto. One or more first monomers may be used.

[0214] Examples of the second monomer may be alkenyl aromatic compounds such as vinyl acetate, vinyl benzoate, styrene, α-methylstyrene, vinyl toluene, or vinyl benzyl methyl ether; unsaturated carboxylic acid ester compounds such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, benzyl acrylate, benzyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, phenyl acrylate, or phenyl methacrylate; unsaturated carboxylic acid aminoalkyl ester compounds such as 2-aminoethyl acrylate, 2-aminoethyl methacrylate, 2-dimethylaminoethyl acrylate, or 2-dimethylaminoethyl methacrylate; maleimides such as N-phenylmaleimide, N-benzylmaleimide, N-alkylmaleimide; unsaturated carboxylic acid glycidyl ester compounds such as glycidyl acrylate or glycidyl methacrylate; vinyl cyanide compounds such as acrylonitrile, methacrylonitrile; or unsaturated amide compounds such as acrylamide or methacrylamide, but are not limited thereto. One or more second monomers may be used.

[0215] Specific examples of the third monomer may include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxybutyl acrylate, or 2-hydroxybutyl methacrylate, but are not limited thereto. One or more third monomers may be used.

[0216] In the carboxylic acid polymer, the amount of the first repeating unit derived from the first monomer may be greater than or equal to about 10 mole percent (mol%), such as greater than or equal to about 15 mole%, greater than or equal to about 25 mole%, or greater than or equal to about 35 mole%, based on the total moles of the carboxylic acid polymer. In the binder including a carboxyl group, the amount of the first repeating unit may be less than or equal to about 90 mole%, such as less than or equal to about 89 mole%, less than or equal to about 80 mole%, less than or equal to about 70 mole%, less than or equal to about 60 mole%, less than or equal to about 50 mole%, less than or equal to about 40 mole%, less than or equal to about 35 mole%, or less than or equal to about 25 mole%, based on the total moles of the carboxylic acid polymer.

[0217] In the carboxylic acid polymer, the amount of the second repeating unit derived from the second monomer may be greater than or equal to about 10 mol%, such as greater than or equal to about 15 mol%, greater than or equal to about 25 mol%, or greater than or equal to about 35 mol%, based on the total moles of the carboxylic acid polymer. In the binder polymer, the amount of the second repeating unit may be less than or equal to about 90 mol%, such as less than or equal to about 89 mol%, less than or equal to about 80 mol%, less than or equal to about 70 mol%, less than or equal to about 60 mol%, less than or equal to about 50 mol%, less than or equal to about 40 mol%, less than or equal to about 35 mol%, or less than or equal to about 25 mol%, based on the total moles of the carboxylic acid polymer.

[0218] In the carboxylic acid polymer, if present, the amount of the third repeating unit derived from the third monomer may be greater than or equal to about 1 mol%, such as greater than or equal to about 5 mol%, greater than or equal to about 10 mol%, or greater than or equal to about 15 mol%, based on the total moles of the carboxylic acid polymer. In the binder polymer, the amount of the third repeating unit may be less than or equal to about 30 mol%, such as less than or equal to about 25 mol%, less than or equal to about 20 mol%, less than or equal to about 18 mol%, less than or equal to about 15 mol%, or less than or equal to about 10 mol%, based on the total moles of the carboxylic acid polymer.

[0219] The carboxylic acid polymer may be a copolymer of (meth)acrylic acid; and at least one second and optionally a third monomer, such as an aralkyl (meth)acrylate, a hydroxyalkyl (meth)acrylate, or styrene. For example, the binder polymer may be a methacrylic acid / methyl methacrylate copolymer, a methacrylic acid / benzyl methacrylate copolymer, a methacrylic acid / benzyl methacrylate / styrene copolymer, a methacrylic acid / benzyl methacrylate / 2-hydroxyethyl methacrylate copolymer, or a methacrylic acid / benzyl methacrylate / styrene / 2-hydroxyethyl methacrylate copolymer.

[0220] The polymer including a carboxylic acid group may include a polymer including a polyaromatic ring. The polymer including a polyaromatic ring may be a cardo binder resin and may be commercially available.

[0221] The polymer containing carboxylic acid groups may have an acid value of greater than or equal to about 50 milligrams of potassium hydroxide / gram (mg KOH / g). For example, the carboxylic acid polymer may have an acid value of greater than or equal to about 60 mg KOH / g, greater than or equal to about 70 mg KOH / g, greater than or equal to about 80 mg KOH / g, greater than or equal to about 90 mg KOH / g, greater than or equal to about 100 mg KOH / g, greater than or equal to about 110 mg KOH / g, greater than or equal to about 120 mg KOH / g, greater than or equal to about 125 mg KOH / g, or greater than or equal to about 130 mg KOH / g. The acid value of the polymer may be, for example, less than or equal to about 250 mg KOH / g, less than or equal to about 240 mg KOH / g, less than or equal to about 230 mg KOH / g, less than or equal to about 220 mg KOH / g, less than or equal to about 210 mg KOH / g, less than or equal to about 200 mg KOH / g, less than or equal to about 190 mg KOH / g, less than or equal to about 180 mg KOH / g, or less than or equal to about 160 mg KOH / g, but is not limited thereto.

[0222] The binder polymer may have a weight average molecular weight of about 1,000 grams per mole (g / mol) or more, such as about 2,000 g / mol or more, about 3,000 g / mol or more, or about 5,000 g / mol or more. The binder polymer may have a weight average molecular weight of about 100,000 g / mol or less, such as about 50,000 g / mol or less.

[0223] In the composition, based on the total weight of the composition, the amount of the binder polymer or the dispersant may be greater than or equal to about 0.5 wt %, for example, greater than or equal to about 1 wt %, greater than or equal to about 5 wt %, greater than or equal to about 10 wt %, greater than or equal to about 15 wt %, or greater than or equal to about 20 wt %, but is not limited thereto. Based on the total weight of the composition, the amount of the binder polymer or the dispersant may be less than or equal to about 35 wt %, for example, less than or equal to about 33 wt %, or less than or equal to about 30 wt %. Within the range, the dispersion of the quantum dots can be ensured. Based on the total weight of the solid content of the composition, the amount of the binder polymer may be about 0.5 wt %-about 55 wt %.

[0224] In the composition, the polymerizable monomer including a carbon-carbon double bond may include a photopolymerizable acrylic monomer. The polymerizable acrylic monomer may include (meth)acrylate (C1 to C18 alkyl), ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate. Acid ester, dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, pentaerythritol hexa(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A epoxy acrylate, trimethylolpropane tri(meth)acrylate, ethylene glycol monomethyl ether (meth)acrylate, novolac epoxy (meth)acrylate, propylene glycol di(meth)acrylate, tri(meth)acryloyloxyethyl phosphate, or a combination thereof.

[0225] Based on the total weight of the composition, the amount of the polymerizable monomer may be greater than or equal to about 0.5 wt%, such as greater than or equal to about 1 wt%, or greater than or equal to about 2 wt%. Based on the total weight of the composition, the amount of the polymerizable monomer may be less than or equal to about 30 wt%, such as less than or equal to about 28 wt%, less than or equal to about 25 wt%, less than or equal to about 23 wt%, less than or equal to about 20 wt%, less than or equal to about 18 wt%, less than or equal to about 17 wt%, less than or equal to about 16 wt%, or less than or equal to about 15 wt%.

[0226] The initiator in the composition can be used for the polymerization of the above-mentioned monomers. The initiator is a compound that can accelerate the free radical reaction (such as the free radical polymerization of the monomer) by generating free radical chemical species under mild conditions (such as via heat or light). The initiator may be a thermal initiator or a photoinitiator. The thermal initiator may include azobisisobutyronitrile, benzoyl peroxide, etc., but is not limited thereto. The photoinitiator is a compound that can initiate the free radical polymerization of the above-mentioned polymerizable acrylic monomer, thiol compound (which will be described later), or a combination thereof by light. The type of the photoinitiator is not particularly limited. The photoinitiator may include a triazine-based compound, an acetophenone compound, a benzophenone compound, a thioxanthone compound, a benzoin compound, an oxime ester compound, an aminoketone compound, a phosphine or phosphine oxide compound, a carbazole-based compound, a diketone compound, a boric acid sulfonium-based compound, a diazo-based compound, a biimidazole-based compound, or a combination thereof, but is not limited thereto. The initiator is not particularly limited.

[0227] In the composition, the amount of the initiator may be appropriately selected in consideration of the type and amount of the polymerizable monomer. In an embodiment, the initiator may be used in an amount ranging from about 0.01 wt % to about 10 wt % based on the total weight of the composition, but is not limited thereto.

[0228] The composition may further include a (multi- or monofunctional) thiol compound having at least one thiol group at a terminal, metal oxide fine particles, or a combination thereof.

[0229] The metal oxide fine particles may include TiO 2 、SiO 2 、BaTiO 3 , Ba 2 TiO 4 , ZnO, or a combination thereof. In the composition, the amount of the metal oxide may be less than or equal to about 15 wt % based on the amount of solids in the composition. The metal oxide fine particles may have a suitably selected diameter without particular limitation. The diameter of the metal oxide fine particles may be greater than or equal to about 100 nm, for example, greater than or equal to about 150 nm, or greater than or equal to about 200 nm and less than or equal to about 1,000 nm or less than or equal to about 800 nm.

[0230] The thiol compound may be a dithiol compound, a trithiol compound, a tetrathiol compound, or a combination thereof. For example, the thiol compound may be diol di-3-mercaptopropionate, diol dithioglycolate, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), 1,6-hexanedithiol, 1,3-propanedithiol, 1,2-ethanedithiol, polyethylene glycol dithiol including 1-10 ethylene glycol repeating units, or a combination thereof.

[0231] Based on the total weight of the composition, the amount of the thiol compound may be less than or equal to about 10 wt%, such as less than or equal to about 9 wt%, less than or equal to about 8 wt%, less than or equal to about 7 wt%, less than or equal to about 6 wt%, or less than or equal to about 5 wt%. Based on the total weight of the composition, the amount of the thiol compound may be greater than or equal to about 0.1 wt%, such as greater than or equal to about 0.5 wt%, or greater than or equal to about 1 wt%.

[0232] The composition may further include an organic solvent (or liquid vehicle). The type of the organic solvent (or liquid vehicle) that can be used is not particularly limited. The type and amount of the organic solvent (or liquid vehicle) can be appropriately determined by considering the above-mentioned main components (i.e., quantum dots, adhesives containing COOH groups, monomers that can be photopolymerized, photoinitiators, and thiol compounds if used), and the types and amounts of additives described subsequently. The composition can include a solvent in a residual amount other than the desired amount of solid content (non-volatile components). The solvent (or liquid vehicle) can be appropriately selected considering other components in the composition (e.g., adhesives, monomers that can be photopolymerized, photoinitiators, and other additives), affinity for alkaline developer solutions, boiling points, etc. Examples of the solvent may include: ethylene glycols, ethyl 3-ethoxypropionate, ethylene glycol, diethylene glycol, or polyethylene glycol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, ethylene glycol diethyl ether, or diethylene glycol dimethyl ether; glycol ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, or diethylene glycol monobutyl ether acetate; propylene glycols such as propylene glycol; propylene glycol ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene ...methyl ether Propylene glycol dimethyl ether, propylene glycol diethyl ether, or dipropylene glycol diethyl ether; propylene glycol ether acetates such as propylene glycol monomethyl ether acetate or dipropylene glycol monoethyl ether acetate; amides such as N-methylpyrrolidone, dimethylformamide, or dimethylacetamide; ketones such as methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), or cyclohexanone; petroleum such as toluene, xylene, or solvent naphtha; esters such as ethyl acetate, butyl acetate, or ethyl lactate; ethers such as diethyl ether, dipropyl ether, or dibutyl ether, aliphatic, alicyclic, or aromatic hydrocarbons or their carboxylic acid ester / ester derivatives (such as cyclohexyl acetate, etc.), and mixtures thereof.

[0233] If desired, in addition to the above components, the composition may further include various additives such as light diffusing agents, leveling agents, or coupling agents. The amount of the additive is not particularly limited, and can be controlled within a suitable range in which the additive does not cause adverse effects on the preparation of the composition and the manufacture of the quantum dot-polymer composite and optionally the patterning of the composite. The additive may be a material having a desired function without particular limitation.

[0234] If used, the additive may be used in an amount of greater than or equal to about 0.1 wt %, such as greater than or equal to about 0.5 wt %, greater than or equal to about 1 wt %, greater than or equal to about 2 wt %, or greater than or equal to about 5 wt %, based on the total weight of the composition, but is not limited thereto. If used, the amount of the additive may be less than or equal to about 20 wt %, such as less than or equal to about 19 wt %, less than or equal to about 18 wt %, less than or equal to about 17 wt %, less than or equal to about 16 wt %, or less than or equal to about 15 wt %, based on the total weight of the composition, but is not limited thereto.

[0235] The composition can be prepared by appropriately mixing the above-mentioned components.

[0236] In an embodiment, the quantum dot-polymer composite comprises: a polymer matrix; and the above-mentioned quantum dots dispersed in the polymer matrix. The polymer matrix may include a thiol-ene resin, a linear or cross-linked substituted or unsubstituted poly (meth) acrylate, a linear or cross-linked polyurethane, a linear or cross-linked epoxy resin, a linear or cross-linked substituted or unsubstituted vinyl polymer, a linear or cross-linked silicone resin, or a combination thereof.

[0237] The polymer matrix may include a cross-linked polymer, an adhesive polymer having a carboxylic acid group, or a combination thereof. The cross-linked polymer may include a thiol-ene resin, a cross-linked poly(meth)acrylate, a cross-linked polyurethane, a cross-linked epoxy resin, a cross-linked vinyl polymer, a cross-linked silicone resin, or a combination thereof.

[0238] In an embodiment, the polymer matrix may include a binder polymer, a polymerization product of a photopolymerizable monomer containing a carbon-carbon double bond, and optionally a polymerization product of the photopolymerizable monomer and a polythiol compound having at least two thiol groups at the terminal. The quantum dots, the binder polymer, the photopolymerizable monomer, and the polythiol compound are the same as described above.

[0239] The quantum dot-polymer composite may have a film shape. The film may have a thickness of, for example, about 200 μm or less, about 190 μm or less, about 180 μm or less, about 170 μm or less, about 160 μm or less, about 150 μm or less, about 140 μm or less, about 130 μm or less, about 120 μm or less, about 110 μm or less, about 1000 μm or less, about 90 μm or less, about 80 μm or less, about 70 μm or less, about 60 μm or less, about 50 μm or less, about 40 μm or less, about 30 μm or less, for example, about 10 μm or less, about 8 μm or less, or about 7 μm or less and about 2 μm or greater, for example, about 3 μm or greater, about 3.5 μm or greater, or about 4 μm or greater.

[0240] In embodiments, the quantum dot polymer composite may be configured to have a reduced level of Stokes shift (e.g., less than or equal to about 30 nm, less than or equal to about 29 nm, less than or equal to about 28 nm, less than or equal to about 27 nm, less than or equal to about 25 nm, less than or equal to about 24 nm, less than or equal to about 23 nm, less than or equal to about 22 nm, less than or equal to about 21 nm, or less than or equal to about 20 nm). In embodiments, the quantum dot polymer composite may be configured to emit light having a FWHM of less than or equal to about 38 nm, such as less than or equal to about 37 nm, less than or equal to about 36 nm, less than or equal to about 35 nm, less than or equal to about 34 nm, or less than or equal to about 33 nm.

[0241] The quantum dot polymer composite may exhibit improved thermal stability. Thus, when heat-treated at about 180° C. for about 30 minutes in a nitrogen atmosphere, the quantum dot polymer composite may exhibit a photoconversion efficiency (PCE) of greater than or equal to about 20%.

[0242] In an embodiment, a display device includes a light source and a photoluminescent element, and the photoluminescent element includes the above-mentioned quantum dot-polymer composite and the light source is configured to provide incident light to the photoluminescent element. The incident light may have a photoluminescent peak wavelength greater than or equal to about 440 nm, for example, greater than or equal to about 450 nm and less than or equal to about 500 nm, for example, less than or equal to about 490 nm, less than or equal to about 480 nm, less than or equal to about 470 nm, or less than or equal to about 460 nm.

[0243] In an embodiment, the photoluminescent element may include a sheet of the quantum dot polymer composite. The display device may further include a liquid crystal panel, and the sheet of the quantum dot polymer composite may be disposed between the light source and the liquid crystal panel. Figure 1A An exploded view of the display device is shown without limitation.

[0244] Reference Figure 1A The display device may have a structure in which a reflector, a light guide plate (LGP) and a blue LED light source (blue LED), the above-mentioned quantum dot-polymer composite sheet (QD sheet), various optical films such as a prism, a double brightness enhancement film (DBEF), etc. are stacked, and a liquid crystal (LC) panel is disposed thereon.

[0245] The display device may not include a liquid crystal layer. The display device may include a blue organic light emitting diode (OLED) as a light source. Figure 1B The display device may include a (blue) organic light emitting diode (OLED) as a light source and a quantum dot polymer composite sheet thereon including a mixture of red and green quantum dots. An absorptive color filter layer (having red / green / blue (R / G / B) segments) and a substrate may be disposed on the quantum dot polymer composite sheet.

[0246] The organic light emitting diode (OLED) may include at least two pixel electrodes on a substrate, a pixel defining layer formed between adjacent pixel electrodes, an organic emission layer on each pixel electrode, and a common electrode layer formed on the organic emission layer.

[0247] The substrate may include an insulating material and may have flexibility. Details of the substrate will be described later.

[0248] A line layer including a thin film transistor and the like is formed on the substrate. The line layer may further include a gate line, a sustaining voltage line, a gate insulating layer, a data line, a source electrode, a drain electrode, a semiconductor, a protective layer, and the like. The detailed structure of the line layer may be verified according to the implementation. The gate line and the sustaining voltage line are electrically separated from each other, and the data line is insulated and crosses the gate line and the sustaining voltage line. The gate electrode, the source electrode, and the drain electrode form a control terminal, an input terminal, and an output terminal of the thin film transistor, respectively. The drain electrode is electrically connected to a pixel electrode to be described later.

[0249] The pixel electrode may serve as an anode of the display device. The pixel electrode may be formed of a transparent conductive material such as indium tin oxide (ITO) or indium zinc oxide (IZO). The pixel electrode may be formed of a material having a light blocking property such as gold (Au), platinum (Pt), nickel (Ni), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), cobalt (Co), copper (Cu), palladium (Pd), titanium (Ti), etc. The pixel electrode may have a two-layer structure in which the above-mentioned transparent conductive material and the above-mentioned material having a light blocking property are sequentially stacked.

[0250] Between two adjacent pixel electrodes, a pixel defining layer (PDL) overlaps ends of the pixel electrodes to divide the pixel electrodes into pixel units. The pixel defining layer is an insulating layer that can electrically block the at least two pixel electrodes.

[0251] The pixel defining layer covers a portion of an upper surface of the pixel electrode, and a remaining area of ​​the pixel electrode not covered by the pixel defining layer may provide an opening. An organic emission layer to be described later may be formed on an area defined by the opening.

[0252] The organic emission layer defines each pixel region through the above-mentioned pixel electrode and pixel defining layer. In other words, one pixel region may be defined as a region in which one organic emission unit layer is formed in contact with one pixel electrode divided by the pixel defining layer.

[0253] For example, in the display device according to the embodiment, the organic emission layer may be defined as a first pixel region, a second pixel region, and a third pixel region, and the pixel regions are spaced apart from each other by the pixel defining layer, leaving a predetermined interval.

[0254] The organic emission layer may emit a third light belonging to the visible light region or the UV region. That is, the first to third pixel regions of the organic emission layer may each emit a third light. In an embodiment, the third light may be light with the highest energy in the visible light region, for example, blue light. When all pixel regions of the organic emission layer are designed to emit the same light, for example, light of the same color, the pixel regions of the organic emission layer may all be formed of the same or similar materials or may exhibit the same or similar properties. Therefore, the process difficulty of forming the organic emission layer may be significantly reduced, for example, minimized or avoided, and the display device may be easily applied to large-scale / large-area processes, for example, formed by it. However, the organic emission layer according to the embodiment is not necessarily limited thereto, but the organic emission layer may be designed to emit at least two different lights, for example, at least two different colors of light.

[0255] The organic emission layer may include an organic emission unit layer in each pixel region, and each organic emission unit layer may further include an auxiliary layer (eg, a hole injection layer, a hole transport layer, an electron transport layer, etc.) in addition to the emission layer.

[0256] The common electrode may serve as a cathode of the display device. The common electrode may be formed of a transparent conductive material such as indium tin oxide (ITO) or indium zinc oxide (IZO). The common electrode may be formed on the organic emission layer and may be integrated therewith.

[0257] A planarization layer or a passivation layer may be formed on the common electrode. The planarization layer may include an (eg, transparent) insulating material for providing electrical insulation to the common electrode.

[0258] The absorptive color filter layer may be formed corresponding to each pixel region. The absorptive color filter layer may include a green (G) segment configured to selectively pass green light and absorb (i.e., block) light of other wavelengths, a red (R) segment configured to selectively pass red light and absorb (i.e., block) light of other wavelengths, and a blue (B) segment configured to selectively pass blue light and absorb (i.e., block) green light and red light (e.g., light of a wavelength less than or equal to about 500 nm).

[0259] In an embodiment, the display device may include a stack structure including a (e.g., transparent) substrate and a light-emitting layer disposed on the substrate as a photoluminescent element, wherein in the stack structure, the light-emitting layer may include a pattern of the quantum dot polymer composite and the pattern includes at least one repeating segment that emits light of a predetermined wavelength.

[0260] The stack structure includes a (e.g., transparent) substrate and a light-emitting layer disposed on the substrate and including a pattern of the quantum dot polymer composite, the quantum dot polymer composite including: a polymer matrix; and a plurality of quantum dots dispersed in the polymer matrix, and the plurality of quantum dots include the above-mentioned quantum dots. The pattern of the quantum dot polymer composite includes at least one repeating segment that emits light of a predetermined wavelength. In an embodiment, the pattern of the quantum dot polymer composite includes at least one repeating segment such as a first segment that emits a first light or a second segment that emits a second light.

[0261] The first light and the second light have different maximum photoluminescence peak wavelengths in the photoluminescence spectrum. In an embodiment, the first light may be red light existing at a maximum photoluminescence peak wavelength of about 600nm to about 650nm (e.g., about 620nm to about 650nm), and the second light may be green light existing at a maximum photoluminescence peak wavelength of about 500nm to about 550nm (e.g., about 510nm to about 550nm). The pattern of the quantum dot polymer composite may further include a third segment that emits or transmits a third light (e.g., blue light) that is different from the first light and the second light. The maximum peak wavelength of the third light may be greater than or equal to about 380nm, for example, greater than or equal to about 420nm, greater than or equal to about 430nm, greater than or equal to about 440nm, or greater than or equal to about 445nm and less than or equal to about 480nm, for example, less than or equal to about 470nm, less than or equal to about 460nm, or less than or equal to about 455nm. The light source may emit the third light.

[0262] In the patterned film of the quantum dot polymer composite of the device according to the embodiment, the first segment may be a segment emitting red light, the second segment may be a segment emitting green light, and the light source may be an element emitting blue light. In this case, an optical element for blocking (e.g., reflecting or absorbing) blue light may be provided on the front surface (light emitting surface) of the first segment and the second segment.

[0263] The substrate may be a substrate including an insulating material. The substrate may include: glass; various polymers such as polyesters (e.g., polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polymethacrylate, polyacrylate, etc.); polycarbonate; polysiloxane (e.g., polydimethylsiloxane (PDMS)); inorganic materials such as Al 2 O 3 and ZnO; or a combination thereof, but not limited thereto. The thickness of the substrate may be appropriately selected in consideration of the substrate material, but is not particularly limited thereto. The substrate may be flexible. The substrate may be configured to have a transmittance of greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, or greater than or equal to about 90% for light emitted from the quantum dots.

[0264] In an embodiment, a method for manufacturing the stack structure includes:

[0265] forming a film of the composition on a substrate;

[0266] exposing selected areas of the film to light (exposure) (e.g., a wavelength of less than or equal to about 400 nm); and

[0267] The exposed film is developed with an alkaline developing solution to obtain a pattern of the quantum dot polymer composite. The substrate and the composition are the same as described above. Figure 2 A non-limiting method of forming the above-mentioned pattern is described.

[0268] The composition is coated on a substrate by a suitable method such as spin coating or slit coating to a predetermined thickness (S1). The formed film may be pre-baked (PRB) optionally. The pre-baking may be performed by selecting suitable conditions such as temperature, time, atmosphere, etc. (S2).

[0269] The formed (or optionally pre-baked) film is exposed (EXP) to light having a predetermined wavelength under a mask having a predetermined pattern (S3). The wavelength and intensity of the light can be selected in consideration of the type and amount of the photoinitiator, the type and amount of the quantum dots, etc.

[0270] The exposed film is treated with an alkaline developing (DEV) solution (e.g., dipped or sprayed) to dissolve the unexposed area and obtain the desired pattern (S4). The obtained pattern may be optionally post-baked (POB) to improve the crack resistance and solvent resistance of the pattern, for example, at about 150° C. to about 230° C. for a predetermined time (e.g., greater than or equal to about 10 minutes or greater than or equal to about 20 minutes) (S5).

[0271] When the pattern of the quantum dot-polymer composite has a plurality of (multiple) repeating segments, a quantum dot-polymer composite having a desired pattern can be obtained by preparing a plurality of compositions including quantum dots (e.g., quantum dots emitting red light, green quantum dots, or optionally blue quantum dots) having desired photoluminescent properties (photoluminescent peak wavelength, etc.) for forming each repeating segment, and for each of the above compositions, repeating the formation of the above pattern a necessary number of times (e.g., two or more times or three or more times) (S6). For example, the quantum dot-polymer composite may have a pattern of at least two repeating color segments (e.g., red / green / blue (RGB) segments). The pattern of the quantum dot-polymer composite can be used as a photoluminescent color filter in a display device.

[0272] In an embodiment, the above-mentioned stack structure can be manufactured using an ink composition. The method may include: depositing it on a desired substrate or an organic light emitting diode (e.g., an OLED emitting blue light) described later (e.g., using a suitable system (e.g., a droplet discharge device such as an inkjet or nozzle printing device) (e.g., to provide a desired pattern), and heating it to remove the solvent and polymerize it. The method can provide a highly accurate quantum dot-polymer composite film or pattern in a simple manner and in a short time.

[0273] In the display device according to an embodiment, the light source may include, for example, an organic light emitting diode (OLED).

[0274] Figure 3A and 3B is a schematic cross-sectional view of a display device according to an embodiment. Figure 3A and Figure 3B , the light source may include an organic light emitting diode OLED. For example, the OLED may emit blue light or light having a wavelength in the region of about 500 nm or less.

[0275] The details of the organic light emitting diode OLED are the same as those described above. The OLED may include (at least two) pixel electrodes 90a, 90b, 90c formed on a substrate 100, pixel defining layers 150a, 150b formed between adjacent pixel electrodes 90a, 90b, 90c, organic light emitting layers 140a, 140b, 140c formed on the pixel electrodes 90a, 90b, 90c, and a common electrode layer 130 formed on the organic light emitting layers 140a, 140b, 140c.

[0276] The pixel areas of the OLED may respectively correspond to first, second, and third segment arrangements which will be described in detail below.

[0277] A stack structure including a quantum dot-polymer composite pattern 170 (e.g., including a first repeating segment comprising quantum dots emitting green light, a second repeating segment comprising quantum dots emitting red light, or a combination thereof) and a substrate, or the quantum dot-polymer composite pattern 170 can be disposed on or above a light source, for example, directly on the light source.

[0278] Light (e.g., blue light) emitted from the light source may enter the second segment 21 and the first segment 11 of the pattern to emit (e.g., converted) red light R and green light G, respectively. Blue light B emitted from the light source passes through the third segment 31 or is transmitted from the third segment 31. An optical element 160 may be disposed on the second segment 21 emitting red light, the first segment 11 emitting green light, or a combination thereof. The optical element may be a blue cutoff layer that cuts off (e.g., reflects or absorbs) blue light and optional green light, or a first optical filter. The blue cutoff layer 160 may be disposed on the upper substrate 240. The blue cutoff layer 160 may be disposed between the upper substrate 240 and the quantum dot-polymer composite pattern 170 and on the first segment 11 and the second segment 21. The details of the blue cutoff layer are the same as those described below for the first optical filter 310.

[0279] The above device may be manufactured by separately manufacturing the above stack structure and an OLED (eg, emitting blue light) and then assembling them. The device may be manufactured by directly forming a quantum dot polymer composite pattern on the OLED.

[0280] In an embodiment, the display device may further include a lower substrate 210, an optical element (e.g., a polarizer) 300 disposed below the lower substrate 210, and a liquid crystal layer 220 between the stack structure and the lower substrate 210. The stack structure may be disposed in such a manner that the light emitting layer (i.e., the quantum dot-polymer composite pattern 170) faces the liquid crystal layer. The display device may further include an optical element (e.g., a polarizer) 300 between the liquid crystal layer 220 and the light emitting layer. The light source may further include an LED and an optional light guide plate.

[0281] Non-limiting examples of a display device (eg, a liquid crystal display device) according to an embodiment are described with reference to the accompanying drawings. Figure 4 2 is a schematic cross-sectional view showing a liquid crystal display according to an embodiment. Figure 4 The display device of the embodiment includes a liquid crystal panel 200, a polarizer 300 disposed under the liquid crystal panel 200, and a backlight unit (BLU) disposed under the polarizer 300.

[0282] The liquid crystal panel 200 includes a lower substrate 210, a stack structure, and a liquid crystal layer 220 disposed between the stack structure and the lower substrate. The stack structure includes a transparent substrate 240 and a light emitting layer 230 including a pattern of the quantum dot polymer composite.

[0283] The lower substrate 210, also referred to as an array substrate, may be a transparent insulating material substrate. The substrate is the same as described above. A line plate 211 is provided on the upper surface of the lower substrate 210. The line plate 211 may include a plurality of gate lines and data lines defining pixel areas, a thin film transistor disposed adjacent to the intersection area of ​​the gate lines and the data lines, and a pixel electrode for each pixel area, but is not limited thereto. The details of such a line plate are not particularly limited.

[0284] The liquid crystal layer 220 may be disposed on the line plate 211. The liquid crystal layer 220 may include an alignment layer 211 on and below the layer 220 to initially align the liquid crystal material included therein. Details of the liquid crystal material and the alignment layer (e.g., liquid crystal material, alignment layer material, method of forming the liquid crystal layer, thickness of the liquid crystal layer, etc.) are not particularly limited.

[0285] The lower polarizer 300 is provided below the lower substrate. The material and structure of the polarizer 300 are not particularly limited. A backlight unit (e.g., emitting blue light) may be provided below the polarizer 300. An upper optical element or lower polarizer 300 may be provided between the liquid crystal layer 220 and the transparent substrate 240, but is not limited thereto. For example, the upper polarizer may be provided between the liquid crystal layer 220 and the light emitting layer 230. The polarizer may be any suitable polarizer used in a liquid crystal display device. The polarizer may be TAC (triacetyl cellulose) having a thickness of less than or equal to about 200 μm, but is not limited thereto. In an embodiment, the upper optical element may be a coating that controls the refractive index without a polarization function.

[0286] The backlight unit includes a light source 110. The light source may emit blue light or white light. The light source may include a blue LED, a white LED, a white OLED, or a combination thereof, but is not limited thereto.

[0287] The backlight unit may further include a light guide plate 120. In an embodiment, the backlight unit may be an edge-type lighting device. For example, the backlight unit may include a reflector, a light guide plate provided on the reflector and providing a planar light source for the liquid crystal panel 200, at least one optical sheet on the light guide plate such as a diffuser, a prism sheet, etc., or a combination thereof, but is not limited thereto. The backlight unit may not include a light guide plate. In an embodiment, the backlight unit may be a direct lighting device. For example, the backlight unit may have a reflector and may have a plurality of fluorescent lamps arranged on the reflector at regular intervals, or may have an LED operating substrate on which a plurality of light-emitting diodes may be arranged, a diffuser plate thereon, and optionally at least one optical sheet. The details of such a backlight unit (e.g., light-emitting diodes, fluorescent lamps, light guide plates, various optical sheets, and components of the reflector) are not particularly limited.

[0288] A black matrix (black matrix, BM) 241 is provided below the transparent substrate 240 and has an opening and hides the gate lines, data lines, and thin film transistors of the line board on the lower substrate. For example, the black matrix 241 may have a dot matrix (lattice) shape. The light-emitting layer 230 is provided in the opening of the black matrix 241 and has a pattern including the following quantum dot-polymer composite: a segment (R) configured to emit a first light (e.g., red light), a segment (G) configured to emit a second light (e.g., green light), and a third segment (B) configured to emit / transmit, for example, blue light. If necessary, the light-emitting layer may further include at least one fourth segment. The fourth segment may include quantum dots that emit a color different from the light emitted from the first to third segments (e.g., cyan, magenta, and yellow light).

[0289] In the light emitting layer 230, segments forming a pattern may be repeated corresponding to a pixel region formed on the lower substrate. A transparent common electrode 231 may be provided on the photoluminescent color filter layer.

[0290] The display device may further include a second filter layer 311 (e.g., a red / green or yellow light recycling layer) disposed between the light emitting layer 230 and the liquid crystal layer 220 (e.g., the light emitting layer 230 and the upper polarizer 300) and transmitting at least a portion of the third light and reflecting at least a portion of the first light and the second light. The second filter layer may reflect light in a wavelength region greater than about 500 nm. The first light may be red light, the second light may be green light, and the third light may be blue light.

[0291] The third segment (B) configured to emit / transmit blue light may be a transparent color filter that does not change the light emission spectrum of the light source. In this case, the blue light emitted from the backlight unit may enter in a polarized state and may be emitted as is through the polarizer and the liquid crystal layer. If desired, the third segment may include quantum dots that emit blue light.

[0292] If necessary, the display device may further have a blue light blocking layer (blue cutoff filter) or a first filter layer. The blue light blocking layer or the first filter layer may be provided between the lower surface of the first segment (R) and the second segment (G) and the upper substrate 300 or on the upper surface of the upper substrate. The blue light blocking layer or the first filter layer may be a sheet having an opening in a region corresponding to a pixel region (third segment) displaying blue and thus formed in a region corresponding to the first and second segments. That is, the first filter layer may be as shown in FIG. Figure 4 In the embodiment shown in FIG. 1 , the first filter layer is disposed at a position other than the position overlapping with the third segment and is disposed integrally therewith, but is not limited thereto. For example, at least two first filter layers may be disposed, leaving spaces at respective positions overlapping with the first and second segments.

[0293] The first filter layer may block light having a predetermined wavelength region, for example, in the visible light region and may transmit light in other wavelength regions, and, for example, may block blue light and may transmit light other than blue light. For example, the first filter layer may transmit green light, red light, and / or yellow light as a mixed color thereof.

[0294] The first filter layer may substantially block, for example, blue light having a wavelength less than or equal to about 500 nm, and may have a property of transmitting visible light having a wavelength greater than about 500 nm and less than or equal to about 700 nm.

[0295] For example, for other visible light having a wavelength greater than 500nm and less than or equal to about 700nm, the first filter layer may have a light transmittance greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, or even about 100%.

[0296] The first filter layer may be a polymer film including pigments and dyes that absorb wavelengths to be blocked, and may absorb greater than or equal to about 80%, greater than or equal to about 90%, greater than or equal to about 95% of blue light, but may have a light transmittance of greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, and even about 100% for other visible light having a wavelength greater than about 500 nm and less than or equal to about 700 nm.

[0297] The first filter layer may substantially block (e.g., absorb) blue light having a wavelength of less than or equal to about 500 nm by absorbing it, and it may selectively transmit, for example, green light, or red light. In this case, at least two first filter layers may be provided spaced apart at positions overlapping the first to second segments, respectively. For example, a first filter layer selectively transmitting red light may be provided in a position overlapping a segment emitting red light, and a first filter layer selectively transmitting green light may be provided at a position overlapping a segment emitting green light. For example, the first filter layer may include: a first region that blocks (e.g., absorbs) blue light and red light and selectively transmits light within a predetermined range (e.g., greater than or equal to about 500 nm, greater than or equal to 510 nm, greater than or equal to about 515 nm and less than or equal to about 540 nm, less than or equal to about 535 nm, less than or equal to about 530 nm, less than or equal to about 525 nm, or less than or equal to about 520 nm), a second region that blocks (e.g., absorbs) blue light and green light and selectively transmits light within a predetermined range (e.g., greater than or equal to about 600 nm, greater than or equal to about 610 nm, or greater than or equal to about 615 nm and less than or equal to about 640 nm, less than or equal to about 635 nm, less than or equal to about 630 nm, less than or equal to about 625 nm, or less than or equal to about 620 nm), or a combination thereof. The first region may be disposed at a position overlapping a segment emitting green light, and the second region may be disposed at a position overlapping a segment emitting red light. The first region and the second region may be optically isolated.Such a first filter layer may contribute to an improvement in the color purity of the display device.

[0298] The first filter layer may be a reflective filter including a plurality of layers (e.g., inorganic material layers) having different refractive indices, and, for example, may be formed by alternately stacking two layers having different refractive indices, for example, by alternately stacking a layer having a high refractive index and a layer having a low refractive index. As the refractive index difference between the layer having a high refractive index and the layer having a low refractive index is higher, the first filter layer provided has higher selectivity to wavelength. The thickness and stacking number of the layer having a high refractive index and the layer having a low refractive index may be determined according to the refractive index of each layer and the reflected wavelength, for example, each layer having a high refractive index may have a thickness of about 3 nm to about 300 nm, and each layer having a low refractive index may have a thickness of about 3 nm to about 300 nm.

[0299] The total thickness of the first filter layer may be, for example, about 3 nm to about 10,000 nm, about 300 nm to about 10,000 nm, or about 1,000 nm to about 10,000 nm. All layers with a high refractive index may have the same thickness and different or the same material as each other, and all layers with a low refractive index may have the same thickness and different or the same material as each other.

[0300] The display device may further include a second filter layer (e.g., a red / green or yellow light recycling layer) disposed between the light emitting layer and the liquid crystal layer (e.g., the light emitting layer and the upper polarizer), transmitting at least a portion of the third light, and reflecting at least a portion of the first light and / or the second light. The second filter layer may reflect light in a wavelength region greater than about 500 nm. The first light may be red light, the second light may be green light, and the third light may be blue light.

[0301] In the display device according to the embodiment, the second filter layer may be formed as an integrated layer having a relatively flat surface.

[0302] In an embodiment, the second filter layer may include a single layer having a low refractive index, for example, the second filter layer may be a transparent film having a refractive index of less than or equal to about 1.4, less than or equal to about 1.3, or less than or equal to about 1.2.

[0303] The second filter layer having a low refractive index may be, for example, porous silicon oxide, a porous organic material, a porous organic / inorganic composite, or a combination thereof.

[0304] In an embodiment, the second filter layer may include a plurality of layers having different refractive indices, for example, the second filter layer may be formed by alternately stacking two layers having different refractive indices, or for example, the second filter layer may be formed by alternately stacking a material having a high refractive index and a material having a low refractive index.

[0305] The layer with a high refractive index in the second filter layer may include, for example, hafnium oxide, tantalum oxide, titanium oxide, zirconium oxide, magnesium oxide, cesium oxide, lanthanum oxide, indium oxide, niobium oxide, aluminum oxide, silicon nitride, or a combination thereof, but according to an embodiment, the layer with a high refractive index in the second filter layer may include various materials having a higher refractive index than the layer with a low refractive index.

[0306] The layer with a low refractive index in the second filter layer may include, for example, silicon oxide, but according to an embodiment, the layer with a low refractive index in the second filter layer may include various materials having a lower refractive index than the layer with a high refractive index.

[0307] As the refractive index difference between the layer having a high refractive index and the layer having a low refractive index is higher, the second filter layer may have higher wavelength selectivity.

[0308] In the second filter layer, the respective thicknesses of the layer with a high refractive index and the layer with a low refractive index and the number of stacking thereof may be determined depending on the refractive index of each layer and the wavelength to be reflected, for example, each layer with a high refractive index in the second filter layer may have a thickness of about 3 nm to about 300 nm, and each layer with a low refractive index in the second filter layer may have a thickness of about 3 nm to about 300 nm. The total thickness of the second filter layer may be, for example, about 3 nm to about 10,000 nm, about 300 nm to about 10,000 nm, or about 1,000 nm to about 10,000 nm. The layer with a high refractive index and the layer with a low refractive index in the second filter layer may each have the same thickness and material or different thicknesses and materials from each other.

[0309] The second filter layer may reflect at least a portion of the first light (R) and the second light (G) and transmit at least a portion (e.g., all) of the third light (B). For example, the second filter layer may transmit only the third light (B) in a blue light wavelength region less than or equal to about 500 nm, and light in a wavelength region greater than about 500 nm, i.e., green light (G), yellow light, red light (R), etc., may not pass through the second filter layer and be reflected. Therefore, the reflected green light and red light may pass through the first and second segments to be emitted to the outside of the display device.

[0310] The second filter layer may reflect a wavelength region greater than about 500 nm by greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, or about 100%.

[0311] At the same time, the second filter layer may have a transmittance in the wavelength region less than or equal to about 500 nm of, for example, greater than or equal to about 90%, greater than or equal to about 92%, greater than or equal to about 94%, greater than or equal to about 96%, greater than or equal to about 98%, greater than or equal to about 99%, or even about 100%.

[0312] Embodiments provide electronic devices including the above quantum dots. The device may include a light emitting diode (LED), an organic light emitting diode (OLED), a sensor, a solar cell, an imaging sensor, or a liquid crystal display (LCD), but is not limited thereto.

[0313] Hereinafter, the embodiments will be described in more detail with reference to Examples. However, they are illustrative examples of the present disclosure, and the present disclosure is not limited thereto.

[0314] Example

[0315] Analytical methods

[0316] 1. Ultraviolet-visible (UV-Vis) spectroscopy

[0317] UV spectroscopy analysis was performed using an Agilent Cary 5000 spectrometer and UV-visible absorption spectra were obtained.

[0318] 2. Photoluminescence Analysis

[0319] A Hitachi F-7000 spectrometer was used to obtain the photoluminescence (PL) spectrum of the fabricated quantum dots at a wavelength of 450 nanometers (nm). During the spectral analysis, the solution had a concentration such that the optical density for UV-Vis 458 nm was 0.09-0.11. The excitation light had a wavelength of about 458 nm.

[0320] 3. Absolute quantum efficiency (quantum yield) of quantum dots

[0321] Photoluminescence spectroscopy was performed using an Otsuka Electronics QE-2100 spectrometer at a radiation wavelength of 450 nm. The maximum photoluminescence peak wavelength, quantum efficiency, and full width at half maximum (FWHM) were evaluated from the photoluminescence spectrum.

[0322] 4. Inductively coupled plasma (ICP) analysis

[0323] Inductively coupled plasma atomic emission spectrometry (ICP-AES) was performed by using Shimadzu ICPS-8100.

[0324] Reference Example 1-1:

[0325] In a 200 milliliter (mL) reaction flask, indium acetate, zinc acetate, and palmitic acid were dissolved in 1-octadecene, and the solution was heated at 120°C under vacuum. Indium and palmitic acid were used in a 1:3 molar ratio. After 1 hour, the atmosphere in the reactor was replaced with nitrogen. After the reactor was heated at 280°C, tris(trimethylsilyl)phosphine (TMS) as a phosphorus precursor was quickly added. 3 A mixed solution of indium (P) and trioctylphosphine was injected therein, and the reaction was carried out for 20 minutes. The reaction solution was quickly cooled to room temperature, acetone was added thereto, the mixture was centrifuged to obtain a precipitate, and the precipitate was dispersed again in toluene. According to 1 mol of indium, TMS 3 The amounts of P and zinc acetate are about 0.5 mol and 0.5 mol, respectively. The InZnP core obtained therefrom has a size of about 2-3 nm.

[0326] Reference Example 1-2:

[0327] InZnP cores were prepared in the same manner as described in Reference Example 1-1, except that the phosphorus precursor was injected, and then another indium precursor was added thereto, and at the later part of the reaction, the phosphorus precursor was added again.

[0328] Reference Example 2:

[0329] A Sn-added InZnP core was obtained according to the same method as Reference Example 1-2, except that Sn acetate was further added as a tin compound in an amount of about 0.03 mol relative to 1 mol of indium during the reaction.

[0330] Comparative Example 1

[0331] (1) Selenium was dispersed in trioctylphosphine to prepare a Se / TOP stock solution (stock solution), and sulfur was dispersed in trioctylphosphine to prepare a S / TOP stock solution.

[0332] Zinc acetate and oleic acid were dissolved in trioctylamine in a 200 mL reaction flask, and the solution was vacuum treated at 120° C. for 10 minutes.

[0333] In use N 2After the interior of the reaction flask was replaced, the temperature of the obtained solution was raised to 180° C. and the core toluene dispersion of Reference Example 1-1 was injected into the solution. After 20 minutes, a predetermined amount of Se / TOP and an optional predetermined amount of zinc acetate were injected into the reaction flask three times while the reactor temperature was raised to 320° C. The reaction was performed to obtain a reaction solution including particles having a ZnSe shell disposed on the core. The reaction took a total of 100 minutes.

[0334] Subsequently, S / TOP stock solution and a predetermined amount of zinc acetate were injected into the reaction solution at the reaction temperature. The reaction was performed to obtain a reaction solution including particles having a ZnS shell disposed on the ZnSe shell. The reaction took 100 minutes.

[0335] In the reaction, the total amount of Se was 6 moles, the total amount of S was 27 moles, and the total amount of zinc was 26 moles based on 1 mole of indium.

[0336] An excess of ethanol was added to the reactant including the obtained core / multi-layer shell quantum dots, and the mixture was centrifuged. After centrifugation, the supernatant was discarded therefrom, the precipitate therein was separated and dried, and then redispersed in chloroform or toluene to obtain a quantum dot solution (hereinafter, QD solution).

[0337] (2) ICP-AES of the obtained QDs was analyzed, and the results are shown in Table 1. UV-Vis spectral analysis and photoluminescence analysis of the QDs were performed. The results are shown in Table 2. The photoluminescence spectrum of the quantum dots is shown in Figure 7 middle.

[0338] Example 1

[0339] Core / multi-layer shell quantum dots were obtained according to the same method as Comparative Example 1, except that the core prepared in Reference Example 1-2 was used and the core injection temperature was lowered to 100° C., and the shell precursor and ammonium fluoride were injected.

[0340] ICP-AES analysis of the QDs was performed and the results are shown in Table 1. UV-Vis spectroscopic analysis and photoluminescence analysis of the QDs were performed. The results are shown in Tables 2 and Figure 5 middle.

[0341] Example 2

[0342] Core / multi-layer shell quantum dots were obtained according to the same method as in Example 1, except that 8 mol of Se, 33 mol of S, and 33 mol of zinc were used relative to 1 mol of indium.

[0343] ICP-AES analysis of the QDs was performed and the results are shown in Table 1. UV-Vis spectroscopy and photoluminescence analysis of the QDs were performed. The results are shown in Table 2 and Figure 6 and Figure 7 middle.

[0344] Example 3

[0345] Core / multi-layer shell quantum dots were obtained according to the same method as Example 1, except that the core prepared in Reference Example 2 was used.

[0346] ICP-AES analysis of the QDs was performed, and the results are shown in Table 1. UV-Vis spectroscopy analysis and photoluminescence analysis of the QDs were performed, and the results are shown in Table 2.

[0347] Table 1

[0348]

[0349] Table 2

[0350]

[0351] Referring to the results of the above table, the quantum dots according to the embodiment have a reduced Stokes shift and show a narrow full width at half maximum (FWHM), compared with the quantum dots according to the comparative example.

[0352] Figure 7 The results show that the quantum dots of the embodiment may have a shorter tail region compared with the quantum dots of the comparative example.

[0353] Experimental Example: Color Reproducibility Measurement Results under BT2020 Standard

[0354] An optical spectrum of light emitted from a light conversion layer including the prepared QDs was obtained, and then a color gamut was calculated under the BT2020 standard through simulation.

[0355] The quantum dot-polymer composite was prepared by the following process. The quantum dots were separated from the quantum dot dispersion by non-solvent precipitation and centrifugation. The separated quantum dots were mixed with a monomer combination for an acrylic polymer to obtain a mixture, which was then applied to a substrate and a barrier film was covered thereon, and the resulting structure was cured.

[0356] The results are shown in Table 3 and Figure 8 (Example 1).

[0357] Table 3

[0358] BT2020 color reproducibility (%) Comparative Example 1 89 Example 1 91 Example 2 91 Example 3 90

[0359] From the results, the quantum dot-polymer composite including the quantum dots of the embodiment can achieve relatively high color reproducibility without a color filter.

[0360] While the present disclosure has been described with respect to what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but, on the contrary, is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. Quantum dots, including a semiconductor nanocrystal core and a semiconductor nanocrystal shell disposed on the semiconductor nanocrystal core, wherein the quantum dots do not include cadmium, The core includes a Group III-V compound including a Group III metal and a Group V element, and The quantum dots have a maximum photoluminescence peak in the green light wavelength region, The half width of the maximum photoluminescence peak is less than 50 nanometers, The difference between the wavelength of the maximum photoluminescence peak and the first absorption peak wavelength of the quantum dots is less than or equal to 23 nanometers, and The quantum dots have a quantum yield greater than or equal to 85%. 2 . The quantum dot of claim 1 , wherein the green light wavelength region is greater than or equal to 500 nanometers and less than or equal to 560 nanometers.

3. The quantum dot of claim 1, wherein the half width of the maximum photoluminescence peak is less than or equal to 35 nanometers.

4. The quantum dot of claim 1, wherein the quantum dot comprises indium and zinc. 5 . The quantum dot of claim 1 , wherein the quantum dot has a size greater than or equal to 5 nanometers and less than or equal to 8 nanometers. The quantum dot of claim 1 , wherein the quantum dot has a quantum yield greater than or equal to 86%.

7. The quantum dot of claim 1, wherein the quantum dot further comprises an additive comprising a Group IV element, As, Sb, Bi, Te, or a combination thereof.

8. The quantum dot of claim 1, wherein the shell comprises a first semiconductor nanocrystalline shell comprising zinc and selenium and a second semiconductor nanocrystalline shell disposed on the first semiconductor nanocrystalline shell, the second semiconductor nanocrystalline shell comprising zinc and sulfur.

9. The quantum dot of claim 8, wherein the first semiconductor nanocrystal shell is disposed directly on the surface of the semiconductor nanocrystal core, and The first semiconductor nanocrystal shell does not include sulfur.

10. The quantum dot of claim 8, wherein the first semiconductor nanocrystal shell has a thickness less than or equal to 6 monolayers.

11. The quantum dot of claim 8, wherein the second semiconductor nanocrystal shell is the outermost layer of the quantum dot.

12. The quantum dot of claim 8, wherein the second semiconductor nanocrystalline shell is disposed directly on the first semiconductor nanocrystalline shell, and the second semiconductor nanocrystalline shell comprises ZnSeS, ZnS, or a combination thereof.

13. The quantum dot of claim 1, wherein in the photoluminescence spectrum of the quantum dot, a ratio of the intensity at the tail start wavelength to the intensity at the maximum photoluminescence peak wavelength is less than or equal to 0.11:1, the tail refers to a portion of the photoluminescence spectrum curve present in a wavelength region at least 50 nm greater than the maximum photoluminescence peak wavelength, and the tail start wavelength is the wavelength at which the tail starts.

14. The quantum dot of claim 8, wherein the second semiconductor nanocrystal shell has a thickness of less than 0.7 nanometers.

15. The quantum dot according to claim 7, wherein the molar amount of the additive is less than 0.1 mole relative to 1 mole of the Group III metal.

16. The quantum dot of claim 1, wherein the core comprises indium, phosphorus, and optionally zinc, and the shell comprises zinc, sulfur, and selenium. 17 . The quantum dot of claim 16 , wherein in the quantum dot, a molar ratio of sulfur to selenium relative to indium ((S+Se) / In) is greater than or equal to 20:1 and less than or equal to 36:

1. 18 . The quantum dot of claim 16 , wherein in the quantum dot, a molar ratio of phosphorus to indium is greater than or equal to 0.6:1 and less than or equal to 0.9:

1. 19 . The quantum dot of claim 16 , wherein in the quantum dot, a molar ratio of zinc to indium is greater than or equal to 25:1 and less than or equal to 40:

1.

20. The quantum dots of claim 1, wherein the quantum dots have an average size greater than or equal to 5.5 nanometers.

21. The quantum dot of claim 1, wherein the difference between the wavelength of the maximum photoluminescence peak and the first absorption peak wavelength of the quantum dot is less than or equal to 20 nanometers.

22. A method for producing a quantum dot as claimed in any one of claims 1 to 21, include: preparing a semiconductor nanocrystal core comprising a Group III-V compound; preparing a first solution including a shell metal precursor and an organic ligand; adding the semiconductor nanocrystal cores to the first solution at a first temperature; and heating the first solution including the semiconductor nanocrystal core to a second temperature and adding a shell non-metal precursor to the first solution to form a semiconductor nanocrystal shell on the surface of the semiconductor nanocrystal core and to produce the quantum dot, Wherein the first temperature is less than or equal to 150°C and the second temperature is greater than or equal to 290°C and less than or equal to 350°C.

23. The method of claim 22, wherein the first temperature is less than or equal to 120°C and the second temperature is greater than or equal to 300°C and less than or equal to 330°C.

24. The method of claim 22, wherein the forming of the semiconductor nanocrystal shell comprises adding the shell non-metal precursor and optional shell metal precursor to the first solution at least twice.

25. The method of claim 22, wherein the method further comprises adding ammonium fluoride, a Group IV element, or a combination thereof to the first solution during formation of the semiconductor nanocrystal shell.

26. The method of claim 22, wherein a Group V element precursor is added at least twice during preparation of the semiconductor nanocrystal core, during formation of the semiconductor nanocrystal shell, or both.

27. A composition comprising the quantum dots of any one of claims 1-21.

28. A composite comprising the quantum dots according to any one of claims 1 to 21.

29. An electronic device comprising the quantum dots as claimed in any one of claims 1 to 21.