Light emitting diode chip and preparation method thereof

By setting multiple sub-gallium nitride layers on the substrate surface of the light emitting diode chip to form a three-dimensional/two-dimensional alternating structure, the problem of low luminescence efficiency caused by non-radiation defects in the traditional method is solved, and high crystal quality and high luminescence efficiency are achieved. LED chip.

CN110752275BActive Publication Date: 2024-11-12ELEC TECH OPTOELECTRONICS TECHWUHUCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911118780.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-11-15
Publication Date
2024-11-12
Estimated Expiration
2039-11-15

AI Technical Summary

Technical Problem

Non-radiation defects caused by traditional GaN-based epitaxial sheet growth methods affect the low luminescence efficiency of the light emitting diode chip, and lattice mismatch and thermal mismatch of the substrate substrate and epitaxial layer lead to deep non-radiation luminescence forming in the composite center.

Method used

By setting multiple sub-gallium nitride layers on the substrate surface, a three-dimensional/two-dimensional alternating structure is formed, alternating from island to layered growth forms, reducing non-radiative defects and improving crystal quality, and using multi-layer three-dimensional/two-dimensional alternating Structure and mesh structure to turn and merge defects.

Benefits of technology

The luminous efficiency of the light emitting diode chip is significantly improved, the underlying defects are reduced, and the high crystal quality LED structure is obtained, which enhances the brightness and light efficiency of the chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110752275B_ABST
    Figure CN110752275B_ABST
Patent Text Reader

Abstract

The present application provides a light-emitting diode chip and a method for preparing the same. A plurality of three-dimensional island structures are arranged on the surface of the buffer layer away from the substrate. The second undoped gallium nitride sublayer is arranged on the surface of the plurality of three-dimensional island structures, covering the plurality of three-dimensional island structures. The second undoped gallium nitride sublayer is a two-dimensional layered structure. At this time, a three-dimensional / two-dimensional alternating structure can be formed by the plurality of three-dimensional island structures and the second undoped gallium nitride sublayer. Thus, the non-radiative defects will turn in direction at the interface where the three-dimensional island structure alternates with the two-dimensional layered structure, thereby causing some defects to turn and merge and annihilate. Moreover, by including a plurality of sub-gallium nitride layers in the undoped gallium nitride layer, a multi-level three-dimensional / two-dimensional alternating structure can be realized, so that most of the non-radiative defects turn in direction and merge and annihilate, thereby greatly reducing the bottom layer defects, obtaining a high-crystalline quality epitaxial wafer, and improving the luminous efficiency of the chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a light emitting diode chip and a method for preparing the same. Background Art

[0002] Light-Emitting Diode (LED) is a semiconductor electronic component that can emit light. It is popular because of its small size, low energy consumption, long life, and low driving voltage, and is widely used in indicator lights, display screens and other fields. The crystal quality of the epitaxial wafer is the key to affecting the brightness of the chip. Therefore, improving the crystal quality and increasing the luminous efficiency of the chip are the key to preparing high-brightness and high-efficiency LED devices.

[0003] The traditional method of growing GaN-based epitaxial wafers is to use chemical vapor deposition to sequentially grow a buffer layer, an undoped uGaN layer, an N-type nGaN layer, a multi-quantum well light-emitting layer, and a P-type pGaN layer on the substrate layer. The traditional light-emitting diode chip structure has a large number of non-radiative defects due to the lattice mismatch and thermal mismatch between the substrate and the epitaxial layer (GaN). The non-radiative defects extend all the way to the light-emitting quantum well to form deep recombination centers, resulting in non-radiative luminescence, thereby affecting the luminous efficiency, making the luminous efficiency of traditional light-emitting diode chips low. Summary of the invention

[0004] Based on this, it is necessary to provide a light emitting diode chip with high light emitting efficiency and a preparation method thereof to address the problem of low light emitting efficiency of traditional light emitting diode chips.

[0005] The present application provides a light-emitting diode chip including a substrate, a buffer layer and an undoped gallium nitride layer. The buffer layer is disposed on the surface of the substrate. The undoped gallium nitride layer is disposed on the surface of the buffer layer away from the substrate. The undoped gallium nitride layer includes a plurality of sub-gallium nitride layers. The plurality of sub-gallium nitride layers are sequentially disposed on the surface of the buffer layer away from the substrate. Each of the sub-gallium nitride layers includes a first undoped gallium nitride sublayer and a second undoped gallium nitride sublayer. The first undoped gallium nitride sublayer is disposed on the surface of the buffer layer away from the substrate. The second undoped gallium nitride sublayer is disposed on the surface of the first undoped gallium nitride sublayer away from the buffer layer. The first undoped gallium nitride sublayer includes a plurality of three-dimensional island structures. The plurality of three-dimensional island structures are sequentially arranged on the surface of the buffer layer away from the substrate. The second undoped gallium nitride sublayer is disposed on the surface of the plurality of three-dimensional island structures away from the buffer layer.

[0006] In one embodiment, the second undoped gallium nitride sublayer is a two-dimensional layered structure, and is disposed on a surface of the plurality of three-dimensional island structures away from the buffer layer.

[0007] In one embodiment, each of the gallium nitride sub-layers further comprises a silicon nitride layer. The silicon nitride layer is disposed on a surface of the second undoped gallium nitride sub-layer away from the first undoped gallium nitride sub-layer.

[0008] In one embodiment, each of the sub-gallium nitride layers further includes a third undoped gallium nitride sub-layer. The third undoped gallium nitride sub-layer is disposed on a surface of the silicon nitride layer away from the second undoped gallium nitride sub-layer.

[0009] In one embodiment, each of the gallium nitride sub-layers further includes a heat treatment layer. The heat treatment layer is disposed on a surface of the third undoped gallium nitride sub-layer away from the silicon nitride layer.

[0010] In one embodiment, the first undoped gallium nitride sub-layers of two adjacent gallium nitride sub-layers among the plurality of gallium nitride sub-layers are disposed on a surface of the heat treatment layer away from the third undoped gallium nitride sub-layer.

[0011] In one embodiment, the undoped gallium nitride layer includes 5 to 50 sub-gallium nitride layers.

[0012] In one embodiment, a method for preparing a light emitting diode chip includes:

[0013] S10, providing a substrate, wherein a buffer layer is prepared on the surface of the substrate;

[0014] S20, preparing a first undoped gallium nitride sublayer on a surface of the buffer layer away from the substrate according to a first preset temperature and a first preset pressure in an environment of a temperature of 1070° C. to 1110° C. and a pressure of 250 torr to 450 torr;

[0015] S30, preparing a second undoped gallium nitride sublayer on a surface of the first undoped gallium nitride sublayer away from the buffer layer under a variable temperature and pressure environment of 1100° C. to 1140° C. and 100 torr to 250 torr;

[0016] S40, preparing a silicon nitride layer on a surface of the second undoped gallium nitride sublayer away from the first undoped gallium nitride sublayer according to a second preset temperature and a second preset pressure under an environment of a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr;

[0017] S50, preparing a third undoped gallium nitride sublayer on a surface of the silicon nitride layer away from the second undoped gallium nitride sublayer according to a third preset temperature and a third preset pressure under an environment of a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr;

[0018] S60 , preparing a heat treatment layer on a surface of the third undoped gallium nitride sublayer away from the silicon nitride layer according to a fourth preset temperature and a fourth preset pressure in an environment of a temperature of 1130° C. to 1170° C. and a pressure of 100 torr to 250 torr.

[0019] In one embodiment, the method for preparing a light emitting diode chip further comprises:

[0020] S70, according to the steps S20 to S60, cyclically preparing the first undoped gallium nitride sublayer, the second undoped gallium nitride sublayer, the silicon nitride layer, the third undoped gallium nitride sublayer and the heat treatment layer in sequence on the surface of the heat treatment layer away from the third undoped gallium nitride sublayer.

[0021] In one embodiment, in step S30, the second undoped gallium nitride sublayer is prepared on the surface of the first undoped gallium nitride sublayer away from the buffer layer in a variable temperature and pressure environment with a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr, in which the temperature gradually increases and the pressure gradually decreases.

[0022] The present application provides a light-emitting diode chip as described above. The buffer layer is provided with the plurality of three-dimensional island structures on the surface away from the substrate, and the second undoped gallium nitride sublayer is provided on the surface of the plurality of three-dimensional island structures to cover the plurality of three-dimensional island structures. The second undoped gallium nitride sublayer is a two-dimensional layered structure. At this time, a three-dimensional / two-dimensional alternating structure can be formed by the plurality of three-dimensional island structures and the second undoped gallium nitride sublayer, that is, the growth form alternates from island to layer. As a result, non-radiative defects will turn in direction at the interface where the three-dimensional island structure alternates to the two-dimensional layered structure, thereby causing some defects to turn and merge and annihilate, thereby obtaining an LED structure with higher crystal quality, thereby increasing the luminous efficiency of the light-emitting diode chip.

[0023] Furthermore, since the undoped gallium nitride layer includes a plurality of sub-gallium nitride layers, a multi-level three-dimensional / two-dimensional alternating structure can be realized, so that most of the non-radiative defects are redirected and merged and annihilated, thereby greatly reducing the bottom layer defects, obtaining high-crystal quality epitaxial wafers, and improving the luminous efficiency of the chip. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the structure of the undoped gallium nitride layer of the light-emitting diode chip provided in the present application;

[0025] Figure 2 A schematic diagram of the cross-sectional structure of the three-dimensional island structure provided in this application;

[0026] Figure 3A schematic diagram of a top view of a three-dimensional island structure provided in this application;

[0027] Figure 4 A schematic diagram of the process flow of the light emitting diode chip preparation method provided in this application;

[0028] Figure 5 A schematic diagram of the structure of an undoped gallium nitride layer in an embodiment provided in the present application.

[0029] Description of Reference Numerals

[0030] Light-emitting diode chip, substrate 10, buffer layer 20, undoped gallium nitride layer 30, sub-gallium nitride layer 310, first undoped gallium nitride sublayer 311, second undoped gallium nitride sublayer 312, three-dimensional island structure 3111, silicon nitride layer 313, third undoped gallium nitride sublayer 314, heat-treated layer 315, N-type semiconductor layer 40, multi-quantum well layer 50, and P-type semiconductor layer 60. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below through embodiments and in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0032] The serial numbers assigned to the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings). In the description of this application, it should be understood that the orientation or position relationship indicated by the terms "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing this application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to this application.

[0033] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0034] See also Figure 1 The present application provides a light-emitting diode chip including a substrate 10, a buffer layer 20 and an undoped gallium nitride layer 30. The buffer layer 20 is disposed on the surface of the substrate 10. The undoped gallium nitride layer 30 is disposed on the surface of the buffer layer 20 away from the substrate 10. The undoped gallium nitride layer 30 includes a plurality of sub-gallium nitride layers 310. The plurality of sub-gallium nitride layers 310 are sequentially disposed on the surface of the buffer layer 20 away from the substrate 10. Each of the sub-gallium nitride layers 310 includes a first undoped gallium nitride sublayer 311 and a second undoped gallium nitride sublayer 312. The first undoped gallium nitride sublayer 311 is disposed on the surface of the buffer layer 20 away from the substrate 10. The second undoped gallium nitride sublayer 312 is disposed on the surface of the first undoped gallium nitride sublayer 311 away from the buffer layer 20. The first undoped gallium nitride sublayer 311 includes a plurality of three-dimensional island structures 3111. The plurality of three-dimensional island structures 3111 are sequentially arranged on a surface of the buffer layer 20 away from the substrate 10 . The second undoped gallium nitride sublayer 312 is disposed on a surface of the plurality of three-dimensional island structures 3111 away from the buffer layer 20 .

[0035] The buffer layer 20 is provided with the plurality of three-dimensional island structures 3111 on the surface away from the substrate 10, and the second undoped gallium nitride sublayer 312 is provided on the surface of the plurality of three-dimensional island structures 3111, covering the plurality of three-dimensional island structures 3111. The second undoped gallium nitride sublayer 312 is a two-dimensional layered structure. At this time, a three-dimensional / two-dimensional alternating structure can be formed by the plurality of three-dimensional island structures 3111 and the second undoped gallium nitride sublayer 312, that is, alternating from island-like to layered growth forms. As a result, non-radiative defects will turn in direction at the interface where the three-dimensional island structure alternates to the two-dimensional layered structure, thereby causing some defects to turn to merge and annihilate, thereby obtaining an LED structure with higher crystal quality, and increasing the luminous efficiency of the light-emitting diode chip.

[0036] Furthermore, since the undoped gallium nitride layer 30 includes a plurality of sub-gallium nitride layers 310, a multi-level three-dimensional / two-dimensional alternating structure can be realized, so that most of the non-radiative defects are redirected and merged and annihilated, thereby greatly reducing the bottom layer defects, obtaining a high-crystal quality epitaxial wafer, and improving the luminous efficiency of the chip.

[0037] See also Figure 2-3 In one embodiment, the second undoped gallium nitride sublayer 312 is a two-dimensional layered structure, and is disposed on a surface of the plurality of three-dimensional island structures 3111 away from the buffer layer 20 .

[0038] Among them, the three-dimensional island structure 3111 can be understood as a frustum structure. The two-dimensional layered structure can be understood as a film layer with a certain thickness. When the second undoped gallium nitride sublayer 312 is arranged on the surface of the multiple three-dimensional island structures 3111 away from the buffer layer 20, the multiple three-dimensional island structures 3111 can be covered. At this time, a plurality of gaps are formed between the second undoped gallium nitride sublayer 312 and the multiple three-dimensional island structures 3111. In addition, non-radiative defects will turn in multiple directions at the interface where the three-dimensional island structure alternates to the two-dimensional layered structure, so that the non-radiative defects transfer direction and then slowly merge and annihilate. Thus, through the three-dimensional / two-dimensional alternating structure, a LED structure with higher crystal quality can be obtained, which improves the luminous efficiency of the light-emitting diode chip.

[0039] In one embodiment, each of the GaN sub-layers 310 further includes a silicon nitride layer 313 . The silicon nitride layer 313 is disposed on a surface of the second undoped GaN sub-layer 312 away from the first undoped GaN sub-layer 311 .

[0040] The silicon nitride (SiN) layer 313 may be configured as a mesh structure. The silicon nitride (SiN) layer 313 is disposed on the surface of the second undoped gallium nitride sublayer 312 away from the first undoped gallium nitride sublayer 311, and may block some defects from extending upward. Moreover, some defects may be deflected when passing through the mesh holes of the silicon nitride (SiN) layer 313, and then merged and annihilated, which may further reduce defects, improve crystal quality, and thus improve the luminous efficiency of the light-emitting diode chip.

[0041] In one embodiment, each of the GaN sub-layers 310 further includes a third undoped GaN sub-layer 314 . The third undoped GaN sub-layer 314 is disposed on a surface of the silicon nitride layer 313 away from the second undoped GaN sub-layer 312 .

[0042] The third undoped gallium nitride sublayer 314 is disposed on the surface of the silicon nitride layer 313, and can cover the mesh structure formed by the silicon nitride (SiN) layer 313. Thus, a plurality of mesh gaps are formed at the interface between the third undoped gallium nitride sublayer 314 and the silicon nitride (SiN) layer 313. At the same time, a plurality of mesh gaps are also formed at the interface between the second undoped gallium nitride sublayer 312 and the silicon nitride (SiN) layer 313. At this time, the direction of some defects can be turned by the mesh gap structure at the interface position, and annihilation is achieved and merged, thereby improving the luminous efficiency of the light-emitting diode chip.

[0043] In one embodiment, each of the GaN sub-layers 310 further includes a heat treatment layer 315 . The heat treatment layer 315 is disposed on a surface of the third undoped GaN sub-layer 314 away from the silicon nitride layer 313 .

[0044] The heat treatment layer 315 is subjected to high temperature and high H 2 The third undoped gallium nitride sublayer 314 is formed by treating the interface of the third undoped gallium nitride sublayer 314 with an atmosphere. At this time, the heat treatment layer 315 is formed by treating the surface of the third undoped gallium nitride sublayer 314 away from the silicon nitride layer 313. The heat treatment layer 315 makes the surface of the third undoped gallium nitride sublayer 314 away from the silicon nitride layer 313 smoother, thereby covering the defects formed by the unflattened crystal growth of the entire layer, thereby obtaining a LED structure with higher crystal quality, thereby improving the luminous efficiency of the light-emitting diode chip.

[0045] See also Figure 5 In one embodiment, the first undoped gallium nitride sub-layers 311 of two adjacent gallium nitride sub-layers 310 among the plurality of gallium nitride sub-layers 310 are disposed on a surface of the heat treatment layer 315 away from the third undoped gallium nitride sub-layer 314 .

[0046] The undoped gallium nitride layer 30 includes a plurality of sub-gallium nitride layers 310, and the plurality of sub-gallium nitride layers 310 are sequentially stacked and arranged on the surface of the buffer layer 20 away from the substrate 10. At this time, the first undoped gallium nitride sub-layer 311 in each adjacent sub-gallium nitride layer 310 is in contact with the heat treatment layer 315. Since each of the sub-gallium nitride layers 310 includes a three-dimensional / two-dimensional alternating structure and a mesh structure, the undoped gallium nitride layer 30 may include a plurality of three-dimensional / two-dimensional alternating structures and mesh structures. Thus, through a plurality of three-dimensional / two-dimensional alternating structures and mesh structures, most defects can be turned in multiple directions, so that the defect transfer direction is gradually merged and annihilated, thereby obtaining an LED structure with higher crystal quality and improving the luminous efficiency of the light-emitting diode chip.

[0047] In one embodiment, the undoped gallium nitride layer 30 includes 5 to 50 gallium nitride sub-layers 310 .

[0048] The number of the plurality of sub-gallium nitride layers 310 included in the undoped gallium nitride layer 30 may be 5 to 50. Within this range of 5 to 50, most defects can be eliminated by the plurality of sub-gallium nitride layers 310, and cost can be saved by limiting the number of the sub-gallium nitride layers 310.

[0049] In one embodiment, the light emitting diode chip further includes an N-type semiconductor layer 40 . The N-type semiconductor layer 40 is disposed on a surface of the undoped gallium nitride layer 30 away from the buffer layer 20 .

[0050] In one embodiment, the light emitting diode chip further includes a multi-quantum well layer 50 . The multi-quantum well layer 50 is disposed on a surface of the N-type semiconductor layer 40 away from the undoped gallium nitride layer 30 .

[0051] The multi-quantum well layer 50 is disposed on the surface of the N-type semiconductor layer 40 away from the undoped gallium nitride layer 30 , which can prevent defects formed at the substrate 10 from extending to the multi-quantum well layer 50 and avoid non-radiative luminescence caused by defects.

[0052] In one embodiment, the light emitting diode chip further includes a P-type semiconductor layer 60 . The P-type semiconductor layer 60 is disposed on a surface of the multi-quantum well layer 50 away from the N-type semiconductor layer 40 .

[0053] The multiple three-dimensional / two-dimensional alternating structures and mesh structures included in the undoped gallium nitride layer 30 eliminate a large number of defects and improve the crystal quality. In addition, the undoped gallium nitride layer 30 solves the problems of leakage current and poor antistatic ability caused by defects, and avoids the defects extending to the multi-quantum well layer 50 to generate defective non-radiative luminescence. Therefore, the undoped gallium nitride layer 30 improves the luminous efficiency of the light-emitting diode chip.

[0054] See also Figure 4 In one embodiment, a method for preparing a light emitting diode chip includes:

[0055] S10, providing a substrate 10, wherein a buffer layer 20 is prepared on the surface of the substrate 10;

[0056] S20, preparing a first undoped gallium nitride sublayer 311 on a surface of the buffer layer 20 away from the substrate 10 according to a first preset temperature and a first preset pressure in an environment of a temperature of 1070° C. to 1110° C. and a pressure of 250 torr to 450 torr;

[0057] S30, forming a second undoped gallium nitride sublayer 312 on a surface of the first undoped gallium nitride sublayer 311 away from the buffer layer 20 under a variable temperature and pressure environment of 1100° C. to 1140° C. and 100 torr to 250 torr;

[0058] S40, forming a silicon nitride layer 313 on a surface of the second undoped gallium nitride sublayer 312 away from the first undoped gallium nitride sublayer 311 according to a second preset temperature and a second preset pressure in an environment of a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr;

[0059] S50, preparing a third undoped gallium nitride sublayer 314 on a surface of the silicon nitride layer 313 away from the second undoped gallium nitride sublayer 312 according to a third preset temperature and a third preset pressure in an environment of a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr;

[0060] S60 , in an environment of a temperature of 1130° C. to 1170° C. and a pressure of 100 torr to 250 torr, a heat treatment layer 315 is prepared on a surface of the third undoped gallium nitride sublayer 314 away from the silicon nitride layer 313 according to a fourth preset temperature and a fourth preset pressure.

[0061] In the step S20, the first undoped gallium nitride sublayer 311 is grown in a metal organic chemical vapor deposition (MOCVD) machine, and a TMGA source is introduced in a nitrogen-hydrogen-ammonia mixed atmosphere to react and grow. Among them, the first preset temperature is set in the temperature range of 1070°C to 1110°C, and the first preset pressure is set in the range of 250torr to 450torr. The first preset temperature is a fixed value in the temperature range of 1070°C to 1110°C, and the first preset pressure is a fixed value in the pressure range of 250torr to 450torr. A constant temperature and pressure environment is set according to the first preset temperature and the first preset pressure, and the first undoped gallium nitride sublayer 311 is prepared on the surface of the buffer layer 20 away from the substrate 10.

[0062] The thickness of the first undoped gallium nitride sublayer 311 can be 0.05um to 0.5um. By preparing the first undoped gallium nitride sublayer 311 with a thickness of 0.05um to 0.5um, it can be ensured that the thickness can fill the substrate pattern and reduce defects to an appropriate range on the basis of minimizing costs. The crystal growth quality can be optimized within the temperature range of 1070℃ to 1110℃, and the crystal growth speed can be optimized, which solves the problems of poor crystal growth quality and slow crystal growth speed, thereby improving production efficiency and chip quality.

[0063] In the step S30 , the second undoped gallium nitride sublayer 312 is prepared on the surface of the first undoped gallium nitride sublayer 311 away from the buffer layer 20 by adopting a variable temperature and pressure method within a temperature range of 1100° C. to 1140° C. and a pressure range of 100 torr to 250 torr.

[0064] Among them, the variable temperature and pressure is a method in which the temperature gradually increases and the pressure gradually decreases. In the step S20, the pressure range is set to 250torr~450torr and the temperature is 1100℃~1140℃, which can provide a change space for the change of variable temperature and pressure in the temperature range of 1100℃~1140℃ and the pressure range of 100torr~250torr in the step S30 while meeting the ultimate pressure of the cavity. At this time, the temperature range and pressure range in the step S30 and the temperature range and pressure range in the step S20 can meet the change of variable temperature and pressure without pulling the pressure and temperature to the limit value. Therefore, through the step S30 and the step S20, the second undoped gallium nitride sublayer 312 can be prepared by the variable temperature and pressure preparation method. The thickness of the second undoped gallium nitride sublayer 312 can be 0.05um~0.5um, and the thickness can be ensured within this range on the basis of minimizing the cost to reduce the defects to an appropriate range.

[0065] Therefore, the method for preparing the light-emitting diode chip can shorten the growth time and increase the probability of defect merging and annihilation by using the variable temperature and variable pressure growth mode, thereby reducing defects and improving the luminous efficiency of the light-emitting diode chip.

[0066] In the step S40, SiH 4 The silicon nitride layer 313 (SiN layer) is prepared by using a gas at a temperature of 1100°C to 1140°C and a pressure of 100torr to 250torr. The second preset temperature is a fixed value within the temperature range of 1100°C to 1140°C, and the second preset pressure is a fixed value within the pressure range of 100torr to 250torr. A constant temperature and pressure environment is set according to the second preset temperature and the second preset pressure, and the silicon nitride layer 313 (SiN layer) is prepared on the surface of the second undoped gallium nitride sublayer 312 away from the first undoped gallium nitride sublayer 311.

[0067] The thickness of the silicon nitride layer 313 (SiN layer) can be 0.01um to 0.05um, and the thickness can be ensured to play a filling role and reduce defects to an appropriate range on the basis of minimizing costs. At the same time, since the growth environment of the SiN layer will affect the compactness of the SiN network, the silicon nitride layer 313 (SiN layer) can be formed into a uniform network structure under the constant temperature and pressure environment set by the second preset temperature and the second preset pressure.

[0068] In the step S50, the third undoped gallium nitride sublayer 314 is grown in a metal organic chemical vapor deposition (MOCVD) machine, and a TMGA source is introduced in a nitrogen-hydrogen-ammonia mixed atmosphere to react and grow. The third preset temperature is a fixed value in the temperature range of 1100° C. to 1140° C., and the third preset pressure is a fixed value in the pressure range of 100 torr to 250 torr. A constant temperature and pressure environment is set according to the third preset temperature and the third preset pressure, and the third undoped gallium nitride sublayer 314 is prepared on the surface of the silicon nitride layer 313 away from the second undoped gallium nitride sublayer 312.

[0069] The thickness of the third undoped gallium nitride sublayer 314 may be 0.01 um to 0.1 um. On the basis of minimizing the cost, the thickness within this range can be ensured to play a filling role and reduce the defects to an appropriate range.

[0070] In the step S60, the fourth preset temperature is a fixed value in the range of 1130°C to 1170°C, and the fourth preset pressure is a fixed value in the range of 100torr to 250torr. A constant temperature and pressure environment is set according to the fourth preset temperature and the fourth preset pressure, and the heat treatment layer 315 is prepared on the surface of the third undoped gallium nitride sublayer 314 away from the silicon nitride layer 313. The heat treatment layer 315 can be used to process the interface and make the surface flat, thereby covering the defects formed by the unflattened crystal growth of the entire layer.

[0071] Therefore, through the step S20, under high pressure and low temperature conditions, the growth form of the first undoped gallium nitride sublayer 311 is changed to three-dimensional island growth. In the step S30, the pressure is gradually reduced and the temperature is gradually increased, that is, variable temperature and pressure growth, and gradually changes to two-dimensional layered growth, thereby forming a three-dimensional / two-dimensional alternating growth pattern, that is, alternating from three-dimensional island growth to two-dimensional layered growth. At this time, the defects will change direction at the interface of alternating island to layer, so that some defects will merge and annihilate. Among them, the relative constant temperature and pressure through variable temperature and pressure can not only save the time required for chamber stabilization, but also make the interface clearer, and the use of multiple pairs of cycles can increase the probability of defect merging and annihilation.

[0072] Subsequently, in step S40, the SiN layer is grown at constant temperature and pressure to form a mesh structure, which, on the one hand, blocks some defects from extending upward, and on the other hand, some defects will change direction when passing through the mesh holes and then merge and annihilate. In step S50, the third undoped gallium nitride sublayer 314 is grown at constant temperature and pressure in a two-dimensional layered growth form, which plays a role of filling up again. Finally, in step S60, the heat treatment layer 315 is no longer grown, and the temperature is simply increased and the H is increased.2 Flow. Through high temperature and high H 2 The atmosphere is conducive to processing the interface and making the surface flat, thereby covering the defects caused by the entire layer of crystal growth not being flattened.

[0073] In one embodiment, the method for preparing a light emitting diode chip further includes:

[0074] S70, according to the steps S20 to S60, the first undoped gallium nitride sublayer 311, the second undoped gallium nitride sublayer 312, the silicon nitride layer 313, the third undoped gallium nitride sublayer 314 and the heat treatment layer 315 are cyclically prepared in sequence on the surface of the heat treatment layer 315 away from the third undoped gallium nitride sublayer 314.

[0075] Through the steps S20 to S60, the chamber temperature and pressure are set to control the growth conditions, and a structure of 5 to 50 cycles of loop (first undoped gallium nitride sublayer 311 / second undoped gallium nitride sublayer 312 / three-dimensional island structure 3111 / silicon nitride layer 313 / third undoped gallium nitride sublayer 314 / heat-treated layer 315) cyclic growth is prepared. Through the three-dimensional / two-dimensional alternating growth mode and variable temperature and pressure at the interface and multiple cyclic growth, the defects can be turned to merge and annihilate with a high probability. At the same time, the third undoped gallium nitride sublayer 314 (filling layer), the silicon nitride layer 313 and the heat-treated layer 315 also play a role in blocking defects. Therefore, the light-emitting diode preparation method can prepare an LED structure with high crystal quality, thereby improving the luminous efficiency of the light-emitting diode.

[0076] In one embodiment, in the step S30, the second undoped gallium nitride sublayer 312 is prepared on the surface of the first undoped gallium nitride sublayer 311 away from the buffer layer 20 in a variable temperature and pressure environment with a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr, where the temperature gradually increases and the pressure gradually decreases.

[0077] In one embodiment, in step S10, the substrate 10 may be a sapphire substrate, or a Si substrate or a SiC substrate. Also, the buffer layer 20 is grown on the surface of the substrate 10 at about 550°, and the buffer layer 20 is GaN. The thickness of the buffer layer 20 is 25nm to 35nm.

[0078] In the step S20 , under a constant temperature and pressure environment of 1090° C. and 350 torr, the first undoped gallium nitride sublayer 311 (uGaN0 layer) with a thickness of 0.05 μm is prepared on the surface of the buffer layer 20 away from the substrate 10 .

[0079] In the step S30, the temperature is gradually increased from 1090° C. in the step S20 to 1120° C., and the pressure is gradually reduced from 350 torr in the step S20 to 150 torr under a variable temperature and pressure environment, and the second undoped gallium nitride sublayer 312 (uGaN1 layer) with a thickness of 0.05 μm is prepared on the surface of the first undoped gallium nitride sublayer 311 away from the buffer layer 20.

[0080] In step S40, the gas introduced is SiH 4 In a constant temperature and pressure environment with a growth temperature of 1120° C. and a growth pressure of 150 torr, the silicon nitride layer 313 (SiN layer) with a thickness of 0.01 um is prepared on the surface of the second undoped gallium nitride sublayer 312 away from the first undoped gallium nitride sublayer 311 .

[0081] In the step S50, under a constant temperature and pressure environment with a growth temperature of 1120°C and a growth pressure of 150 torr, the third undoped gallium nitride sublayer 314 (uGaN2 layer) with a thickness of 0.02 um is prepared on the surface of the silicon nitride layer 313 away from the second undoped gallium nitride sublayer 312.

[0082] In step S60, H 2 The gas 12L rapidly raises the growth temperature to 1150° C. and the growth pressure is 150 torr in a constant temperature and pressure environment, and a heat treatment layer 315 is prepared on the surface of the third undoped gallium nitride sublayer 314 away from the silicon nitride layer 313 .

[0083] According to the above steps S20 to S60 and the cyclic growth period is set to 10 periods, the undoped gallium nitride layer 30 is grown on the surface of the buffer layer 20. At this time, the undoped gallium nitride layer 30 prepared by the light-emitting diode preparation method includes 10 sub-gallium nitride layers 310 (a first undoped gallium nitride sub-layer 311, a second undoped gallium nitride sub-layer 312, a silicon nitride layer 313, a third undoped gallium nitride sub-layer 314, and a heat treatment layer 315).

[0084] The light emitting diode preparation method further comprises:

[0085] S70, growing a high temperature N-type semiconductor layer 40 (N-GaN layer) at a growth temperature of 1070°C to 1110°C, with a Si doping concentration of 1.00E19-4.00E19 and a thickness of 0.5 μm-2.0 μm.

[0086] S80, preparing the multi-quantum well layer 50 on the surface of the N-type semiconductor layer 40 away from the undoped gallium nitride layer 30. When preparing the multi-quantum well layer 50, the number of cycles is between 8 and 15. The multi-quantum well layer 50 is composed of an InxGa(1-x)N(x=0.20-0.22) quantum well layer and a Si-doped GaN quantum barrier layer. The thickness of a single quantum well layer is between 20nm and 40nm, and the thickness of a single quantum barrier layer is between 100nm and 140nm.

[0087] S90 , preparing a 100 nm to 120 nm Mg-doped high temperature P-type semiconductor layer 60 (P-type GaN layer) on a surface of the multi-quantum well layer 50 away from the N-type semiconductor layer 40 at a growth temperature of 900° C. to 1000° C.

[0088] Through the light-emitting diode preparation method, a large number of defects can be eliminated, the crystal quality is improved, the problems of leakage channel leakage and poor anti-static ability caused by defects are solved, the defects are avoided from extending to the multi-quantum well layer 50 to generate defective non-radiative luminescence, and the luminous efficiency of the light-emitting diode chip is improved.

[0089] In one embodiment, the light-emitting diode preparation method may adopt the metal-organic chemical vapor deposition method (Metal-organic Chemical Vapor Deposition, MOCVD) or MOVPE (Metal-organic Vapor-Phase Epitaxy) and the like.

[0090] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0091] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A light emitting diode chip, characterized in that: include: A substrate (10), wherein a buffer layer (20) is provided on the surface of the substrate (10); an undoped gallium nitride layer (30) disposed on a surface of the buffer layer (20) away from the substrate (10); The undoped gallium nitride layer (30) comprises a plurality of gallium nitride sub-layers (310), and the plurality of gallium nitride sub-layers (310) are sequentially arranged on a surface of the buffer layer (20) away from the substrate (10); Each of the sub-gallium nitride layers (310) comprises a first undoped gallium nitride sub-layer (311) and a second undoped gallium nitride sub-layer (312), wherein the first undoped gallium nitride sub-layer (311) is arranged on a surface of the buffer layer (20) away from the substrate (10), and the second undoped gallium nitride sub-layer (312) is arranged on a surface of the first undoped gallium nitride sub-layer (311) away from the buffer layer (20); The first undoped gallium nitride sublayer (311) comprises a plurality of three-dimensional island structures (3111), the plurality of three-dimensional island structures (3111) being arranged in sequence on a surface of the buffer layer (20) away from the substrate (10), and the second undoped gallium nitride sublayer (312) being arranged on a surface of the plurality of three-dimensional island structures (3111) away from the buffer layer (20); The second undoped gallium nitride sublayer (312) is a two-dimensional layered structure, and is arranged on a surface of the plurality of three-dimensional island structures (3111) away from the buffer layer (20); Each of the gallium nitride sub-layers (310) further comprises: a silicon nitride layer (313), arranged on a surface of the second undoped gallium nitride sublayer (312) away from the first undoped gallium nitride sublayer (311), the silicon nitride layer (313) being a mesh structure; a third undoped gallium nitride sublayer (314), arranged on a surface of the silicon nitride layer (313) away from the second undoped gallium nitride sublayer (312); The heat treatment layer (315) is arranged on a surface of the third undoped gallium nitride sublayer (314) away from the silicon nitride layer (313).

2. The light emitting diode chip according to claim 1, characterized in that: The first undoped gallium nitride sublayer (311) of two adjacent gallium nitride sublayers (310) among the plurality of gallium nitride sublayers (310) is arranged on a surface of the heat treatment layer (315) away from the third undoped gallium nitride sublayer (314).

3. The light emitting diode chip according to claim 1, characterized in that: The undoped gallium nitride layer (30) comprises 5 to 50 sub-gallium nitride layers (310).

4. A method for preparing a light emitting diode chip, characterized in that: The following steps are involved: S10, providing a substrate (10), wherein a buffer layer (20) is prepared on the surface of the substrate (10); S20, preparing a first undoped gallium nitride sublayer (311) on a surface of the buffer layer (20) away from the substrate (10) according to a first preset temperature and a first preset pressure in an environment of a temperature of 1070° C. to 1110° C. and a pressure of 250 torr to 450 torr; S30, preparing a second undoped gallium nitride sublayer (312) on a surface of the first undoped gallium nitride sublayer (311) away from the buffer layer (20) under a variable temperature and pressure environment of 1100° C. to 1140° C. and 100 torr to 250 torr; S40, in an environment of a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr, preparing a silicon nitride layer (313) on a surface of the second undoped gallium nitride sublayer (312) away from the first undoped gallium nitride sublayer (311) according to a second preset temperature and a second preset pressure, wherein the silicon nitride layer (313) is a mesh structure; S50, preparing a third undoped gallium nitride sublayer (314) on a surface of the silicon nitride layer (313) away from the second undoped gallium nitride sublayer (312) according to a third preset temperature and a third preset pressure in an environment of a temperature of 1100° C. to 1140° C. and a pressure of 100 torr to 250 torr; S60, preparing a heat treatment layer (315) on a surface of the third undoped gallium nitride sublayer (314) away from the silicon nitride layer (313) according to a fourth preset temperature and a fourth preset pressure in an environment of a temperature of 1130° C. to 1170° C. and a pressure of 100 torr to 250 torr; S70, according to S20 to S60, cyclically preparing the first undoped gallium nitride sublayer (311), the second undoped gallium nitride sublayer (312), the silicon nitride layer (313), the third undoped gallium nitride sublayer (314), and the heat treatment layer (315) in sequence on a surface of the heat treatment layer (315) away from the third undoped gallium nitride sublayer (314).

5. The method for preparing a light emitting diode chip according to claim 4, characterized in that: In S30, in an environment of temperature 1100° C. to 1140° C. and pressure 100 torr to 250 torr, in a variable temperature and pressure environment in which the temperature gradually increases and the pressure gradually decreases, the second undoped gallium nitride sublayer (312) is prepared on a surface of the first undoped gallium nitride sublayer (311) away from the buffer layer (20).