Semiconductor device and method for manufacturing the same

By stacking the polysilicon gate on the metal gate in DRAM and burying it, combining the composite wire and conductive contact structure, the leakage current problem caused by the metal gate is solved, and the efficiency and reliability of the DRAM are improved.

CN110896077BActive Publication Date: 2024-12-06CHANGXIN MEMORY TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811070392.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-13
Publication Date
2024-12-06
Estimated Expiration
2038-09-13

AI Technical Summary

Technical Problem

The leakage current problem caused by the metal gate in existing dynamic random access memory (DRAM) affects device performance and reliability.

Method used

A polysilicon gate is stacked on the metal gate to form a composite gate, and buried it through a gate isolation layer to reduce leakage current, and optimize contact resistance through a composite structure of the wire and conductive contact structure.

Benefits of technology

While ensuring a low resistance value of the gate, the leakage current in the overlapping areas of the gate, source and drain are reduced, and the device efficiency and reliability are improved. It is suitable for buried channel array transistor structure DRAM.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110896077B_ABST
    Figure CN110896077B_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor device and a method for preparing the same. By stacking a polysilicon gate on top of a metal gate to form a composite gate, the electric field distribution in the overlapping region between the composite gate and the source and drain can be improved, thereby being compatible with the advantages of the metal gate and the polysilicon gate. While ensuring that the gate has a low resistance value, the leakage current in the overlapping region between the gate and the source and drain can also be reduced to improve device performance and reliability. Furthermore, the first conductive contact structure under the wire is a composite structure mainly composed of a metal layer and a polysilicon layer stacked, which can reduce contact resistance and improve device performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of integrated circuit manufacturing, and in particular to a semiconductor device and a preparation method thereof. Background Art

[0002] Dynamic Random Access Memory (DRAM) is a well-known semiconductor storage device that is currently widely used in various electronic devices. Dynamic Random Access Memory (DRAM) consists of many repeated memory cells, each of which is mainly composed of a transistor and a capacitor controlled by the transistor, and the memory cells are arranged in an array. Each memory cell is electrically connected to each other through a word line (WL) and a bit line (BL).

[0003] In order to improve the integration of dynamic random access memory (DRAM) and speed up the operation speed of components, and to meet the needs of consumers for miniaturized electronic devices, the design of the length of the transistor channel region in dynamic random access memory (DRAM) has a trend of continuously shortening. However, this will cause serious problems such as short channel effect and reduced on current in the transistor. A known solution is to change the horizontal transistor structure in the dynamic random access memory (DRAM) to a vertical buried channel array transistor (BCAT) structure. The structure of the dynamic random access memory (DRAM) with a buried channel array transistor (BCAT) is as follows. Figure 1As shown, it includes: a semiconductor substrate 100, a gate (i.e., a word line of DRAM) 104, and a wire (i.e., a bit line of DRAM) 111. The gate 104 of the word BCAT is buried in a U-shaped longitudinal trench (not shown) of the semiconductor substrate 100 through a gate isolation layer 106, and is insulated and isolated from the semiconductor substrate 100 through a gate dielectric layer 102. Source / drain regions (not shown) are respectively formed in the semiconductor substrate 100 on both sides of the gate 104. The wire 111 is connected to the source / drain region on one side of the gate 104 through a first conductive contact structure 109. The source / drain region on the other side of the word line 104 is led outward through a second conductive contact structure (i.e., a conductive plug) 113 above. The wire 111 and the second conductive contact structure 113 are both formed in an interlayer dielectric layer 112. Since the current needs to flow along the U-shaped longitudinal groove portion between the source region (i.e., the source / drain region on one side of the gate 104) and the drain region (the source / drain region on the other side of the gate 104, not shown in the figure), the actual effective channel length becomes longer, which reduces the area occupied by the BCAT transistor in each storage unit and can suppress the short channel effect.

[0004] The word lines of existing dynamic random access memories are mostly formed of metal materials, that is, the gate 104 of the BCAT of the memory cell is mostly a metal gate. Compared with the polysilicon gate, the metal gate has a low resistance characteristic and better control ability for channel switching. However, when the channel is in a closed state, the metal gate will cause leakage current (such as GIDL, Gate Induced Drain leakage) in the overlapping area of ​​the gate and the source and drain, which will affect the performance and reliability of the memory cell and even cause problems such as DRAM data access errors.

[0005] In view of this, it is necessary to design a new semiconductor device and a preparation method thereof to solve the above problems. Summary of the invention

[0006] The object of the present invention is to provide a semiconductor device and a method for preparing the same, which can combine the advantages of a metal gate and a polysilicon gate, and can reduce the leakage current in the overlapping area between the gate and the source and drain while ensuring that the gate has a low resistance value, so as to improve the device performance and reliability.

[0007] In order to solve the above technical problems, the present invention provides a method for preparing a semiconductor device, comprising the following steps:

[0008] Providing a semiconductor substrate having a gate trench;

[0009] Filling a metal gate in the gate trench, wherein the height of the metal gate is smaller than the depth of the gate trench; and,

[0010] A polysilicon gate is filled in the gate trench, and the polysilicon gate is stacked on the metal gate to form a composite gate.

[0011] Optionally, the top surface of the polysilicon gate is lower than the top surface of the semiconductor substrate on the side wall of the gate trench, and the method for preparing the semiconductor device also includes: filling a gate isolation layer in the gate trench, the gate isolation layer fills the gate trench to bury the metal gate and the polysilicon gate therein.

[0012] Optionally, before filling the metal gate in the gate trench, a gate dielectric layer is first formed on the sidewalls and bottom wall of the gate trench.

[0013] Optionally, after forming the gate dielectric layer and before filling the metal gate, a metal barrier layer is formed on the surface of the gate dielectric layer, and after the metal gate is filled, the metal barrier layer surrounds the bottom wall and side walls of the metal gate and exposes the surface of the gate dielectric layer above the metal gate, so that the side walls of the polysilicon gate are directly in contact with the surface of the gate dielectric layer.

[0014] Optionally, the method for preparing a semiconductor device further includes:

[0015] forming a first conductive contact structure on the semiconductor substrate at one side of the gate trench;

[0016] forming a conductive line on the first conductive contact structure;

[0017] forming an interlayer dielectric layer covering the gate trench and the semiconductor substrate, wherein the interlayer dielectric layer buries the conductive wire and the first conductive contact structure; and,

[0018] A second conductive contact structure is formed in the interlayer dielectric layer, wherein a bottom surface of the second conductive contact structure contacts a surface of the semiconductor substrate at the other side of the gate trench.

[0019] Optionally, at least one active area is formed in the semiconductor substrate, two gate trenches are arranged side by side in the active area, a first source / drain area is formed in the active area between the two gate trenches, second source / drain areas are respectively formed in the active areas on opposite sides of the two gate trenches, the first conductive contact structure is formed above the first source / drain area and the bottom surface is in contact with the top surface of the first source / drain area, and the second conductive contact structure is formed above the second source / drain area and the bottom surface is in contact with the top surface of the second source / drain area.

[0020] Optionally, the step of forming the first conductive contact structure includes:

[0021] Forming a hard mask layer covering the gate trench and the semiconductor substrate, wherein the hard mask layer has an opening exposing a surface of the active area between the two gate trenches;

[0022] Using the hard mask layer as a mask, etching the exposed active area to form a contact trench, wherein the bottom surface of the contact trench is higher than the top surface of the polysilicon gate; and,

[0023] The first conductive contact structure is filled in the contact trench, and the hard mask layer is removed.

[0024] Optionally, the contact trench is connected to the two gate trenches at side walls respectively, and the step of forming the conductive line includes:

[0025] Forming a sacrificial layer covering the gate trench, the semiconductor substrate and the first conductive contact structure, wherein the sacrificial layer has an opening exposing a portion of the surface of the first conductive contact structure;

[0026] filling the conductive line in the opening of the sacrificial layer; and,

[0027] The sacrificial layer is removed, and the first conductive contact structure is etched to the interface between the bottom surface of the first conductive contact structure and the semiconductor substrate using the conductive line as a mask, so that the first conductive contact structure is as wide as the conductive line.

[0028] Optionally, the first conductive contact structure is a composite structure including a metal layer and a polysilicon layer stacked on the metal layer, and the material of the conductive line includes metal.

[0029] The present invention also provides a semiconductor device, comprising:

[0030] A semiconductor substrate having a gate trench;

[0031] a metal gate filled in the gate trench, wherein the height of the metal gate is less than the depth of the gate trench; and

[0032] A polysilicon gate is filled in the gate trench and is stacked on the metal gate.

[0033] Optionally, the top surface of the polysilicon gate is lower than the top surface of the semiconductor substrate on the side wall of the gate trench, and the semiconductor device also includes: a gate isolation layer filled in the gate trench, the gate isolation layer fills the gate trench to bury the metal gate and the polysilicon gate therein.

[0034] Optionally, the semiconductor device also includes a gate dielectric layer and a metal barrier layer, the gate dielectric layer is formed on the side walls and bottom walls of the gate trench, the metal barrier layer is formed between the gate dielectric layer and the metal gate, surrounds the bottom wall and side walls of the metal gate and exposes the surface of the gate dielectric layer above the metal gate, and the side walls of the polysilicon gate are directly in contact with the side wall surfaces of the gate dielectric layer exposed by the metal barrier layer.

[0035] Optionally, the semiconductor device further includes:

[0036] A first conductive contact structure is formed on the semiconductor substrate at one side of the gate trench;

[0037] A conductive line formed on the first conductive contact structure;

[0038] an interlayer dielectric layer, covering the gate trench and the semiconductor substrate, wherein the interlayer dielectric layer buries the conductive wire and the first conductive contact structure; and

[0039] A second conductive contact structure is formed in the interlayer dielectric layer, and a bottom surface of the second conductive contact structure contacts a surface of the semiconductor substrate at the other side of the gate trench.

[0040] Optionally, at least one active area is formed in the semiconductor substrate, two gate trenches are arranged side by side in the active area, a first source / drain area is formed in the active area between the two gate trenches, second source / drain areas are respectively formed in the active areas on opposite sides of the two gate trenches, the first conductive contact structure is formed above the first source / drain area and the bottom surface is in contact with the top surface of the first source / drain area, and the second conductive contact structure is formed above the second source / drain area and the bottom surface is in contact with the top surface of the second source / drain area.

[0041] Optionally, a gap is formed between the first conductive contact structure and the sidewalls of the gate trench facing each other, and the interlayer dielectric layer fills the gap.

[0042] Optionally, the first conductive contact structure is a composite structure including a metal layer and a polysilicon layer stacked on the metal layer, and the material of the conductive line includes metal.

[0043] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0044] 1. The semiconductor device and its preparation method of the present invention can improve the electric field distribution in the overlapping area between the composite gate and the source and drain by stacking a polysilicon gate on top of a metal gate to form a composite gate, thereby being compatible with the advantages of the metal gate and the polysilicon gate, and while ensuring that the gate has a low resistance value, it can also reduce the leakage current in the overlapping area between the gate and the source and drain to improve the device performance and reliability. Furthermore, the first conductive contact structure under the wire (i.e., the bit line in the memory) is a composite structure mainly composed of a metal layer and a polysilicon layer stacked, which can reduce the contact resistance and improve the device performance.

[0045] 2. The semiconductor device and preparation method of the present invention are suitable for manufacturing any product with a metal gate, and are particularly suitable for dynamic random access memory (DRAM) with a buried channel array transistor (BCAT) structure. They can improve the data access errors of DRAM caused by the leakage path in the overlapping area between the gate and the source and drain, and improve the performance of DRAM. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 FIG. 1 is a schematic diagram of a cross-sectional structure of a known DRAM with BCAT (only the structure at one active region is shown).

[0047] Figure 2 The present invention is a flow chart of a method for preparing a semiconductor device according to a specific embodiment of the present invention.

[0048] Figures 3A to 3I yes Figure 2 A schematic cross-sectional view of a device structure in a method for preparing a semiconductor device is shown.

[0049] Figure 4 It is a schematic cross-sectional view of a semiconductor device according to an embodiment of the present invention.

[0050] The reference numerals are as follows:

[0051] 100- semiconductor substrate;

[0052] 1002-first source / drain region;

[0053] 1003- second source / drain region;

[0054] 101-gate trench;

[0055] 102-gate dielectric layer;

[0056] 103, 1042, 1094, 1097 - metal barrier layer;

[0057] 104-metal gate;

[0058] 1041, 1093, 1098 - metal adhesion layer;

[0059] 1043, 1095, 1096-Metal silicide layer

[0060] 105-polysilicon gate;

[0061] 106-gate isolation layer;

[0062] 107-hard mask layer;

[0063] 108-contact groove;

[0064] 108a-gap;

[0065] 109-a first conductive contact structure;

[0066] 1091 - a metal layer in a first conductive contact structure;

[0067] 1092-polysilicon layer in the first conductive contact structure;

[0068] 110-sacrificial layer;

[0069] 111 - conductor (when the semiconductor device is a memory, the conductor is a bit line);

[0070] 112-interlayer dielectric layer;

[0071] 113 - second conductive contact structure. DETAILED DESCRIPTION

[0072] The integrated circuit memory and the method for manufacturing the same proposed by the present invention are further described in detail below in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer according to the following description. It should be noted that the accompanying drawings are in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0073] Please refer to Figure 2 An embodiment of the present invention provides a method for preparing a semiconductor device, comprising the following steps:

[0074] S1, providing a semiconductor substrate having a gate trench;

[0075] S2, filling a metal gate in the gate trench, wherein the height of the metal gate is smaller than the depth of the gate trench; and

[0076] S3, filling a polysilicon gate in the gate trench, wherein the polysilicon gate is stacked on the metal gate to form a composite gate;

[0077] S4, filling a gate isolation layer in the gate trench, and forming a first conductive contact structure and a conductive line stacked on the semiconductor substrate at one side of the gate trench;

[0078] S5, forming an interlayer dielectric layer on the semiconductor substrate and the gate isolation layer, and forming a second conductive contact structure in the interlayer dielectric layer, wherein the interlayer dielectric layer buries the conductive wire, and the second conductive contact structure contacts the semiconductor substrate on the other side of the gate trench.

[0079] Please refer to Figure 3A First, step S1 is performed to provide a semiconductor substrate 100 having a gate trench 101. The specific process includes:

[0080] Step 1, provide a semiconductor substrate 100. The semiconductor substrate 100 can be any substrate known to those skilled in the art for carrying semiconductor integrated circuit components, such as silicon-on-insulator (SOI), bulk silicon, germanium, silicon germanium, gallium arsenide or germanium on insulator. The semiconductor substrate 100 in this embodiment includes a base 1001 and a semiconductor epitaxial layer (not shown) epitaxially grown on its surface. The semiconductor substrate 100 can be defined with at least one active area (not shown, formed in the semiconductor epitaxial layer) for forming a buried channel array transistor (BCAT) and a shallow trench isolation structure (not shown) for isolating the active area from the surrounding environment. The active area can be a fin-type three-dimensional structure or a planar structure. When the semiconductor device to be manufactured is a memory, the shallow trench isolation structure can isolate all active areas into an array arrangement to manufacture a memory array of the memory. The shallow trench isolation structure may include a shallow trench (not shown) located in the semiconductor substrate 100 and a dielectric material filling the shallow trench. The dielectric material may include a liner oxide layer (line oxide layer) formed by a thermal oxidation process and covering the shallow trench. The invention relates to a method for forming a shallow trench isolation structure of a semiconductor substrate 100, wherein the semiconductor substrate 100 is provided with a pad oxide layer and a silicon dioxide layer located on the surface of the pad oxide layer and filling the shallow trench, thereby improving the isolation performance of the shallow trench isolation structure. The specific formation process includes: (1) forming a pad oxide layer (not shown) on the surface of the semiconductor substrate 100 by a thermal oxidation process; (2) forming a silicon nitride hard mask layer (not shown) by a chemical vapor deposition process, and further forming a patterned photoresist layer (not shown) on the silicon nitride hard mask layer by photoresist coating, exposure, development and other photolithography processes, wherein the patterned photoresist layer covers the active area and the layers above it, and exposes the silicon nitride hard mask layer above the semiconductor substrate 100 used as an isolation area between the active areas; (3) using the patterned photoresist layer as a mask, performing photolithography on the exposed silicon nitride hard mask layer and the pad oxide layer below it and the semiconductor substrate 100 at a certain depth. (4) removing the patterned photoresist layer; (5) forming a liner oxide layer (not shown) on the sidewall and bottom surface of the shallow trench by a vapor deposition process or a thermal oxidation process; (6) depositing silicon dioxide on the surface of the shallow trench and the surface of the silicon nitride hard mask layer by a process such as chemical vapor deposition until the silicon dioxide fills the shallow trench; (7) flattening the top surface of the silicon dioxide by a chemical mechanical planarization process until the top surface of the silicon dioxide is flush with the top surface of the silicon nitride hard mask layer to form a shallow trench isolation structure; (8) removing the silicon nitride hard mask layer by a process such as wet etching.Further, after depositing silicon dioxide, or after flattening the top surface of the silicon dioxide, or after removing the silicon nitride hard mask layer, the silicon dioxide is subjected to densification by high-energy light activation processes such as high-temperature thermal annealing, ultraviolet light (UV) or laser, etc., so as to increase the density of the dielectric material, ensure the isolation effect of the shallow trench isolation structure, and strengthen its mechanical strength. The process temperature of the high-temperature thermal annealing process is, for example, 800°C to 1200°C, and highly reactive gases such as ozone (O3) and / or carbon monoxide (CO) may be further introduced during the high-temperature thermal annealing process. In addition, after forming the shallow trench isolation structure, a well region (not shown) may be formed in each active region by an ion implantation process and further combined with annealing activation processes, wherein the doping type of the well region is determined by the conductivity type of the BCAT transistor to be formed. For example, in this embodiment, if the formed BCAT transistor is an N-type transistor, the well region is a P-type doped region. The doping depth of the well region can be adjusted according to actual conditions. It should be noted that the above-mentioned pad oxide layer can protect the semiconductor substrate 100 and the active area during the process of forming the shallow trench isolation structure, and the pad oxide layer can continue to be retained as a protective layer for the top surface of the semiconductor substrate 100 and the active area in subsequent processes.

[0081] Step 2, please continue to refer to Figure 3A, a patterned hard mask layer (not shown) is sequentially formed on the surface of the shallow trench isolation structure and the pad oxide layer. The specific formation process includes: (1) a hard mask layer can be formed on the surface of the shallow trench isolation structure and the pad oxide layer by chemical vapor deposition (CVD), physical vapor deposition (PVD) or atomic layer deposition (ALD) and other processes. The material of the hard mask layer includes at least one of silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride, metal nitride, metal oxide and metal carbide, preferably silicon nitride (SiN). Silicon nitride material is easy to obtain, low in cost, mature in manufacturing method, and has a high etching selectivity with the pad oxide layer; (2) a hard mask layer can be formed by photoresist coating, using a gate mask (gate (1) a photoresist layer having the opening is used as a mask, and the hard mask layer is etched to the surface of the pad oxide layer to transfer the gate (i.e., word line) pattern in the photoresist to the hard mask layer; (2) the photoresist is removed, and the hard mask layer is used as a mask to continue etching downward, that is, the pad oxide layer and the semiconductor substrate 100 (including the active area and the shallow trench isolation structure) are etched in sequence to form a gate trench 101 in the semiconductor substrate 100. In this embodiment, the bottom wall of the gate trench 101 also extends downward into the substrate 1001. The shape of the gate trench 101 can be a rounded U-shape, a right-angled U-shape, or a trapezoidal shape with a wide top and a narrow bottom. Since the electrical characteristics of the buried channel array transistor (BCAT) can be changed according to the depth from the upper surface (i.e., the top surface) of the semiconductor substrate to the bottom surface of its buried gate, the depth of the gate trench 101 can be adjusted to achieve the required electrical characteristics of the buried channel array transistor (BCAT), thereby improving the electrical performance and reliability of the ultimately formed semiconductor device.

[0082] Step 3, please continue to refer to Figure 3A , the pad oxide layer, hard mask layer, etc. on the surface of the semiconductor substrate 100 can be removed by etching process or chemical mechanical planarization process, and further cleaned to expose the clean active area surface and the sidewall and bottom surface of the gate trench 101, so as to prepare for the formation of the composite gate. In this embodiment, two gate trenches 101 are arranged side by side in an active area of ​​the semiconductor substrate 100, and the active area between the two gate trenches 101 is used to form the first source / drain area later, and the active areas on the opposite sides of the two gate trenches 101 are used to form the second source / drain area respectively later, so that two BCATs can be made in one active area, which is conducive to improving the device integration.

[0083] Please continue to refer to Figure 3AIn step S2, a metal gate 104 is filled in the gate trench 101. The specific process includes:

[0084] Step 1: A thermal oxidation (dry oxygen or wet oxygen) process, chemical vapor deposition, atomic layer deposition and other processes may be used to cover the gate dielectric layer 102 on the active area and the sidewall and bottom surface of the gate trench 101. The material of the gate dielectric layer 102 is preferably a high-K dielectric (dielectric constant K is greater than 7). The material of the high-K dielectric is, for example, Ta2O5, TiO2, TiN, Al2O3, Pr2O3, La2O3, LaAlO3, HfO2, ZrO2 or other metal oxides, etc., to be compatible with the metal gate 104 to be formed, which is conducive to improving the mobility of carriers and improving device performance. It is also preferred to use atomic layer deposition (ALD) to prepare the gate dielectric layer 102 of high-K dielectric material to maintain the film quality and thickness uniformity of the gate dielectric layer 102.

[0085] Step 2, depositing a metal barrier layer 103 on the surface of the gate dielectric layer 102 by physical vapor deposition, chemical vapor deposition, atomic layer deposition and other processes. Preferably, the metal barrier layer 103 is prepared by atomic layer deposition process to protect the gate dielectric layer 102 and prevent the gate dielectric layer 102 from deteriorating in quality. The metal barrier layer 103 is also called a metal barrier layer or a metal adhesion barrier layer, which is intended to protect the gate dielectric layer 102 from the introduction of metal impurities in subsequent steps, and to improve the adhesion between the gate dielectric layer 102 and the metal gate 104. For example, in this embodiment, the metal gate 104 includes one or more work function metal layers. In the absence of the metal barrier layer 103, the metal materials from those work function metal layers will diffuse into the gate dielectric layer 102, thereby causing manufacturing defects. In various embodiments, the metal barrier layer 103 includes a metal layer such as Ti or Ta, a metal nitride layer such as TiAlN, TaCN, TaSiN, TiN or TaN, or any combination of metals and metal nitrides. It should be recognized that in some cases, a single-layer metal barrier layer 103 may not provide sufficient protection for the gate dielectric layer 102, and it is necessary to form a metal barrier layer 103 with a composite structure of multiple layers stacked in the gate trench 101 to enhance the protection of the gate dielectric layer 102 to prevent the surface metal barrier layer 103 from being etched and damaged, and the material in the metal gate 104 will be contaminated and diffused into the gate dielectric layer 102, causing device defects.

[0086] Step three, depositing metal gate material on the surface of the metal barrier layer 103 by processes such as evaporation, electroplating, chemical vapor deposition, and atomic layer deposition. The deposition thickness of the metal gate material on the bottom surface of the first gate trench 101 must at least reach the thickness required for the metal gate 104 to be formed.

[0087] In step 4, the metal gate material on the area outside the gate trench 101 can be removed by etching back, and the metal gate material is only filled in the gate trench 101 to serve as the metal gate 104. The etching back process makes the height of the metal gate 104 smaller than the depth of the gate trench 101, and reduces the height of the metal barrier layer 103 to not higher than the metal gate 104. The metal gate 104 is generally a stacked structure, including a work function metal layer covering the metal barrier layer 103 and a metal electrode layer surrounded by the work function metal layer. The material selection of the work function metal layer is determined by the conductivity type of the BCAT transistor to be formed. When the BCAT transistor to be formed is a P-type transistor, the work function metal layer in the metal gate 104 is a P-type work function metal material, and the P-type work function metal material may include TiN, TaN, Ru, Mo, Al, WN, ZrSi2, MoSi2, TaSi2, NiSi2, W, other suitable P-type work function materials, or a combination thereof. When the BCAT transistor to be formed is an N-type transistor, the work function metal layer in the metal gate 104 is an n-type work function metal material, and the n-type work function metal material includes Ti, Ag, TaAl, TaAlC, TiAlN, TaC, TaCN, TaSiN, Mn, Zr, other suitable N-type work function materials, or a combination thereof. The work function metal layer may be a single layer or multiple layers. In this embodiment, the top surface of the metal gate 104 is lower than the top surface of the semiconductor substrate 100 on both sides, and further lower than the top surface of the first source / drain region 1002 and the second source / drain region 1003 formed subsequently, so that the distance between the work function metal layer and the first source / drain region 1002 and the second source / drain region 1003 is increased, which is beneficial to prevent the work function metal layer from causing gate-induced drain leakage (GIDL) between the first source / drain region 1002 and the second source / drain region 1003. The material of the metal electrode layer may include Al, W, Cu and / or other suitable metal materials.

[0088] Please refer to Figure 3B In step S3, a polysilicon gate 105 is filled in the gate trench 101. The specific process includes:

[0089] Step 1: Atomic layer deposition is used to deposit a metal adhesion layer 1141, a metal barrier layer 1142, and a metal silicide layer 1143. The metal adhesion layer 1141 can enhance the adhesion between the metal gate 104 and the polysilicon gate 105 to prevent the composite gate formed in the end from breaking. The material of the adhesion layer 1141 can be a metal such as W, Ti, or Ta. The metal barrier layer 1142 can prevent the metal in the metal gate 104 from diffusing into the polysilicon gate 105 and affecting the performance of the metal gate 104 and the polysilicon gate 105. The material of the metal barrier layer 1142 can be a metal nitride such as TiAlN, TaCN, TaSiN, TiN, or TaN. The metal silicide layer 1143 can reduce the contact resistance between the metal gate 104 and the polysilicon gate 105 to reduce the resistance of the composite gate formed. The metal silicide layer 1143 can be a metal silicide containing at least one of the metal elements such as Ti, W, Co, Ni, Zr, Mo, and Ta.

[0090] In step two, physical vapor deposition, chemical vapor deposition, atomic layer deposition and other processes may be used to deposit polysilicon material on the gate dielectric layer 102, the metal barrier layer 103, the metal gate 104 and the surface of the semiconductor substrate 100. The polysilicon material may include at least one of doped polysilicon and undoped polysilicon, and the doping ion type of the doped polysilicon is the same as the doping ion type of the first source / drain region 1002 and the second source / drain region 1003 to be formed.

[0091] In step three, the deposited polysilicon material can be etched back using a dry etching or wet etching process to remove the polysilicon material on the area outside the gate trench 101, so that the polysilicon material is only filled in the gate trench 101 and used as a polysilicon gate 105 stacked on the metal gate 104.

[0092] Please refer to Figures 3B to 3G In step S4, a gate isolation layer 106 is filled in the gate trench 101, and a first conductive contact structure 109 and a wire 111 are formed and stacked on the semiconductor substrate 100 on one side of the gate trench 101. The specific process includes:

[0093] Step 1: Please refer to Figure 3B and 3C A gate isolation layer 106 is deposited on the semiconductor substrate 100 and the polysilicon gate 105 by using physical vapor deposition, chemical vapor deposition, atomic layer deposition and other processes. The material of the gate isolation layer 106 includes but is not limited to silicon oxide, silicon nitride and silicon oxynitride.

[0094] Step 2: Please refer to Figure 3C, the redundant gate isolation layer 106 and the gate dielectric layer 102 on the top surface of the semiconductor substrate 100 can be removed by a chemical mechanical planarization process to form a composite gate buried in the gate trench 101, the composite gate comprising a metal gate 104 and a polysilicon gate 105 stacked thereon, and further using the composite gate and the gate isolation layer 106 as masks, LDD (lightly doped drain) ion implantation, Halo (halo) ion implantation, and source-drain heavily doped ion implantation are performed on the active regions on both sides of the composite gate (i.e., the gate trench 101), so as to form a first source / drain region 1002 and a second source / drain region 1003 in the active regions on both sides of the composite gate (i.e., the gate trench 101), respectively. Thus, the composite gate and the first source / drain region 1002 and the second source / drain region 1003 separated on both sides of the composite gate constitute the main part of the BCAT structure. In this embodiment, since two gate trenches 101 are formed in one active area, two BCATs can be manufactured in one active area, and a first source / drain region 1002 common to the two BCATs is formed in the active area between the two gate trenches 101. The common first source / drain region 1002 can be a drain region electrically connected to a subsequently formed conductive line 111 (i.e., a bit line of the memory), and the second source / drain region 1003 can be a source region electrically connected to a subsequently formed second conductive contact structure. In other embodiments of the present invention, the gate dielectric layer 102 and the gate isolation layer 106 on the surface of the active region between the two composite gates and outside the two composite gates can also be etched by an etching process to form an opening exposing the surface of the active region for forming the first source / drain region 1002 and the second source / drain region 1003, and then, the exposed active region is subjected to LDD (lightly doped drain) ion implantation, Halo (halo) ion implantation, and source / drain heavily doped ion implantation, etc., using the remaining gate dielectric layer 102 and the gate isolation layer 106 as a mask, so as to form the first source / drain region 1002 and the second source / drain region 1003 in the active region on both sides of the composite gate. When the gate trench 101 is a U-shaped trench, a U-shaped conductive channel can be formed along the conduction direction of the current (i.e., the current flow direction from the source region to the drain region on both sides of the composite gate), thereby increasing the length of the conductive channel. Thus, as the size of the transistor decreases, even if the absolute distance between the source region and the drain region on both sides of the composite gate decreases, the short channel effect of the transistor structure can be effectively improved because the formed conductive channel is a U-shaped channel.Moreover, since the composite gate is mainly formed by a polysilicon gate and a metal gate stacked together, the electric field distribution in the overlapping area between the composite gate and the first source / drain region 1002 and the second source / drain region 1003 can be improved. Thus, the advantages of the metal gate and the polysilicon gate can be compatible. While ensuring that the gate has a low resistance value, the leakage current in the overlapping area between the gate and the first source / drain region 1002 and the second source / drain region 1003 can also be reduced, thereby improving device performance and reliability. In addition, the first source / drain region 1002 and the second source / drain region 1003 are doped with ions of corresponding conductivity types according to transistor structures of different conductivity types. For example, when the transistor structure is an N-type transistor, the doped ions in the source / drain region are N-type doped ions, and the N-type doped ions are, for example, phosphorus (P) ions, arsenic (As) ions, and antimony (Sb) ions; when the transistor structure is a P-type transistor, the doped ions in the source / drain region are P-type doped ions, and the P-type doped ions are, for example, boron (B) ions and boron fluoride (BF2). + ) ions, gallium (Ga) ions, and indium (In) ions.

[0095] Step 3: Please refer to Figure 3D A hard mask layer 107 is formed on the semiconductor substrate 100 and the gate isolation layer 106, and the hard mask layer 107 above the first source / drain region 1002 is opened by photolithography and etching processes to form an opening exposing the surface of the first source / drain region 1002.

[0096] Step 4: Please refer to Figure 3D , using the hard mask layer 107 with the opening as a mask, the first source / drain region 1002 is etched to a certain depth to form a contact trench 108, the bottom surface of the contact trench 108 is higher than the top surface of the polysilicon gate 105. In this embodiment, the contact trench 108 is connected to the two gate trenches 101 at the sidewalls.

[0097] Step 5: Please refer to Figure 3D and 3E , by using physical vapor deposition, chemical vapor deposition, atomic layer deposition and other processes, polysilicon material is deposited on the surface of the contact trench 108 and the hard mask layer 107 until the deposited polysilicon material fills the contact trench 108, and the polysilicon material may include at least one of doped polysilicon and undoped polysilicon. A chemical mechanical planarization (CMP) process is further used to remove the polysilicon material outside the hard mask layer 107 and the contact trench 108 to form a first conductive contact structure 109.

[0098] Step 6: Please refer to Figure 3F and 3GThe sacrificial layer 110 can be formed by spin coating, chemical vapor deposition, physical vapor deposition and other processes to cover the gate isolation layer 106, the semiconductor substrate 100 and the first conductive contact structure 109, and an opening 110a is further formed in the sacrificial layer 110 by photolithography, etching and the like, and the width of the opening 110a is less than Figure 3D The width of the contact groove 108 shown in the figure is to expose a portion of the top surface of the first conductive contact structure 109; the deposition thickness of the sacrificial layer 110 can determine the height of the wire 110, and its material can be silicon oxide, silicon nitride, silicon oxynitride, fluorine-doped silicate glass (FSG), low-k dielectric material and / or other suitable insulating materials.

[0099] Step 7. Please refer to Figure 3F and 3G The opening 110 a is filled with Al, W, Cu and / or other suitable metal materials through processes such as evaporation, electroplating, chemical vapor deposition, and atomic layer deposition, and the metal material on the top of the sacrificial layer 110 is further removed by a chemical mechanical planarization process to form a wire 111 .

[0100] Step 8. Please refer to Figure 3G and Figure 3H , the sacrificial layer 110 is removed by a suitable process such as etching, and the first conductive contact structure 109 is further etched using the conductive line 111 as a mask, and the etching stops at the interface between the first source and drain region 1002 and the first conductive contact structure 109 to form a gap 108a. At this time, the first conductive contact structure 109 is the same width as the conductive line 111.

[0101] Please refer to Figure 4In other embodiments of the present invention, the first conductive contact structure 109 may also be a composite structure, mainly composed of a metal layer 1091 and a polysilicon layer 1092 stacked on the metal layer 1091, thereby reducing the contact resistance and avoiding the problem that when the first conductive contact structure 109 is etched using the wire 111 as a mask, the side wall of the remaining first conductive contact structure 109 is reduced in cross-sectional area due to lateral etching. In one embodiment of the present invention, there are a metal silicide layer (not shown), a metal barrier layer (not shown) and a metal adhesion layer (not shown) between the metal layer 1091 and the first source and drain region 1002 from bottom to top, wherein the metal adhesion layer can enhance the adhesion between the metal layer 1091 and the first source and drain region 1002 to prevent poor contact between the first conductive contact structure 109 and the first source and drain region 1002, and the material of the metal adhesion layer can be a metal such as W, Ti or Ta; the metal barrier layer can prevent the metal in the metal layer from diffusing into the first source and drain region 1002 and affecting the performance of the first source and drain region 1002, and the material of the metal barrier layer can be a metal nitride such as TiAlN, TaCN, TaSiN, TiN or TaN; the metal silicide layer can reduce the contact resistance between the metal layer and the first source and drain region 1002, and the metal silicide layer can be a metal silicide containing at least one of the metal elements such as Ti, W, Co, Ni, Zr, Mo, Ta, etc.In another embodiment of the present invention, a metal adhesion layer 1093, a metal barrier layer 1094, and a metal silicide layer 1095 are sequentially formed between the metal layer 1091 and the polysilicon layer 1092 from bottom to top, and a metal silicide layer 1096, a metal barrier layer 1097, and a metal adhesion layer 1098 are sequentially formed between the polysilicon layer 1092 and the bit line 111 from bottom to top, wherein the metal adhesion layer 1093 can enhance the adhesion between the metal layer 1091 and the polysilicon layer 1092 to prevent the metal layer 1091 and the polysilicon layer 1092 from having poor contact or even cracking, the metal adhesion layer 1098 can enhance the adhesion between the wire 111 and the polysilicon layer 1092 to prevent the bit line 111 and the polysilicon layer 1092 from having poor contact or even cracking, and the materials of the metal adhesion layers 1093 and 1098 can be metals such as W, Ti, or Ta; the metal barrier layer 1094 can be Prevent the metal in the metal layer 1091 from diffusing into the polysilicon layer 1092. The metal barrier layer 1097 can prevent the metal in the wire 111 from diffusing into the polysilicon layer 1092. The materials of the metal barrier layers 1094 and 1097 can be metal nitrides such as TiAlN, TaCN, TaSiN, TiN or TaN. The metal silicide layer 1095 can reduce the contact resistance between the metal layer 1091 and the polysilicon layer 1092, and further prevent the metal in the metal layer 1091 from diffusing into the polysilicon layer 1092. The metal silicide layer 1096 can reduce the contact resistance between the wire 111 and the polysilicon layer 1092 and further prevent the metal in the wire 111 from diffusing into the polysilicon layer 1092. The metal silicide layers 1095 and 1096 can be metal silicides containing at least one of the metal elements such as Ti, W, Co, Ni, Zr, Mo, Ta, etc.

[0102] Please refer to Figure 3H , 3I as well as Figure 4In step S5, first, a process such as spin coating, chemical vapor deposition, physical vapor deposition, etc. can be used, which can be further combined with a chemical mechanical planarization process to form an interlayer dielectric layer 112 with a flat top surface to cover the gate isolation layer 106, the first source / drain region 1002, the second source / drain region 1003, the first conductive contact structure 109 and the wire 111. The interlayer dielectric layer 112 fills the gap 108a and buries the wire 111 and the first conductive contact structure 109 therein. The material of the interlayer dielectric layer 112 can be silicon oxide, silicon nitride, silicon oxynitride, fluorine-doped silicate glass (FSG), low-k dielectric material and / or other suitable insulating materials. Then, a contact hole (not shown) aligned with the second source / drain region 1003 is formed in the interlayer dielectric layer 112 by photolithography, etching and other processes, and the contact hole exposes the top surface of the second source / drain region 1003 to expose part of the top surface of the first conductive contact structure 109. Next, a metal material is filled into the contact hole by electroplating, sputtering and other processes to form a second conductive contact structure 113 (i.e., a conductive contact plug) filled in the contact hole of the interlayer dielectric layer 112, and the bottom surface of the second conductive contact structure 113 contacts the top surface of the second source / drain region 1003.

[0103] The method for preparing a semiconductor device of the present invention substantially replaces the existing single metal gate with a composite gate formed by stacking a polysilicon gate on top of the metal gate, thereby improving the electric field distribution in the overlapping area between the composite gate and the source and drain. Thus, it is compatible with the advantages of the metal gate and the polysilicon gate. While ensuring that the gate has a low resistance value, it is also possible to reduce the leakage current in the overlapping area between the gate and the source and drain, thereby improving the device performance and reliability. Furthermore, the first conductive contact structure below the wire (i.e., the bit line in the memory) is a composite structure mainly composed of a stack of metal layers and polysilicon layers, which can reduce contact resistance and improve device performance, and is particularly suitable for the manufacture of memories. When the method for preparing a semiconductor device of the present invention is applied to the manufacture of memories, the composite gates of multiple active areas are aligned and connected together to form the word lines of the memory, and the wires 111 of multiple active areas are aligned and connected together to form the bit lines of the memory. For example, please refer to Figures 3A to 3IIn one embodiment of the present invention, the semiconductor substrate 100 has a plurality of active areas arranged in unit rows (i.e., corresponding to the word line direction) and unit columns (i.e., corresponding to the bit line direction), and a shallow trench isolation structure is also provided between adjacent active areas, that is, all shallow trench isolation structures may include several parallel lines and several intersecting lines, thereby isolating all active areas into an array structure arranged in unit rows and unit columns, for making a memory array of a memory. Each of the active areas arranged along the word line direction intersects with two adjacent gate trenches 101. The composite gate filled in each gate trench serves as the word line corresponding to the corresponding unit row, and the wire 110 on the active area between the two gate trenches 101 serves as the bit line on the corresponding unit column.

[0104] Please refer to Figures 3A to 3I An embodiment of the present invention provides a semiconductor device, which is preferably prepared by the above-mentioned method for preparing a semiconductor device of the present invention. The semiconductor device includes: a semiconductor substrate 100 having a gate trench 101, a metal gate 104, a polysilicon gate 105, a first conductive contact structure 109, a wire 111, an interlayer dielectric layer 112 and a second conductive contact structure 113.

[0105] Among them, a first source / drain region 1002 and a second source / drain region 1103 are respectively formed in the semiconductor substrate 100 on both sides of the gate trench 101, the metal gate 104 is filled in the gate trench 101, and the height of the metal gate 104 is less than the depth of the gate trench 101; the polysilicon gate 105 is filled in the gate trench 101 and stacked on the metal gate 104.

[0106] In this embodiment, the top surface of the polysilicon gate 105 is lower than the top surface of the semiconductor substrate 100 on the side wall of the gate trench 101. The semiconductor device also includes a gate isolation layer 106, which is filled in the gate trench 101 and fills the gate trench 101, burying the metal gate 104 and the polysilicon gate 105 therein.

[0107] In this embodiment, the semiconductor device further includes a gate dielectric layer 102 and a metal barrier layer 103, wherein the gate dielectric layer 102 is formed on the side walls and bottom walls of the gate trench 101, and the metal barrier layer 103 is formed between the gate dielectric layer 102 and the metal gate 104 and surrounds the bottom wall and side walls of the metal gate 104, and the metal barrier layer 103 exposes the side wall surface of the gate dielectric layer 102 above the metal gate 104, and the side wall of the polysilicon gate 105 is directly in contact with the side wall surface of the gate dielectric layer 102 exposed by the metal barrier layer 103. The material of the gate dielectric layer 102 is preferably a high-K dielectric (dielectric constant K is greater than 7), and the material of the high-K dielectric is, for example, Ta2O5, TiO2, TiN, Al2O3, Pr2O3, La2O3, LaAlO3, HfO2, ZrO2 or other metal oxides, so as to be compatible with the metal gate 104 to be formed, which is conducive to improving the mobility of carriers and improving device performance. The metal barrier layer 103 is intended to protect the gate dielectric layer 102, avoid the introduction of metal impurities into the gate dielectric layer 102, and improve the adhesion between the gate dielectric layer 102 and the metal gate 104. The metal barrier layer 103 can be a single-layer structure or a stacked structure, including a metal layer such as Ti or Ta, a metal nitride layer such as TiAlN, TaCN, TaSiN, TiN or TaN, or at least one of a metal and a metal nitride. In this embodiment, the metal gate 104 may include one or more work function metal layers and a metal electrode layer surrounded by the work function metal layer, wherein the material selection of the work function metal layer is determined by the conductivity type of the BCAT transistor to be formed. When the BCAT transistor to be formed is a P-type transistor, the work function metal layer in the metal gate 104 is a p-type work function metal material, and the p-type work function metal material may include TiN, TaN, Ru, Mo, Al, WN, ZrSi2, MoSi2, TaSi2, NiSi2, W and other suitable p-type work function materials or a combination thereof. When the BCAT transistor to be formed is an N-type transistor, the work function metal layer in the metal gate 104 is an n-type work function metal material, and the n-type work function metal material includes Ti, Ag, TaAl, TaAlC, TiAlN, TaC, TaCN, TaSiN, Mn, Zr, other suitable n-type work function materials or a combination thereof; the material of the metal electrode layer may include Al, W, Cu and / or other suitable metal materials.

[0108] Preferably, a metal adhesion layer 1141 , a metal barrier layer 1142 and a metal silicide layer 1143 are sequentially formed between the metal gate 104 and the polysilicon gate 105 from bottom to top. Among them, the metal adhesion layer 1141 can enhance the adhesion between the metal gate 104 and the polysilicon gate 105 to prevent the final composite gate from breaking. The material of the adhesion layer 1141 can be metal such as W, Ti or Ta; the metal barrier layer 1142 can prevent the metal in the metal gate 104 from diffusing into the polysilicon gate 105 and affecting the performance of the metal gate 104 and the polysilicon gate 105. The material of the metal barrier layer 1142 can be metal nitride such as TiAlN, TaCN, TaSiN, TiN or TaN; the metal silicide layer 1143 can reduce the contact resistance between the metal gate 104 and the polysilicon gate 105 to reduce the resistance of the formed composite gate. The metal silicide layer 1143 can be a metal silicide containing at least one of the metal elements such as Ti, W, Co, Ni, Zr, Mo, Ta, etc.

[0109] In this embodiment, the first conductive contact structure 109 is formed on the first source / drain region 1002, and the top surface of the first conductive contact structure 109 is flush with the top surface of the gate isolation layer 106, and a gap is formed between the first conductive contact structure 109 and the sidewalls facing the gate trench 101; the wire 111 is formed on the first conductive contact structure 109, and the wire 111 is arranged with the same width as the first conductive contact structure 109; the interlayer dielectric layer 112 covers the gate isolation layer 106, the first source / drain region 1002, the second source / drain region 1003, the wire 111 and the first conductive contact structure 109, and the interlayer dielectric layer 112 fills the gap between the sidewalls of the first conductive contact structure 109 and buries the wire 111 and the first conductive contact structure 109. The second conductive contact structure 113 is formed in the interlayer dielectric layer 112, and the bottom surface of the second conductive contact structure 113 contacts the top surface of the second source / drain region 1003.

[0110] In one embodiment of the present invention, a plurality of active areas (not shown) are formed in the semiconductor substrate 100, two gate trenches 101 are arranged side by side in each of the active areas, a first source / drain area 1002 is formed in the active area between the two gate trenches 101, second source / drain areas 1003 are respectively formed in the active areas on opposite sides of the two gate trenches 101, the first conductive contact structure 109 is formed above the first source / drain area 1002 and the bottom surface is in contact with the top surface of the first source / drain area 1002, the second conductive contact structure 113 is formed above the second source / drain area 1003 and the bottom surface is in contact with the top surface of the second source / drain area 1003, thereby forming two BCATs in one active area to improve device integration. When the semiconductor device is a memory, the multiple active areas are arranged in an array of cell rows and cell columns, the composite gates on each cell row are connected as a word line of the memory, and the conductors 111 on each cell column are connected as a bit line of the memory.

[0111] Please refer to Figure 4 In other embodiments of the present invention, the first conductive contact structure 109 is a composite structure, including a metal layer 1091 and a polysilicon layer 1092 stacked on the metal layer 1091, and the material of the conductive line 111 includes metal.

[0112] In one embodiment of the present invention, there are a metal silicide layer (not shown), a metal barrier layer (not shown) and a metal adhesion layer (not shown) between the metal layer 1091 and the first source and drain region 1002 from bottom to top, wherein the metal adhesion layer can enhance the adhesion between the metal layer 1091 and the first source and drain region 1002 to prevent poor contact between the first conductive contact structure 109 and the first source and drain region 1002, and the material of the metal adhesion layer can be a metal such as W, Ti or Ta; the metal barrier layer can prevent the metal in the metal layer from diffusing into the first source and drain region 1002 and affecting the performance of the first source and drain region 1002, and the material of the metal barrier layer can be a metal nitride such as TiAlN, TaCN, TaSiN, TiN or TaN; the metal silicide layer can reduce the contact resistance between the metal layer and the first source and drain region 1002, and the metal silicide layer can be a metal silicide containing at least one of the metal elements such as Ti, W, Co, Ni, Zr, Mo, Ta, etc.

[0113] In another embodiment of the present invention, a metal adhesion layer 1093, a metal barrier layer 1094, and a metal silicide layer 1095 are sequentially formed between the metal layer 1091 and the polysilicon layer 1092 from bottom to top, and a metal silicide layer 1096, a metal barrier layer 1097, and a metal adhesion layer 1098 are sequentially formed between the polysilicon layer 1092 and the bit line 111 from bottom to top, wherein the metal adhesion layer 1093 can enhance the adhesion between the metal layer 1091 and the polysilicon layer 1092 to prevent the metal layer 1091 and the polysilicon layer 1092 from having poor contact or even cracking, the metal adhesion layer 1098 can enhance the adhesion between the wire 111 and the polysilicon layer 1092 to prevent the bit line 111 and the polysilicon layer 1092 from having poor contact or even cracking, and the materials of the metal adhesion layers 1093 and 1098 can be metals such as W, Ti, or Ta; the metal barrier layer 1094 can be Prevent the metal in the metal layer 1091 from diffusing into the polysilicon layer 1092. The metal barrier layer 1097 can prevent the metal in the wire 111 from diffusing into the polysilicon layer 1092. The materials of the metal barrier layers 1094 and 1097 can be metal nitrides such as TiAlN, TaCN, TaSiN, TiN or TaN. The metal silicide layer 1095 can reduce the contact resistance between the metal layer 1091 and the polysilicon layer 1092, and further prevent the metal in the metal layer 1091 from diffusing into the polysilicon layer 1092. The metal silicide layer 1096 can reduce the contact resistance between the wire 111 and the polysilicon layer 1092 and further prevent the metal in the wire 111 from diffusing into the polysilicon layer 1092. The metal silicide layers 1095 and 1096 can be metal silicides containing at least one of the metal elements such as Ti, W, Co, Ni, Zr, Mo, Ta, etc.

[0114] In addition, the present invention also provides an electronic device, including the semiconductor device of the present invention. The electronic device of the present invention can be various mobile terminals such as mobile phones, wearable devices, laptop computers, tablet computers, etc., and the wearable devices include smart glasses, head-mounted devices, and wrist-mounted devices such as watches and bracelets.

[0115] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A method for preparing a semiconductor device, characterized in that: include: Providing a semiconductor substrate having a gate trench; Filling a metal gate in the gate trench, wherein the height of the metal gate is smaller than the depth of the gate trench; and, Filling a polysilicon gate in the gate trench, wherein the polysilicon gate is stacked on the metal gate to form a composite gate; Wherein, a metal adhesion layer, a metal barrier layer and a metal silicide layer are sequentially formed between the metal gate and the polysilicon gate from bottom to top.

2. The method for preparing a semiconductor device according to claim 1, wherein: The top surface of the polysilicon gate is lower than the top surface of the semiconductor substrate on the side wall of the gate trench. The method for preparing the semiconductor device also includes: filling a gate isolation layer in the gate trench, wherein the gate isolation layer fills the gate trench to bury the metal gate and the polysilicon gate therein.

3. The method for preparing a semiconductor device according to claim 1, wherein: Before filling the metal gate in the gate trench, a gate dielectric layer is first formed on the sidewall and bottom wall of the gate trench.

4. The method for preparing a semiconductor device according to claim 3, wherein: After forming the gate dielectric layer and before filling the metal gate, a metal barrier layer is formed on the surface of the gate dielectric layer, and after the metal gate is filled, the metal barrier layer surrounds the bottom wall and side wall of the metal gate and exposes the surface of the gate dielectric layer above the metal gate, so that the side wall of the polysilicon gate is directly in contact with the surface of the gate dielectric layer.

5. The method for preparing a semiconductor device according to any one of claims 1 to 4, characterized in that: Also includes: forming a first conductive contact structure on the semiconductor substrate at one side of the gate trench; forming a conductive line on the first conductive contact structure; forming an interlayer dielectric layer on the gate trench and the semiconductor substrate, wherein the interlayer dielectric layer buries the conductive wire and the first conductive contact structure; as well as, A second conductive contact structure is formed in the interlayer dielectric layer, wherein a bottom surface of the second conductive contact structure contacts a surface of the semiconductor substrate at the other side of the gate trench.

6. The method for preparing a semiconductor device according to claim 5, characterized in that: At least one active area is formed in the semiconductor substrate, two gate trenches are arranged side by side in the active area, a first source / drain area is formed in the active area between the two gate trenches, second source / drain areas are respectively formed in the active areas on opposite sides of the two gate trenches, the first conductive contact structure is formed above the first source / drain area and the bottom surface is in contact with the top surface of the first source / drain area, and the second conductive contact structure is formed above the second source / drain area and the bottom surface is in contact with the top surface of the second source / drain area.

7. The method for preparing a semiconductor device according to claim 6, wherein: The step of forming the first conductive contact structure comprises: Forming a hard mask layer covering the gate trench and the semiconductor substrate, wherein the hard mask layer has an opening exposing a surface of the active area between the two gate trenches; Using the hard mask layer as a mask, etching the exposed active area to form a contact trench, wherein the bottom surface of the contact trench is higher than the top surface of the polysilicon gate; and, The first conductive contact structure is filled in the contact trench, and the hard mask layer is removed.

8. The method for preparing a semiconductor device according to claim 7, wherein: The contact trench is connected to the two gate trenches at the sidewalls respectively, and the step of forming the conductive line comprises: Forming a sacrificial layer covering the gate trench, the semiconductor substrate and the first conductive contact structure, wherein the sacrificial layer has an opening exposing a portion of the surface of the first conductive contact structure; filling the conductive line in the opening of the sacrificial layer; and, The sacrificial layer is removed, and the first conductive contact structure is etched to the interface between the bottom surface of the first conductive contact structure and the semiconductor substrate using the conductive line as a mask, so that the first conductive contact structure is as wide as the conductive line.

9. The method for preparing a semiconductor device according to claim 5, wherein: The first conductive contact structure is a composite structure, including a metal layer and a polysilicon layer stacked on the metal layer, and the material of the conductive line includes metal.

10. A semiconductor device, characterized in that: include: A semiconductor substrate having a gate trench; a metal gate filled in the gate trench, wherein the height of the metal gate is less than the depth of the gate trench; and A polysilicon gate is filled in the gate trench, and the polysilicon gate is stacked on the metal gate; Wherein, a metal adhesion layer, a metal barrier layer and a metal silicide layer are sequentially arranged between the metal gate and the polysilicon gate from bottom to top.

11. The semiconductor device according to claim 10, wherein: The top surface of the polysilicon gate is lower than the top surface of the semiconductor substrate on the side wall of the gate trench. The semiconductor device also includes: a gate isolation layer filled in the gate trench, and the gate isolation layer fills the gate trench to bury the metal gate and the polysilicon gate therein.

12. The semiconductor device according to claim 10, wherein: It also includes a gate dielectric layer and a metal barrier layer, wherein the gate dielectric layer is formed on the side walls and bottom walls of the gate trench, the metal barrier layer is formed between the gate dielectric layer and the metal gate, surrounds the bottom wall and side walls of the metal gate and exposes the surface of the gate dielectric layer above the metal gate, and the side walls of the polysilicon gate are directly in contact with the side wall surfaces of the gate dielectric layer exposed by the metal barrier layer.

13. The semiconductor device according to claim 11, wherein: Also includes: A first conductive contact structure is formed on the semiconductor substrate at one side of the gate trench; A conductive line formed on the first conductive contact structure; an interlayer dielectric layer, covering the gate isolation layer and the semiconductor substrate, wherein the interlayer dielectric layer buries the conductive wire and the first conductive contact structure; as well as, A second conductive contact structure is formed in the interlayer dielectric layer, and a bottom surface of the second conductive contact structure contacts a surface of the semiconductor substrate at the other side of the gate trench.

14. The semiconductor device according to claim 13, wherein: At least one active area is formed in the semiconductor substrate, two gate trenches are arranged side by side in the active area, a first source / drain area is formed in the active area between the two gate trenches, second source / drain areas are respectively formed in the active areas on opposite sides of the two gate trenches, the first conductive contact structure is formed above the first source / drain area and the bottom surface is in contact with the top surface of the first source / drain area, and the second conductive contact structure is formed above the second source / drain area and the bottom surface is in contact with the top surface of the second source / drain area.

15. The semiconductor device according to claim 13, wherein: A gap is formed between the first conductive contact structure and the sidewalls of the gate trench facing each other, and the interlayer dielectric layer fills the gap.

16. The semiconductor device according to any one of claims 13 to 15, characterized in that The first conductive contact structure is a composite structure, including a metal layer and a polysilicon layer stacked on the metal layer, and the material of the conductive line includes metal.