Radiation-oriented sintered NdFeB magnetic tile and preparation method and molding device
Through the two-powder filling and molding process and a special molding device, the problems of uneven magnetic properties and molding fracture of the NdFeB radiated tile magnets are solved, and a consistent magnet production with high orientation and high magnetic properties is achieved.
Patent Information
- Application Number
- CN201911286542.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2039-12-13
AI Technical Summary
The existing neodymium iron boron radiated tile magnets have problems such as uneven magnetic properties, lower residual magnetism at the edges and corners than in the middle, complex and expensive forming equipment, low flexibility, and poor powder flow, resulting in easy breakage of the green body.
Using the process of two powder filling and two molding, the weight of the first powder filling is 0.2M≤W1≤0.5M, the magnetic field of the first magnetic filling is 0.1 Tesla≤T1≤0.3 Tesla, and the pre-pressure density At 0.8P≤P1≤0.9P, the weight of the powder is M-W1 for the second time, the magnetic field for the second time is 0.3 Tesla
The magnetic performance consistency of the neodymium iron boron tiles is improved, and the unevenness of the upper and lower orientation of the green body and the problem of release and breakage are reduced, ensuring the high orientation and high pass rate of the magnet.
Smart Images

Figure CN110783051B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the manufacturing field of sintered NdFeB, in particular to a radiation-oriented sintered NdFeB magnetic tile and a preparation method and a molding device. Background Art
[0002] Permanent magnet servo motors are widely used around the world due to their high efficiency, low power consumption and high precision. The permanent magnet inside is an important core component that determines the performance of permanent magnet servo motors. At present, the magnets of permanent magnet servo motors are mostly single-piece tiles or square pieces parallel to the radial direction, which are bonded to the rotor to form the main body of the motor. However, this assembly method is prone to cause disadvantages such as large motor vibration and noise.
[0003] In order to overcome the shortcomings of single-piece tiles and square magnetic steel, some servo motors are assembled by radiating magnetic rings. Most of the current NdFeB magnetic rings are manufactured by isotropic bonded magnets or hot-pressed magnetic rings. However, the former has adhesive inside that reduces the magnetic energy product, and the latter has low magnetic performance consistency, pass rate and material utilization.
[0004] Some manufacturers have also developed a manufacturing process for sintered NdFeB radiation tiles or radiation magnetic rings. Although it can improve the magnetic properties compared to hot-pressed NdFeB magnetic rings, this process also has the problem of low magnetic properties. Secondly, the molding equipment is complex and expensive. What's worse, the magnet is prone to cracking during the sintering process.
[0005] In addition, in the existing manufacturing method of NdFeB radiation tiles, it is necessary to design special magnet forming and orientation equipment for products with different performance requirements of different sizes, which has low flexibility, long design cycle, single product brand, and is not conducive to the rapid switching and production of new products. For example, patent number CN 107579628A discloses a method for manufacturing radial radiation oriented rare earth permanent ferrite arch magnets. Although this method can improve the magnetic performance utilization rate of magnetic steel, its forming equipment is extremely complex and is not conducive to actual production.
[0006] Secondly, the existing disclosed method for preparing NdFeB magnets for radiation tiles still has the problem of uneven magnetic properties, and the residual magnetism of the corners is lower than that of the middle. For example, patent number CN 203209691 discloses a mold for NdFeB radiation-oriented magnets, which is characterized in that magnetic conductive side plates are respectively arranged in the mold cavity to form a radial orientation magnetic field. The main disadvantage of this method is that the magnetic field orientation will deteriorate at the position where the mold cavity has a larger angle, resulting in reduced performance of the angled part of the magnetic steel.
[0007] Again, the existing sintered NdFeB radiation oriented magnetic rings or tiles have poor powder fluidity during the molding and orientation process, and there is a compression density deviation in the upper and lower height directions of the green body, which is easy to break during the demolding process. In order to solve the above problems, Patent Publication No. CN 1173028 discloses a preforming device for green bodies, which heats the mold and performs molding by adding thermosetting resin to the powder. The biggest problem with this method is that NdFeB powder is easily oxidized by heat, and the residual resin seriously reduces the magnetic properties. Patent No. CN 110415964 discloses a method for preparing NdFeB multi-pole magnetic rings, mixing surface-modified anisotropic powder with paraffin, pre-pressing the magnetic powder, and forming a preformed body. Although this method solves the problem of orientation stability, the addition of paraffin will inevitably cause the performance of the magnet to deteriorate. Patent Announcement No. CN 103971917 adopts a method of applying preforming pressure to first obtain a preformed magnetic ring. The patent claims that this method can improve the density consistency of the magnetic ring and improve the yield rate. However, the patent does not limit the weight of powder fed during preforming, or in other words, does not divide the powder into multiple feedings. The reason for paying attention to the weight of powder fed during preforming is that when producing magnets with relatively large green compact pressing heights, the consistency of the orientation or density of the green compact in the vertical direction can only be improved to a limited extent. Therefore, the technical solution of the patent is not perfect for improving the orientation consistency of the radiation tile or magnetic ring. Summary of the invention
[0008] The technical problem to be solved by the present invention is to design a sintered NdFeB radiation tile magnet with uniform radiation orientation, good overall magnetic property consistency, high NdFeB main phase orientation, high magnet qualification rate and not prone to sintering cracking, as well as a preparation method and molding device.
[0009] The remanence of NdFeB mainly comes from the main phase, that is, the 2:14:1 phase (Nd2Fe 14 2). When the magnet composition is determined, the main factors affecting the remanence of sintered NdFeB magnets include the orientation degree of the main phase, the proportion of the main phase in the magnet and the sintering density of the magnet. The latter two parameters are greatly affected by the sintering and aging processes. The first parameter is greatly affected by the molding orientation process. When the particle size of the powder and the amount of lubricant added are consistent, the larger the molding orientation magnetic field, the higher the orientation degree of the powder, the higher the orientation degree of the main phase of the final magnet, and the higher the remanence of the magnet.
[0010] However, for radiation-oriented NdFeB tiles, during the process of orienting and pressing the powder in the forming magnetic field to form a green body, the applied external magnetic field either cannot reach the magnetic field range consistent with the conventional parallel magnetic field, or the orientation field is uneven, or the angle θ between the orientation angle and the actual value deviates, and the larger the angle θ, the lower the residual magnetism of the magnet will be. When testing the magnetic surface field distribution of the magnet, the surface field distribution curve will fluctuate. In addition to the impact on magnetic properties, in actual production, the green body will break after demolding due to uneven molding pressure and orientation.
[0011] One of the technical solutions of the present invention is to solve the problem of uneven upper and lower orientation and forming fracture of the above-mentioned magnet, and specifically provides a process of placing sintered NdFeB powder into a radially oriented DC magnetic field press cavity for secondary powder loading and secondary forming:
[0012] The first powder loading, the first magnetization and pre-pressing: The weight w1 of the first powder loading satisfies the relationship: 0.2M≤W1≤0.5M, where M is the weight of the final blank. The magnetic field T1 of the first magnetization satisfies the relationship: 0.1 Tesla≤T1≤0.3 Tesla; the density P1 of the green body after pre-pressing satisfies the relationship: 0.8P≤P1≤0.9P, where P is the relative density of the green body before sintering, and P satisfies the relationship 3.8≤P≤4.5.
[0013] The second powder loading, the second magnetization and the final molding: the weight of the second powder loading is w2=M-W1, the magnetic field of the final molding is 0.3 Tesla<T2≤2.5 Tesla, and the density of the green body after the final molding is p2=P.
[0014] By adopting this molding method, the orientation degree of each position of the green body is consistent, and the molding qualification rate after demoulding is high.
[0015] More specifically, before the second powder filling and the second molding, the NdFeB thin sheet alloy is firstly prepared according to the rapid solidification thin strip process, and the NdFeB thin sheet alloy is subjected to hydrogen treatment and air flow milling process to obtain sintered NdFeB powder.
[0016] The second technical solution of the present invention is to solve the problem that the orientation fields at both ends and the center of the radiating magnet tile are inconsistent, and the actual direction of the magnetic field deviates from the designed direction. There is an angular deviation between the actual orientation direction of the magnet and the designed direction.
[0017] Specifically, a forming device for a radially oriented sintered NdFeB magnetic ring is provided, comprising a non-magnetic mold body, a mold cavity, a magnetic conductive component, and a magnetic conductive plate; a mold cavity is arranged in the mold body, the mold cavity is tile-shaped, both sides are curved arc surfaces, the inner arc surface is an arc surface concave inwardly, and the outer arc surface is an arc surface protruding outwardly, the magnetic conductive component is two magnetic conductive blocks located on both sides of the mold cavity, the first magnetic conductive block is located on one side of the inner arc surface of the tile shape, and the second magnetic conductive block is located on one side of the outer arc surface of the tile shape, wherein the center points of the first magnetic conductive block, the tile-shaped mold cavity, and the second magnetic conductive block are located on the same straight line; two symmetrically distributed uniform magnetic conductive plates are arranged between the outer arc surface of the tile-shaped mold cavity and the second magnetic conductive block.
[0018] More specifically, the surface of the first magnetic conductive block facing the inner arc surface is in an arc shape, and the radius of the arc shape is smaller than the radius of the inner arc surface of the tile-shaped mold cavity.
[0019] More specifically, the surface of the second magnetic conductive block facing the outward arc surface is bent, and the bending angle of the bend is 90 degrees. The tile-shaped mold cavity is located within the space radiated by the bent surface of the second magnetic conductive block.
[0020] More specifically, the two magnetic conductive plates are respectively located at two ends of the outer arc surface of the tile-shaped mold cavity, and the center point of each magnetic conductive plate is located on the extension line of the radius of the tile-shaped mold cavity.
[0021] More specifically, the thickness W of the magnetic conductive plate satisfies: 0.5 cavity thickness ≤ W ≤ 1.0 cavity thickness, and its length L satisfies: 0.2 inner arc length ≤ L ≤ 0.4 inner arc length, where the inner arc length is the length of the inner arc surface of the tile-shaped cavity, the surface where the straight edge of the tile-shaped cavity is located is in the same plane as the outer side surface of the magnetic conductive plate, and the cavity thickness is 5mm-25mm.
[0022] More specifically, the molding device further comprises upper and lower pressure heads, wherein the upper pressure head is located directly above the tile-shaped mold cavity, and the lower pressure head is located directly below the tile-shaped mold cavity.
[0023] In the technical solution of the present application, the sintered Nd2Fe 14 The orientation degree of the B main phase is above 92%, the deviation between the orientation angle of the radiation orientation and the target value △θ≤1 degree, and the overall residual magnetism deviation △Br of the sintered NdFeB tile magnet is ≤2%.
[0024] Compared with the prior art, the present invention is beneficial in that:
[0025] By adopting the manufacturing process of the present application, performing two powder feedings and two moldings, and controlling the weight of each powder feeding and the size of the orientation field within a reasonable range, the problems of uneven upper and lower orientations and cracking of green pieces can be solved. The molding device of the present application, by using the added uniform magnetic conductive plate and reasonably designing its size and angle, can make the magnetic field lines of the tile-shaped sheet mold cavity consistent with the design value under the condition of increasing the external orientation field, thereby improving the remanence and magnetic property consistency of the NdFeB magnetic tile. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the molding device of the present invention.
[0027] Marking instructions: 1. First magnetic conductive block, 2. Mold body, 3. Mold cavity, 4. Magnetic conductive plate, 5. Direction of magnetic lines of force, 6. Inner arc surface, 7. Second magnetic conductive block, 8. Outer arc surface.
[0028] Specific implementation method:
[0029] The present invention is further described below in conjunction with specific implementation modes, and the embodiments are only used to explain the present invention and do not have any limiting effect thereon.
[0030] The production requirements for the NdFeB magnetic tiles of this application are as follows: Radiation oriented magnet Nd2Fe 14 The orientation degree of the B main phase is above 92%, the deviation between the orientation angle in the radiation direction and the target value △θ≤1 degree, and the remanence deviation △Br of the overall magnet is ≤2%.
[0031] The NdFeB thin sheet alloy is prepared in advance according to the rapid solidification thin strip process, and the NdFeB thin sheet alloy is subjected to hydrogen treatment and air flow grinding to obtain sintered NdFeB powder.
[0032] The magnet powder can be prepared by a method for preparing sintered NdFeB powder that is well known or recognized, or it can be a commercially available general-purpose sintered NdFeB powder. a T (1-a-b-3) B b M C , where a, b, and c represent the mass percentage of each element in the composition ratio, Re is a rare earth element, at least one of Pr, Nd, Dy, Tb, Ho, and Gd, T is at least one of Fe or Co, B is a B element, and M is at least one of Al, Cu, Ga, Ti, Zr, Nb, Mo, and V, with a specific content of 28%≤a≤32%, 0.8%≤b≤1.2%, and c≤5%. The above alloy ratio is subjected to rapid solidification ribbon smelting, hydrogen treatment, air flow milling, and other processes to obtain NdFeB powder.
[0033] The sintered NdFeB powder is placed into a radiation-oriented mold cavity for two powder filling, magnetization and molding processes:
[0034] The first powder loading, magnetization and pre-pressing: according to the required weight W1, the sintered NdFeB powder is weighed and placed into the mold cavity of the DC magnetic field press, and the magnetic field and molding pressure are adjusted to form the first green compact;
[0035] Second powder loading, magnetization and final molding: Weigh the sintered NdFeB powder according to the required weight W2 and put it into the mold cavity of the DC magnetic field press, adjust the magnetic field and molding pressure to form the second green body.
[0036] The green compact after the two-time molding and orientation is sintered and aged to obtain the required radiation-oriented NdFeB tile.
[0037] The radiation-oriented mold cavity in the present application can be achieved by using a DC magnetic field press or a pulsed magnetic field.
[0038] Through experiments, it was found that since most tile-type products are small in size, the corresponding mold cavity is also smaller than that of conventional square magnets. This leads to poor fluidity of the powder with the pressure head during the molding of tile-type magnets. If the orientation and molding process similar to that of square magnets is adopted, it is easy to have uneven orientation of the green body up and down, and the green body will break after demolding. The reasonable range here means that the weight w1 of the first powder loading must satisfy the relationship: 0.2M≤w1≤0.5M, where M is the weight of the final finished blank. Because when the weight of the first powder feeding is greater than 0.5M, the green body begins to have uneven orientation up and down, and when the weight of the first powder feeding is less than 0.2M, the effect of improving the uneven orientation up and down is not obvious. During the first pre-pressing, if the designed pressing density is too high, a density difference will be formed between the two moldings and the green body will break. However, if the pressing density is too low, the pre-pressing effect will not be achieved. Therefore, the density of the green body during pre-pressing is designed to be 0.8P≤p1≤0.9P, where P is the relative density of the final green body.
[0039] As attached Figure 1As shown, the forming device of the radiant NdFeB tile includes a non-magnetic mold body 2 and a tile-shaped mold cavity 3, wherein the two curved arc surfaces of the mold cavity 3 are respectively an inner arc surface and an outer arc surface with the same center, the arc surface of the inner arc surface is concave inward, and the arc surface of the outer arc surface is protruding outward, and the forming device also includes upper and lower pressure heads, and magnetic blocks on both sides of the mold cavity, a first magnetic block 1 and a second magnetic block 7, wherein the end of the first magnetic block 1 facing the inner arc surface is arc-shaped, and the side of the second magnetic block 7 facing the outer arc surface is bent, which is 90 degrees in this embodiment, and the two sides of the bend are symmetrical, and the center of the arc-shaped end of the first magnetic block 1 is on the same line as the bending center of the second magnetic block 7 and the center of the tile-shaped mold cavity, and the radius of the arc-shaped end of the first magnetic block 1 is smaller than the radius of the arc surface inside the tile-shaped mold cavity.
[0040] Two symmetrically distributed uniform magnetic conductive plates are arranged between the outer arc surface of the tile-shaped mold cavity of the molding device and the second magnetic conductive block 7. Each magnetic conductive plate is close to the attached Figure 1 As shown,
[0041] The side surface connecting the inner arc surface and the outer arc surface is S2, and the side close to the side wall of the mold body is S1. The side surface S1 is in the same plane as the outer side surface S2 of the tile-shaped mold cavity. The center points of the two magnetic conductive plates are located on the extension line of the radius of the tile-shaped mold cavity, and each magnetic conductive plate is located at both ends of the outer arc of the tile-shaped mold cavity.
[0042] The thickness W of the uniform magnetic conductive plate satisfies: 0.5 cavity thickness ≤ W ≤ 1.0 cavity thickness, and its length L satisfies: 0.2 inner arc length ≤ L ≤ 0.4 inner arc length, where the inner arc length is the length of the inner arc surface of the tile-shaped cavity, and the cavity thickness is 5mm-25mm.
[0043] The purpose of setting two symmetrical uniform magnetic conductive plates is to attract the magnetic lines of force on both sides of the tile so that their direction is consistent with the magnetic field design, making the angle θ ≤ 1 degree.
[0044] Although magnetic conductive components are provided at both ends of the cavity of the radial tile mold, so that the magnetic lines of force form an ideal radial shape and pass through the cavity. However, as the strength of the external magnetic field increases, the magnetic lines of force begin to tend to a straight direction, flowing from the N pole of the press to the S pole. On the left and right sides (edge parts) of the tile cavity, the normals of the magnetic lines of force and the arc are no longer 90 degrees. This leads to a contradictory problem, that is, if the orientation field is increased, the orientation angle of the edge part of the tile cavity will deviate, the residual magnetism of the magnet will decrease, and the performance consistency of the magnet will deteriorate. In order to improve the orientation angle and consistency, the orientation magnetic field must be reduced, which will also lead to a decrease in the residual magnetism of the magnet and a deterioration in performance consistency.
[0045] By adopting the molding device of the present invention, utilizing the added uniform magnetic conductive plate and rationally designing its size and angle, it is possible to make the direction of the magnetic lines of force of the tile-shaped mold cavity consistent with the design value under the condition of increasing the external orientation field, thereby improving the residual magnetism and magnetic property consistency of the magnet.
[0046] The reasonable design of the size and angle here means that if the L of the uniform magnetic conductive plate is too small, it will not correct the magnetic lines of force, and the residual magnetism at the edge of the tile will still be lower than that at the center. If L is too large, the magnetic lines of force at the center of the tile will be affected by the uniform magnetic conductive plate, resulting in too low residual magnetism in the middle of the tile. In addition, the effect of too large or too small W of the uniform magnetic conductive plate is similar to L. If W is too large, the magnetic lines of force will tilt toward the edge of the tile, and the residual magnetism at the edge of the tile will be too high. If W is too small, it will not improve the magnetic lines of force. Therefore, the ranges of L and W are set to W satisfying: 0.5 cavity thickness ≤ W ≤ 1.0 cavity thickness, L satisfying: 0.2 inner arc length ≤ L ≤ 0.4 inner arc length, and its side surface S1 is in the same plane as the outer side surface S2 of the tile-shaped cavity.
[0047] In accordance with the manufacturing process and manufacturing device of the present application, sintered NdFeB tiles are manufactured through Examples 1-3, and the molded sintered NdFeB tiles are measured. At the same time, control groups 1-3 that are different from the manufacturing process of the present application are provided for performance comparison. For the sake of convenience, in the following embodiments and comparative examples of the present application, the total amount of powder is 50g, the thickness of the mold cavity is 11mm, the inner arc length is 40mm, and different magnetic fields are used for the magnetic powder in the mold cavity. The density of the magnet generated for the first time is required to be 3.4, and the density of the magnet generated for the second time is 4.2. The density values of P1 and P2 are not affected by the mold cavity thickness and the magnetic field, but are determined by the molding pressure brought by the molding device. The performance of the magnet is compared under the same density conditions.
[0048] Embodiment 1:
[0049] 1) Prepare the composition (PrNd) 32 Co 1.0 Al 0.1 Cu 0.1 Ti 0.1 B 1.0 Fe bal of powder;
[0050] 2) Weigh w1=20g of powder;
[0051] 3) Place the weighed powder into a tile-shaped mold cavity, wherein the thickness of the mold cavity is 11 mm, the inner arc length is 40 mm, the length L of the uniform magnetic conductive plate is 10 mm, and W is 8 mm;
[0052] 4) The upper and lower pressure heads of the molding device squeeze the mold cavity, and the magnetic field size is set to 0.1 Tesla;
[0053] 5) adjusting the molding pressure provided to the molding device so that the relative density of the green body is 3.4;
[0054] 6) Remove the external magnetic field and keep the pressure head away from the mold cavity;
[0055] 7) Weigh W2 = 30 g of powder for the second time and place it into the tile-shaped mold cavity again;
[0056] 8) The upper and lower pressure heads squeeze the mold cavity and set the magnetic field size to 1.0 Tesla;
[0057] 9) Adjust the molding pressure so that the relative density of the green body is 4.2;
[0058] 10) Demolding, isostatically pressing the green body and placing it in a sintering furnace for sintering, and then in an aging furnace for aging;
[0059] 11) A DC magnetic property measuring instrument and an EBSD (electron backscatter diffractometer) were used to measure the magnetic properties, orientation degree and angle difference θ at the center and edge of the tile blank after aging.
[0060] The selected parameters are calculated based on 50g magnetic powder, 0.2M≤w1≤0.5M, the range of W1 is 10-25g, w2=M-w1; 0.1 Tesla≤T1≤0.3 Tesla; according to the value of P 3.8≤P≤4.5, 0.8P≤P1≤0.9P, P2=P, to calculate the value range of P1 and P2; 0.3 Tesla<T2≤2.5 Tesla; the cavity thickness is 5mm-25mm, and the thickness W of the magnetic conductive plate is calculated according to the cavity thickness to be between 2.5-25mm, 0.5 cavity thickness≤W≤1.0 cavity thickness; 0.2 inner arc length≤L≤0.4 inner arc length, the inner arc length is less than the width of the mold body and is used in conjunction with the cavity thickness.
[0061] In Example 1, W1 is 20g, the mold cavity thickness is 11mm, the inner arc length is 40mm, the length L of the magnetic conductive plate is 10mm, the thickness W of the magnetic conductive plate is 8mm, the first magnetic field T1 is 0.1 Tesla, P1 is 3.4, W2 is 30g, the second magnetic field T2 is 1.0 Tesla, and the P2 density is 4.2.
[0062] Embodiment 2:
[0063] The weight of the powder selected for the first time and the powder selected for the second time are different from those in Example 1, but the total weight is still 50 g, and the magnetic field for the first time and the magnetic field for the second time are also different from those in Example 1.
[0064] 1) Prepare the composition (PrNd) 32 Co 1.0 Al 0.1 Cu0.1 Ti 0.1 B 1.0 Fe bal of powder;
[0065] 2) Weigh w1=25g of powder;
[0066] 3) Place the weighed powder into a tile-shaped mold cavity, wherein the thickness of the mold cavity is 11 mm, the inner arc length is 40 mm, the length L of the uniform magnetic conductive plate is 10 mm, and W is 8 mm;
[0067] 4) The upper and lower pressure heads of the molding device squeeze the mold cavity, and the magnetic field size is set to 0.2 Tesla;
[0068] 5) adjusting the molding pressure provided to the molding device so that the relative density of the green body is 3.4;
[0069] 6) Remove the external magnetic field and keep the pressure head away from the mold cavity;
[0070] 7) Weigh W2 = 25 g of powder for the second time and place it into the tile-shaped mold cavity again;
[0071] 8) The upper and lower pressure heads squeeze the mold cavity and set the magnetic field size to 1.5 Tesla;
[0072] 9) Adjust the molding pressure so that the relative density of the green body is 4.2;
[0073] 10) Demolding, placing the green body in a sintering furnace for sintering, and then in an aging furnace for aging;
[0074] 11) A DC magnetic property meter and an EBSD (electron backscatter diffractometer) were used to measure the △Br, orientation degree and angle difference θ at the center and edge of the tile blank after aging.
[0075] The parameter selection range is similar to that of Example 1, but in terms of specific values, W1 is 25g, the mold cavity thickness is 11mm, the inner arc length is 40mm, the length L of the magnetic conductive plate is 10mm, the thickness W of the magnetic conductive plate is 8mm, the first magnetic field T1 is 0.2 Tesla, P1 is 3.4, W2 is 25g, the second magnetic field T2 is 1.5 Tesla, and the P2 density is 4.2.
[0076] Embodiment 3:
[0077] Compared with Example 2, the thickness of the mold cavity in this embodiment has changed and become smaller, from 10 mm to 8 mm.
[0078] 1) Prepare the composition (PrNd) 32 Co 1.0 Al 0.1 Cu 0.1 Ti0.1 B 1.0 Fe bal of powder;
[0079] 2) Weigh W1=25g of powder;
[0080] 3) Place the weighed powder into a tile-shaped mold cavity, where the thickness of the mold cavity is 8 mm, the inner arc length is 40 mm, the length L of the uniform magnetic conductive plate is 10 mm, and W is 8 mm;
[0081] 4) The upper and lower pressure heads of the molding device squeeze the mold cavity, and the magnetic field size is set to 0.2 Tesla;
[0082] 5) adjusting the molding pressure provided to the molding device so that the relative density of the green body is 3.4;
[0083] 6) Remove the external magnetic field and keep the pressure head away from the mold cavity;
[0084] 7) Weigh w2 = 25 g of powder for the second time and place it into the tile-shaped mold cavity again;
[0085] 8) The upper and lower pressure heads of the molding device squeeze the mold cavity, and the magnetic field size is set to 1.5 Tesla;
[0086] 9) Adjust the molding pressure so that the relative density of the green body is 4.2;
[0087] 10) Demolding, isostatically pressing the green body, placing it in a sintering furnace for sintering, and then in an aging furnace for aging;
[0088] 11) A DC magnetic property meter and an EBSD (electron backscatter diffractometer) were used to measure the △Br, orientation degree and angle difference θ at the center and edge of the tile blank after aging.
[0089] The parameter selection range is similar to that of Example 1, but in terms of specific values, W1 is 25g, the mold cavity thickness is 8mm, the inner arc length is 40mm, the length L of the magnetic conductive plate is 10mm, the thickness W of the magnetic conductive plate is 8mm, the first magnetic field T1 is 0.2 Tesla, P1 is 3.4, W2 is 25g, the second magnetic field T2 is 1.0, and the P2 density is 4.2.
[0090] Comparative Example 1:
[0091] In Comparative Example 1, powder loading, magnetization and molding processes are performed only once, and 50 g of powder is taken at a time. The mold cavity is placed in the same environment as in Example 1. The thickness of the mold cavity is 8 mm, the inner arc length is 40 mm, the length L of the uniform magnetic conductive plate is 10 mm, and W is 8 mm. The magnetic field is provided only once and 1.5 Tesla is selected, which is larger than the T1 value of Example 1, but within the value range of T2, and the generated density is 4.2.
[0092] 1) Prepare the composition (PrNd) 32 Co 1.0 Al 0.1 Cu 0.1 Ti 0.1 B 1.0 Fe bal of powder;
[0093] 2) Weigh W1=50g of powder;
[0094] 3) Place the weighed powder into a tile-shaped mold cavity, where the thickness of the mold cavity is 8 mm, the inner arc length is 40 mm, the length L of the uniform magnetic conductive plate is 10 mm, and W is 8 mm;
[0095] 4) The upper and lower pressure heads of the molding device fit the mold cavity, and the magnetic field size is set to 1.5 Tesla;
[0096] 5) adjusting the molding pressure provided to the molding device so that the relative density of the green body is 4.2;
[0097] 6) Remove the external magnetic field and keep the pressure head away from the mold cavity;
[0098] 7) Demolding, isostatically pressing the green body, placing it in a sintering furnace for sintering, and then in an aging furnace for aging;
[0099] 8) A DC magnetic property meter and an EBSD (electron backscatter diffractometer) were used to measure the △Br, orientation degree and angle difference θ at the center and edge of the tile blank after aging.
[0100] Comparative Example 2:
[0101] Comparative Example 2 was subjected to powder loading, magnetizing and molding processes twice, with the same weight as Example 1 and placed in the same environment as Example 1. The thickness of the mold cavity was 8 mm, the inner arc length was 40 mm, W was 8 mm, but the length L of the magnetic conductive plate was changed from 10 mm to 30 mm. The first magnetic field was 1.5 Tesla, generating a density of 3.1, which was larger than the T1 value of Example 1. The second magnetic field was 1.5 Tesla, within the value range of T2, generating a density of 4.2.
[0102] 1) Prepare the composition (PrNd) 32 Co 1.0 Al 0.1 Cu 0.1 Ti 0.1 B 1.0 Fe bal of powder;
[0103] 2) Weigh W1=20g of powder;
[0104] 3) Place the weighed powder into a tile-shaped mold cavity, wherein the thickness of the mold cavity is 11 mm, the inner arc length is 40 mm, the length L of the uniform magnetic conductive plate is 30 mm, and W is 8 mm;
[0105] 4) Close the pressure head and set the magnetic field to 1.5 Tesla;
[0106] 5) Adjust the molding pressure so that the relative density of the green body is 3.4;
[0107] 6) Remove the external magnetic field and raise the pressure head;
[0108] 7) Weigh W2 = 30 g of powder for the second time and place it into the tile-shaped mold cavity again;
[0109] 8) Close the pressure head and set the magnetic field to 1.5 Tesla;
[0110] 9) Adjust the molding pressure so that the relative density of the green body is 4.2;
[0111] 10) Demolding, placing the green body in a sintering furnace for sintering, and then in an aging furnace for aging;
[0112] 11) A DC magnetic property meter and an EBSD (electron backscatter diffractometer) were used to measure the △Br, orientation degree and angle difference θ at the center and edge of the tile blank after aging.
[0113] Comparative Example 3:
[0114] Comparative Example 3 carried out two powder filling, magnetizing and molding processes, taking a total of 50 g of powder and placing it in the same environment as Example 1. The thickness of the mold cavity was 8 mm, the inner arc length was 40 mm, but there was no uniform magnetic conductive plate. The magnetic field was 0.1 Tesla, the same as T1 in Example 1, and the second magnetic field was 1.0 Tesla, the same as T2 in Example 1, and the generated density was 4.2.
[0115] 1) Prepare the composition (PrNd) 32 Co 1.0 Al 0.1 Cu 0.1 Ti 0.1 B 1.0 Fe bal of powder;
[0116] 2) Weigh w1=20g of powder;
[0117] 3) The weighed powder is placed in a tile-shaped mold cavity, wherein the thickness of the mold cavity is 11 mm, the inner arc length is 40 mm, and no uniform magnetic conductive plates are set on both sides of the mold cavity;
[0118] 4) Close the pressure head and set the magnetic field to 0.1 Tesla;
[0119] 5) Adjust the molding pressure so that the relative density of the green body is 3.4;
[0120] 6) Remove the external magnetic field and raise the pressure head;
[0121] 7) Weigh w2 = 30 g of powder for the second time and place it into the tile-shaped mold cavity again;
[0122] 8) Close the pressure head and set the magnetic field to 1.0 Tesla;
[0123] 9) Adjust the molding pressure so that the relative density of the green body is 4.2;
[0124] 10) Demolding, placing the green body in a sintering furnace for sintering, and then in an aging furnace for aging;
[0125] 11) A DC magnetic property meter and an EBSD (electron backscatter diffractometer) were used to measure the △Br, orientation degree and angle difference θ at the center and edge of the tile blank after aging.
[0126] The results of magnetic properties, orientation degree and angle difference θ of the magnets with the same density obtained in Examples 1, 2, 3 and Comparative Examples 1, 2, 3 are statistically shown in Table 1.
[0127] Sample Type △Br Orientation edge Orientation degree medium Angle difference θ edge Angle difference θ middle Example 1 1.0% 92.5%. 92.9% 0.2 degrees 0.1 degrees Example 2 1.1% 92.8% 93.7% 0.5 degrees 0.1 degrees Example 3 0.9% 94.5% 95.1% 0.5 degrees 0.2 degrees Comparative Example 1 3.1% 88.1% 90.0% 3.0 degrees 0.2 degrees Comparative Example 2 4.0% 80.0% 91.5% 4.0 degrees 1.0 degrees Comparative Example 3 5.5% 68.2% 87.1% 15.2 degrees 1.0 degrees
[0128] From the comparison of the effects of the embodiments and the comparative examples, it can be seen that the radiation tile magnet produced using the process method and device of the present invention can improve the overall consistency of magnetic properties, reduce the deviation of the orientation angle at each position, and the orientation degree of the magnet can also be greatly improved. The distribution of the overall magnetic lines of force of the magnet is consistent with the expected model design.
[0129] The above embodiments are only preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. It should be noted that, for those skilled in the art, without departing from the concept of the present invention, several substitutions and improvements can be made, which all belong to the scope of protection of the present invention.
Claims
1. Radiation-oriented sintered NdFeB tiles, characterized by: The sintered Nd2Fe magnet tile 14 The orientation degree of the B main phase is above 92%, the orientation angle of the radiation orientation and the target value deviation △θ≤1 degree, and the overall remanence deviation △Br of the sintered NdFeB tile magnet is ≤2%; The sintered NdFeB tile is manufactured using the following manufacturing steps: Step 1, preparing NdFeB thin sheet alloy according to the rapid solidification thin strip process, and preparing sintered NdFeB powder by subjecting the NdFeB thin sheet alloy to hydrogen treatment and air flow milling; Step 2: Place the sintered NdFeB powder into a radiation-oriented mold cavity and perform two powder filling, magnetization and molding processes: Step 21, first powder loading, magnetization and pre-pressing: weigh the sintered NdFeB powder according to the required weight W1 and put it into the mold cavity of the DC magnetic field press, adjust the magnetic field and molding pressure to form the first green compact; In step 21, the weight W1 of the first powder charge satisfies the relationship: 0.2M≤W1≤0.5M, where M is the weight of the final blank; the magnetic field T1 of the first magnetization satisfies the relationship: 0.1 Tesla≤T1≤0.3 Tesla; the density P1 of the green body after pre-pressing satisfies the relationship; 0.8P≤P1≤0.9P, where P is the relative density of the green body before sintering, and P satisfies the relationship 3.8≤P≤4.5; Step 22, second powder loading, magnetization and final molding: weigh the sintered NdFeB powder according to the required weight W2 and put it into the mold cavity of the DC magnetic field press, adjust the magnetic field and molding pressure to form the second green compact; In step 22, the weight of the second powder charge is W2=M-W1, the final molding magnetic field is 0.3 Tesla<T2≤2.5 Tesla, and the density of the green body after final molding is P2=P; Step 3: Sinter and age the green compact after two molding and orientation to obtain the required radiation-oriented NdFeB tiles.
2. A forming device for sintered NdFeB magnetic tiles with radiation orientation, characterized in that: The sintered Nd2Fe magnet tile 14 The orientation degree of the B main phase is above 92%, the orientation angle of the radiation orientation and the target value deviation △θ≤1 degree, and the overall remanence deviation △Br of the sintered NdFeB tile magnet is ≤2%; The forming device for making sintered NdFeB magnetic tiles comprises a non-magnetic mold body, a mold cavity, a magnetic conductive component, and a magnetic conductive plate; a mold cavity is arranged in the mold body, the mold cavity is tile-shaped, both sides of the mold cavity are curved arc surfaces, the inner arc surface is an arc surface concave inwardly, and the outer arc surface is an arc surface protruding outwardly, the magnetic conductive component is two magnetic conductive blocks located on both sides of the mold cavity, the first magnetic conductive block is located on one side of the inner arc surface of the tile shape, and the second magnetic conductive block is located on one side of the outer arc surface of the tile shape, wherein the center points of the first magnetic conductive block, the tile-shaped mold cavity, and the second magnetic conductive block are located on the same straight line; two symmetrically distributed uniform magnetic conductive plates are arranged between the outer arc surface of the tile-shaped mold cavity and the second magnetic conductive block; The surface of the first magnetic conductive block facing the inner arc surface is in an arc shape, and the radius of the arc shape is smaller than the radius of the inner arc surface of the tile-shaped mold cavity; The surface of the second magnetic conductive block facing the outer arc surface is bent, and the bending angle of the bending shape is 90 degrees, and the tile-shaped mold cavity is located in the space radiated by the bent surface of the second magnetic conductive block; The two magnetic conductive plates are respectively located at two ends of the outer arc surface of the tile-shaped mold cavity, and the center point of each magnetic conductive plate is located on the extension line of the radius of the tile-shaped mold cavity; The thickness W of the magnetic conductive plate satisfies: 0.5 cavity thickness ≤ W ≤ 1.0 cavity thickness, and its length L satisfies: 0.2 inner arc length ≤ L ≤ 0.4 inner arc length, where the inner arc length is the length of the inner arc surface of the tile-shaped cavity, the surface where the straight edge of the tile-shaped cavity is located is in the same plane as the outer side surface of the magnetic conductive plate, and the cavity thickness is 5mm-25mm; The molding device further comprises an upper pressing head and a lower pressing head, wherein the upper pressing head is located directly above the tile-shaped mold cavity, and the lower pressing head is located directly below the tile-shaped mold cavity.
Citation Information
Cited By
A two-way forming device and method for a high-aspect-ratio neodymium-iron-boron radiation magnetic ring
CN122683110A