A coating structure for enhancing the corrosion resistance of mobile phone connectors

By adopting an environmentally friendly cyanide-free silver-plated layer and multi-layer coating structure on the mobile phone plug-in, the problems of short plug-and-pull and unplugging and environmental pollution are solved, and the corrosion resistance and service life are achieved. The diversified needs and environmental protection requirements of customers.

CN110820024BActive Publication Date: 2024-11-22SUZHOU MICRO JUST-TECH CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN201911359209.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-25
Publication Date
2024-11-22
Estimated Expiration
2039-12-25

AI Technical Summary

Technical Problem

The existing mobile phone charging interface has a short resistant coating and a short service life. Traditional high cyanide silver plating is harmful to the human body and the environment, and cannot meet customers' diverse needs and strict environmental protection requirements.

Method used

Using an environmentally friendly silver-plating layer without cyanide, the nickel plating layer is eliminated, and a coating structure is designed including a copper plating from bottom to top, a first silver plating, a first nickel tungsten plating, a first gold plating, a second nickel tungsten plating, and a second Gold plating, second silver plating and rhodium alloy plating enhance conductivity, oxidation resistance and corrosion resistance.

Benefits of technology

It reduces pollution to the human body and the environment, avoids skin allergies, improves the number of plug-ins and pull-up times and service life, enhances conductive properties and corrosion resistance, and meets the demanding testing needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110820024B_ABST
    Figure CN110820024B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of mobile phone accessories, and specifically relates to a coating structure that enhances the corrosion resistance of mobile phone connectors. The present invention enhances the corrosion resistance of mobile phone connectors. The connector includes a functional area, and the functional area is plated with a copper coating, a first silver coating, a first nickel-tungsten coating, a first gold coating, a second nickel-tungsten coating, a second gold coating, a second silver coating, and a rhodium alloy coating from bottom to top. The copper coating is plated on the substrate of the functional area. Through the combination of the above coatings, the hardness of the coating can be improved, so that the coating has the characteristics of wear resistance, corrosion resistance, and anti-discoloration, and the service life of the fast charging interface is extended, so that the product's coating can withstand more plug-in and unplug times, and the service life of the coating and the charging efficiency are improved, so as to achieve a more practical purpose.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mobile phone accessories, and in particular relates to a plating structure for enhancing the corrosion resistance of a mobile phone connector. Background Art

[0002] With the upgrading of smart phones, the screen size of mobile phones continues to increase, and the power consumption also increases accordingly. Mobile phones are charged more and more frequently. The plating of existing mobile phone charging interfaces mostly adopts nickel plating on copper, palladium nickel / palladium plus rhodium alloy plating, and rhodium alloy is used to enhance the corrosion resistance of the product. Traditional plating has few plug-in and pull-out resistance times, short service life, unstable electroplating process, and many abnormalities, which cannot meet the increasing diversified needs of customers and stringent environmental protection requirements. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a coating structure for enhancing the corrosion resistance of mobile phone connectors in view of the deficiencies of the above-mentioned prior art. The coating structure of the present invention adopts an environmentally friendly cyanide-free silver plating layer to reduce the harm of traditional high-cyanide silver plating to the human body and reduce the pollution to the environment, cancels the nickel plating layer, reduces the contact of the human body with the nickel layer, avoids causing skin allergies, thereby reducing the harm of electronic connectors to the human body and enhancing the conductivity, oxidation resistance and corrosion resistance of electronic products, and can increase the number of plug-in resistance and service life, meeting the increasing diversified needs of customers and stringent environmental protection requirements.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a plating structure for enhancing the corrosion resistance of a mobile phone connector, the connector comprising a functional area portion, the functional area portion being plated with a copper plating layer, a first silver plating layer, a first nickel-tungsten plating layer, a first gold plating layer, a second nickel-tungsten plating layer, a second gold plating layer, a second silver plating layer and a rhodium alloy plating layer from bottom to top, wherein the copper plating layer is plated on a substrate of the functional area portion.

[0005] The substrate of the functional area is a copper substrate.

[0006] The thickness of the copper plating layer is 0.4~5.5μm, the thickness of the first silver plating layer is 0.4~5.5μm, the thickness of the first nickel-tungsten plating layer is 0.4~5.5μm, the thickness of the first gold plating layer is 0.02~0.55μm, the thickness of the second nickel-tungsten plating layer is 0.4~5.5μm, the thickness of the second gold plating layer is 0.02~0.55μm, the thickness of the second silver plating layer is 0.4~5.5μm, and the thickness of the rhodium alloy plating layer is 0.4~5.5μm.

[0007] The cyanide content in the first silver coating and the second silver coating is zero, and the silver content in the coating is not less than 99.5%.

[0008] Compared with the prior art, the present invention has the following advantages:

[0009] The coating structure of the present invention adopts an environmentally friendly cyanide-free silver plating layer to reduce the harm of traditional high-cyanide silver plating to the human body and reduce the pollution to the environment, eliminates the nickel plating layer, reduces the contact of the human body with the nickel layer, avoids causing skin allergies, reduces the harm of electronic connectors to the human body and enhances the conductivity, oxidation resistance and corrosion resistance of electronic products, and can meet the demanding testing requirements of customers. By providing a corrosion-resistant intermediate coating layer, an oxidation-resistant layer and a wear-resistant and corrosion-resistant surface coating layer, the corrosion resistance and wear resistance of the substrate can be improved, the substrate is protected from corrosion and oxidation, the service life is long, and the corrosion resistance of the electroplating coating is enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 It is a schematic cross-sectional structure diagram of the plating structure of the mobile phone connector according to Example 1 of the present invention.

[0011] Explanation of the reference numerals: 1 - copper plating layer; 2 - first silver plating layer; 3 - first nickel tungsten plating layer; 4 - first gold plating layer; 5 - second nickel tungsten plating layer; 6 - second gold plating layer; 7 - second silver plating layer; 8 - rhodium alloy plating layer; 9 - substrate of the functional area. DETAILED DESCRIPTION

[0012] The specific implementation of the present invention is described in detail below in conjunction with the technical scheme and the accompanying drawings.

[0013] Example 1

[0014] like Figure 1 The present invention discloses a plating structure for enhancing the corrosion resistance of a mobile phone connector. The connector comprises a functional area, and the plating layers of the functional area are, from bottom to top, a copper plating layer 1, a first silver plating layer 2, a first nickel-tungsten plating layer 3, a first gold plating layer 4, a second nickel-tungsten plating layer 5, a second gold plating layer 6, a second silver plating layer 7, and a rhodium alloy plating layer 8, wherein the copper plating layer 1 is plated on a substrate 9 of the functional area.

[0015] The substrate 9 of the functional area is a copper substrate.

[0016] The copper plating layer 1 has a thickness of 1 μm, the first silver plating layer 2 has a thickness of 3 μm, the first nickel tungsten plating layer 3 has a thickness of 1.25 μm, the first gold plating layer 4 has a thickness of 0.04 μm, the second nickel tungsten plating layer 5 has a thickness of 1.25 μm, the second gold plating layer 6 has a thickness of 0.04 μm, the second silver plating layer 7 has a thickness of 1.25 μm, and the rhodium alloy plating layer 8 has a thickness of 2.0 μm.

[0017] The cyanide content in the first silver plating layer 2 and the second silver plating layer 7 is zero, and the silver content in the plating layer is 99.5%.

[0018] Example 2

[0019] A plating structure for enhancing the corrosion resistance of a mobile phone connector, the connector comprising a functional area, the plating layers of the functional area being, from bottom to top, a copper plating layer 1, a first silver plating layer 2, a first nickel-tungsten plating layer 3, a first gold plating layer 4, a second nickel-tungsten plating layer 5, a second gold plating layer 6, a second silver plating layer 7, and a rhodium alloy plating layer 8, wherein the copper plating layer 1 is plated on a substrate 9 of the functional area.

[0020] The substrate 9 of the functional area is a copper substrate.

[0021] The thickness of the copper plating layer 1 is 0.5 μm, the thickness of the first silver plating layer 2 is 2.5 μm, the thickness of the first nickel tungsten plating layer 3 is 0.75 μm, the thickness of the first gold plating layer 4 is 0.06 μm, the thickness of the second nickel tungsten plating layer 5 is 0.75 μm, the thickness of the second gold plating layer 6 is 0.03 μm, the thickness of the second silver plating layer 7 is 1 μm, and the thickness of the rhodium alloy plating layer 8 is 3.0 μm.

[0022] The cyanide content in the first silver plating layer 2 and the second silver plating layer 7 is zero, and the silver content in the plating layer is 99.5%.

[0023] Example 3

[0024] A plating structure for enhancing the corrosion resistance of a mobile phone connector, the connector comprising a functional area, the plating layers of the functional area being, from bottom to top, a copper plating layer 1, a first silver plating layer 2, a first nickel-tungsten plating layer 3, a first gold plating layer 4, a second nickel-tungsten plating layer 5, a second gold plating layer 6, a second silver plating layer 7, and a rhodium alloy plating layer 8, wherein the copper plating layer 1 is plated on a substrate 9 of the functional area.

[0025] The substrate 9 of the functional area is a copper substrate.

[0026] The thickness of the copper plating layer 1 is 0.5 μm, the thickness of the first silver plating layer 2 is 1.25 μm, the thickness of the first nickel tungsten plating layer 3 is 0.4 μm, the thickness of the first gold plating layer 4 is 0.04 μm, the thickness of the second nickel tungsten plating layer 5 is 0.5 μm, the thickness of the second gold plating layer 6 is 0.04 μm, the thickness of the second silver plating layer 7 is 0.75 μm, and the thickness of the rhodium alloy plating layer 8 is 5.5 μm.

[0027] The cyanide content in the first silver plating layer 2 and the second silver plating layer 7 is zero, and the silver content in the plating layer is 99.5%.

[0028] In embodiments 1-3 of the present invention, the copper plating layer is used to increase the flatness of the substrate, the first silver plating layer uses a cyanide-free process, is pollution-free to the environment, harmless to humans, and is used to increase the ductility of the product, the first nickel-tungsten plating layer has stable performance, and is used to improve the wear resistance and corrosion resistance of the plating layer, the first gold plating layer is used to improve the binding force of the product, the second nickel-tungsten plating layer is used to improve the wear resistance and corrosion resistance of the plating layer, the second gold plating layer is used to improve the binding force of the product, the second silver plating layer is used to improve the conductivity of the product, and the rhodium alloy plating layer is used to improve the hardness and corrosion resistance of the product. The combination of the above plating layers improves the hardness of the plating layer, makes the plating layer wear-resistant, corrosion-resistant, and discoloration-resistant, extends the service life of the fast charging interface, increases the number of plug-in and unplugging resistance of the product plating layer, improves the service life of the plating layer and the charging efficiency, and achieves a more practical purpose.

[0029] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A coating structure for enhancing the corrosion resistance of a mobile phone connector, characterized in that: The plug connector comprises a functional area portion, wherein the functional area portion is plated with a copper plating layer (1), a first silver plating layer (2), a first nickel-tungsten plating layer (3), a first gold plating layer (4), a second nickel-tungsten plating layer (5), a second gold plating layer (6), a second silver plating layer (7) and a rhodium alloy plating layer (8) in sequence from bottom to top, wherein the copper plating layer (1) is plated on a substrate (9) of the functional area portion; The substrate (9) of the functional area is a copper substrate; The copper plating layer (1) has a thickness of 0.4 to 5.5 μm, the first silver plating layer (2) has a thickness of 0.4 to 5.5 μm, the first nickel-tungsten plating layer (3) has a thickness of 0.4 to 5.5 μm, the first gold plating layer (4) has a thickness of 0.02 to 0.55 μm, the second nickel-tungsten plating layer (5) has a thickness of 0.4 to 5.5 μm, the second gold plating layer (6) has a thickness of 0.02 to 0.55 μm, the second silver plating layer (7) has a thickness of 0.4 to 5.5 μm, and the rhodium alloy plating layer (8) has a thickness of 0.4 to 5.5 μm; The cyanide content in the first silver coating (2) and the second silver coating (7) is zero, and the silver content in the coating is not less than 99.5%.

Citation Information

Patent Citations

  • Synthesis of liquid fuels from biomass

    CN102203034A

  • Electrifying corrosion-resistant plating of mobile phone rapid charge interface

    CN109853009A

  • Corrosion resistant coating of silver combined coating

    CN110396708A

  • Corrosion-resistant coating for interface of electronic device

    CN110401056A

  • Cell -phone fills corrosion resistant special cladding material of interface circular telegram soon

    CN206188898U