Mold, orientation molding press and method for preparing lace magnetic steel
By combining magnetic and non-magnetic areas in the mold and using coils to generate magnetic fields to oriented magnetic powder, the problems of cracks and low residual magnetism in the production of special-shaped lace magnetic steel are solved, and high-quality and high residual magnetism are achieved. Effect.
Patent Information
- Application Number
- CN201911379278.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-12-27
AI Technical Summary
The prior art is prone to the problems of cracks and low residual magnetism when producing special-shaped lace magnetic steel, resulting in low product quality and high cost.
A mold is designed, which includes a front side plate, a rear side plate, a left side plate and a right side plate. The combination of the magnetic conduction area and the non-magnetic region are combined. The magnetic field is generated by energizing the coils on both sides of the mold, so that the magnetic powder is rearranged and oriented. , a powder distribution consistent with the shape of the magnetically conductive region is formed, and pressed using arc-shaped or flat upper and lower punches.
High residual magnet (residual magnet ≥13.5kGs), low crack rate and high quality lace magnet production are achieved, while simplifying the process and reducing costs.
Smart Images

Figure CN110899694B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a mold, an orientation forming press and a method for preparing lace magnetic steel. Background Art
[0002] In the actual use of the motor, it is found that the four corners of the square magnetic steel are subjected to a large demagnetization current and are prone to demagnetization. If the four corners of the square magnetic steel can be eliminated and magnets with higher remanence are used, the anti-demagnetization ability can be improved and the amount of raw materials used for the magnetic steel can be reduced. Therefore, it is necessary to produce special-shaped sheet magnetic steel products without four corners.
[0003] In the prior art, parallel orientation pressing technology can be used to produce special-shaped products. However, since parallel pressing will destroy the orientation of the magnetic steel, high remanence products cannot be produced. Therefore, when it is necessary to produce special-shaped products with high remanence, vertical orientation pressing technology needs to be used. However, if a vertical orientation process is used to prepare high remanence lace magnetic steel products, since the upper ends of most vertical orientation pressing powder cavities used are flat, special-shaped products cannot be produced directly. At this time, when producing special-shaped products, it is necessary to first press the square blank, then perform electric spark cutting of the arc, and then perform grinding wheel grinding, resulting in low yield, high cost, and low efficiency.
[0004] The prior art attempts to solve the above problems. For example, patent CN202861397U can directly produce special-shaped products by setting the upper and lower punches to arc shape, saving processes. Another example is patent CN208391003U discloses a mold system that can also produce special-shaped products. However, patents CN202861397U and CN208391003U are only suitable for tile-shaped products with a small arc (the distance between the highest point and the lowest point in the height direction of the special-shaped surface of the pressed blank is less than 8mm) ( Figure 1 ) production, and in the production of Figures 2 to 4 When producing the type of lace-shaped products shown, if the method of patent CN202861397U is used, the powder will be deformed greatly, density unevenness will be easily produced after the upper punch is pressed, and excessive powder flow will destroy the orientation, resulting in cracks (crack rate is 1%-5%) and low remanence (local remanence of the magnetic steel is less than 12kGs, and the magnetic field of the magnetic steel is uneven).
[0005] Therefore, it is necessary to develop a preparation process for lace magnetic steel to produce products with complex shapes in the orientation direction, while ensuring that the products have high remanence and high quality, simplifying the operation, increasing the yield and reducing the cost. Summary of the invention
[0006] The technical problem to be solved by the present invention is that in the prior art, when using special-shaped molds to produce special-shaped products, cracks are easily generated and the residual magnetism is low. The present invention provides a mold, an orientation molding press and a method for preparing lace magnetic steel. The present invention can simplify the process, increase the yield and reduce the cost while ensuring that the prepared lace magnetic steel has high residual magnetism (residual magnetism ≥ 13.5kGs) and high quality.
[0007] The present invention solves the above technical problems through the following technical solutions.
[0008] The present invention provides a mold for preparing lace magnetic steel, characterized in that it includes a front side plate, a rear side plate, a left side plate and a right side plate;
[0009] The front side plate, the rear side plate, the left side plate and the right side plate form a cavity with upper and lower openings;
[0010] Wherein, the left side plate and the right side plate are both made of non-magnetic conductive materials;
[0011] The central areas of the front side plate and the rear side plate close to the cavity are both magnetic conductive areas, and the areas other than the central areas are all non-magnetic conductive areas;
[0012] The width of the magnetic conductive area is equal to the width of the cavity, and the shape corresponds to the lace magnetic steel.
[0013] In the present invention, the lace magnetic steel can be a conventional ferromagnetic anisotropic magnetic steel in the art. Preferably, the lace magnetic steel is a neodymium iron boron magnetic steel, a samarium cobalt magnetic steel or a ferrite magnetic steel.
[0014] In the present invention, the connection method of the front side panel, the rear side panel, the left side panel and the right side panel can be a conventional connection method in the art. Preferably, the connection method between the front side panel, the rear side panel, the left side panel and the right side panel is bolt connection. More preferably, the front side panel and the rear side panel are connected by 3-4 M12-M16 bolts penetrating the left side panel; the front side panel and the rear side panel are connected by 3-4 M12-M16 bolts penetrating the right side panel.
[0015] In the present invention, when using the mold, those skilled in the art know that when preparing the lace magnetic steel, coils can be set on both sides of the magnetic conductive area to generate a magnetic field after adding magnetic powder to the mold to complete the powder distribution, so that the magnetic powder is rearranged and oriented to form a powder distribution consistent with the shape of the magnetic conductive area.
[0016] Preferably, the upper edge shape of the magnetic conductive area is the same as the upper edge shape of the lace magnetic steel, the lower edge shape of the magnetic conductive area is the same as the lower edge shape of the lace magnetic steel, and the left edge and the right edge of the magnetic conductive area are both straight lines.
[0017] Preferably, the height of the magnetic conductive area is 2-2.2 times the height of the green compact. Those skilled in the art know that the green compact height refers to the height of the green compact after compression molding. In the present invention, the inventors found that when preparing the lace magnetic steel, if the height of the loose powder after powder distribution is equal to the height of the magnetic conductive area, the green compact obtained after compression can have a suitable density.
[0018] Those skilled in the art know that the magnetic conductive area and the non-magnetic conductive area are located in the same plane, forming a cavity with a smooth surface and upper and lower openings.
[0019] In the present invention, in order to better fix the magnetic conductive area and the non-magnetic conductive area, the front side plate and the rear side plate preferably include a magnetic conductive plate provided with a magnetic conductive portion, and a non-magnetic conductive plate provided with a hollow portion; the magnetic conductive portion is nested in the hollow portion, so that the magnetic conductive plate is fixed to the non-magnetic conductive plate.
[0020] More preferably, the magnetic conductive plate is fixed to the non-magnetic conductive plate by 6-8 M6-M8 bolts.
[0021] More preferably, the left side plate, the right side plate and the non-magnetic plate are provided with a plurality of circular channels parallel to the mold cavity, which are used to install the mold inside an orientation molding press used in conjunction therewith.
[0022] In the present invention, those skilled in the art can know after seeing the technical solution of the present invention that when the magnetic conductive plate is fixed to the non-magnetic conductive plate by bolt connection, the magnetic conductive part can be fixed to the non-magnetic conductive plate in a nested manner. Therefore, the functions of the magnetic conductive plate and the hollow part are: on the one hand, they can be used to fix the magnetic conductive part to the non-magnetic conductive plate; on the other hand, they can play a positioning role, ensuring that the side of the magnetic conductive part close to the cavity and the side of the non-magnetic conductive plate close to the cavity are in the same plane; in addition, the design of the magnetic conductive plate can also play a role in strengthening the magnetic field and binding the magnetism.
[0023] In the present invention, those skilled in the art may know after seeing the technical solution of the present invention that the width, height and shape of the magnetic conductive portion are the same as those of the magnetic conductive area.
[0024] In the present invention, those skilled in the art can know after seeing the technical solution of the present invention that the non-magnetic area, the non-magnetic plate, the left plate, the right plate and the connecting structure are all made of non-magnetic materials. Preferably, the non-magnetic material is non-magnetic tungsten steel, G60 or 70Mn.
[0025] In the present invention, those skilled in the art can know after seeing the technical solution of the present invention that the magnetic conductive plate or the magnetic conductive area is made of magnetic conductive material. Preferably, the magnetic conductive material is 45#, Cr 12 , pure iron or iron cobalt.
[0026] In the present invention, those skilled in the art can know after seeing the technical solution of the present invention that when using the mold to prepare lace magnetic steel, it is necessary to cooperate with the orientation forming press, and in order to obtain the lace magnetic steel of the target structure, the upper punch and the lower punch of the orientation forming press need to be designed corresponding to the shape of the lace magnetic steel. Preferably, the shape of the upper punch surface corresponds to the shape of the upper edge of the lace magnetic steel, and the shape of the lower punch surface corresponds to the shape of the lower edge of the lace magnetic steel.
[0027] The present invention also provides an orientation forming press for preparing lace magnetic steel, characterized in that it includes the mold as described above.
[0028] Preferably, the orientation forming press further comprises the upper punch and the lower punch.
[0029] Preferably, the upper punch and the lower punch are made of non-magnetic conductive material.
[0030] More preferably, the non-magnetic material is non-magnetic tungsten steel, G60 or 70Mn.
[0031] The present invention also provides a method for preparing lace magnetic steel, which uses the orientation forming press as described above, and comprises the following steps:
[0032] S1. Add magnetic powder to the mold to complete the powder distribution;
[0033] S2. Under the condition that the coils on both sides of the die are energized, the upper punch moves downward, so that the magnetic powder is piled up in the shape of the magnetic conductive area and then pressed to obtain a compact;
[0034] S3. Reversely demagnetize the compact and then sinter it.
[0035] Preferably, before performing step S1, the magnetic field of the orientation molding press is detected, the cavity magnetic field strength is greater than 16500 Gs, and the multi-point detection deviation is less than 500 Gs.
[0036] In step S1, after seeing the technical solution of the present invention, a person skilled in the art may know that the mold needs to be lowered before applying the powder until the lower edge of the magnetic conductive area is flush with the surface of the lower punch, and the amount of magnetic powder added needs to be coordinated with the lace magnetic steel.
[0037] In step S1, preferably, magnetic powder is added to the mold until the height of the powder is the same as the height of the magnetic conductive area.
[0038] In step S2, those skilled in the art may know after seeing the technical solution of the present invention that the upper punch needs to move downward to the mold closing position, and the mold closing position needs to cooperate with the lace magnetic steel of the target structure.
[0039] In step S2, the coils on both sides of the mold are energized to generate a magnetic field. At this time, the magnetic induction lines around will gather towards the magnetic conductive area (magnetic beam effect of the magnetic conductive material), the magnetic induction lines in the magnetic conductive area are vertically injected, and the magnetic induction lines outside the area are injected at a certain angle. Therefore, the number of magnetic induction lines passing through the magnetic conductive area is much larger than that of other parts, and the number of magnetic induction lines gathers and there is an obvious gathering phenomenon, so that the magnetic field intensity of the magnetic conductive area is also higher than that of other parts. When the magnetic induction lines enter the cavity from the magnetic conductive area, the magnetic field intensity of the part between the magnetic conductive areas of the front side plate and the rear side plate is the strongest, so that the magnetic powder is rearranged and oriented, and the magnetic powder moves to the area with high magnetic field intensity, and finally forms a powder distribution consistent with the shape of the magnetic conductive area. Therefore, even if the upper punch descends quickly, it can ensure that the compact will crack due to the uneven density of the magnetic powder during the pressing process, and a compact with a low crack rate and consistent orientation can be obtained, so that it can obtain a high remanence and high-quality product after demagnetization and sintering.
[0040] Preferably, in step S2, the upper punch moves downward at a speed of 100-300 mm / s, for example, 200 mm / s.
[0041] Preferably, in step S2, the coil continuously generates a 16000Gs magnetic field after being energized.
[0042] Preferably, in step S2, the pressing comprises: after the upper punch moves downward to the mold closing position, floating pressing of the upper punch and the mold is performed.
[0043] Preferably, the powder density when the upper punch descends to the mold closing position is about 2.23-2.25 g / cm 3 , for example, 2.24 g / cm 3 .
[0044] More preferably, in the floating pressing, the speed ratio of the upper punch to the die is 1.1-1.3:1, for example, 1.2:1, and the pressing tonnage is 15-20T, for example, 18T.
[0045] In step S2, those skilled in the art know that the pressing is completed after the pressing reaches a set size, and the pressing can be maintained. Preferably, the pressing is maintained for 2-5 seconds after the pressing is completed.
[0046] Preferably, in step S2, after the pressure holding is completed, the coils on both sides of the mold are stopped from being energized.
[0047] Preferably, in step S3, the reverse demagnetization is followed by pressure relief to obtain a compact.
[0048] Preferably, in step S3, the sintering temperature is 1000-1100°C.
[0049] Those skilled in the art know that the lace magnetic steel can be obtained after sintering. Preferably, the lace magnetic steel is sliced perpendicular to the cross-sectional direction to obtain a plurality of sheet-shaped lace magnetic steels.
[0050] More preferably, the thickness of the sheet lace magnetic steel is 1.7-2.1 mm.
[0051] The present invention also provides a lace magnetic steel, characterized in that it is prepared by the preparation method as described above.
[0052] Preferably, the remanence of the lace magnetic steel is ≥13.5 kGs.
[0053] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0054] The reagents and raw materials used in the present invention are commercially available.
[0055] The positive and progressive effects of the present invention are:
[0056] In the present invention, the central areas of the front and rear side plates of the mold close to one side of the cavity are all magnetic conductive areas, and the areas other than the central areas are all non-magnetic conductive areas; when preparing lace magnetic steel, the coils on both sides of the mold are energized to rearrange and orient the magnetic powder, thereby greatly reducing the crack rate caused by the uneven density of the magnetic powder generated during the pressing process; at the same time, upper and lower punches with arcs or planes (but not limited to arcs or planes) that are matched with the mold are used to prepare the lace magnetic steel, which can simplify the process, increase the yield and reduce the cost while ensuring that it has high remanence (remanence ≥13.5kGs), high quality (low crack rate), and excellent magnetic properties (Hcj ≥24kOe, Hcb ≥12.5kOe, maximum magnetic energy product ≥43.5MGOe). BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 This is a schematic diagram of a tile-shaped product with a small curvature (the distance between the highest point and the lowest point in the height direction of the profiled surface of the pressed blank is less than 8 mm).
[0058] Figure 2 This is a schematic diagram of the lace magnetic steel of Example 1.
[0059] Figure 3This is a schematic diagram of the lace magnetic steel of Example 2.
[0060] Figure 4 Schematic diagram of the lace magnetic steel of Example 3.
[0061] Figure 5 This is a schematic diagram of the magnetic flux lines after the coils on both sides of the mold are energized during the preparation process of Example 1.
[0062] Figure 6 This is a schematic diagram of the change in magnetic powder accumulation before and after the coils on both sides of the mold are energized during the preparation process of Example 1.
[0063] Figure 7 This is a schematic diagram of the lace magnetic steel of Example 1.
[0064] Figure 8 This is a schematic diagram of the lace magnetic steel of Example 2.
[0065] Fig. 9 Schematic diagram of the lace magnetic steel of Example 3.
[0066] Fig.10 Schematic diagram of the positional relationship of the assembled mold, upper punch and lower punch of Example 1. Fig.11 This is a schematic diagram of the assembled mold of Example 1.
[0067] Fig.12 Schematic diagram of the rear side panel of Example 1.
[0068] Fig.13 Schematic diagram of the magnetic conductive plate of Example 1.
[0069] Fig.14 Schematic diagram of the non-magnetic plate of Example 1.
[0070] Fig.15 This is a schematic diagram of the left side panel of Example 1.
[0071] Fig.16 Schematic diagram of the upper punch of Example 1.
[0072] Fig.17 Schematic diagram of the lower punch of Example 1.
[0073] Description of Reference Numerals
[0074] Mold 1
[0075] Front side panel 2
[0076] Rear side panel 3
[0077] Left side panel 4
[0078] Right side panel 5
[0079] Cavity 6
[0080] Magnetic area 7
[0081] Non-magnetic area 8
[0082] M13 bolt connection 9
[0083] Magnetic conductive part 71
[0084] Magnetic plate 72
[0085] Hollow part 81
[0086] Non-magnetic plate 82
[0087] M7 bolt connection 10
[0088] Circular channel 11
[0089] Upper punch 12
[0090] Lower punch 13 DETAILED DESCRIPTION
[0091] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product instructions.
[0092] Example 1
[0093] Example 1 The object is to prepare Figure 7 The dimensions of the lace magnet shown meet the following conditions: a=40mm, b=30mm, radius R=11mm.
[0094] In order to prepare the target lace magnetic steel in this embodiment, the mold 1 as described below is required.
[0095] The mold 1 includes a front side plate 2 ( Fig.15 ), rear side plate 3, left side plate 4 and right side plate 5. Among them, the front side plate 2, the rear side plate 3, the left side plate 4 and the right side plate 5 surround a cavity 6 (opened up and down) Fig.11 ).
[0096] The central areas of the front side plate 2 and the rear side plate 3 near the cavity 6 are all magnetic conductive areas 7, and the areas other than the central areas are all non-magnetic conductive areas 8 ( Fig.12 ); the materials of the left side plate 4 and the right side plate 5 are both non-magnetic conductive materials.
[0097] The width of the magnetic conductive area 7 is equal to the width of the cavity 6, and the shape corresponds to the lace magnetic steel.
[0098] The lace magnet is a neodymium iron boron magnet.
[0099] The front side plate 2 and the rear side plate 3 are connected by four M13 bolts 9 penetrating the left side plate 4 ; the front side plate 2 and the rear side plate 3 are connected by four M13 bolts 9 penetrating the right side plates 5 .
[0100] The non-magnetic conductive area 8, the left side plate 4, the right side plate 5 and the connection structure are all made of non-magnetic conductive materials, which are non-magnetic conductive tungsten steel.
[0101] When using the mold 1, when preparing lace magnetic steel, coils can be set on both sides of the magnetic conductive area 7, which are used to generate a magnetic field by turning on power after adding magnetic powder to the mold 1 and completing the powder distribution, so that the magnetic powder is rearranged and oriented to form a powder distribution consistent with the shape of the magnetic conductive area 7.
[0102] The upper edge shape of the magnetic conductive area 7 is the same as the upper edge shape of the lace magnetic steel, the lower edge shape of the magnetic conductive area 7 is the same as the lower edge shape of the lace magnetic steel, and the left edge and the right edge of the magnetic conductive area 7 are both straight lines.
[0103] The height of the magnetic conductive area 7 is twice the height of the green compact, which refers to the height of the green compact after compaction. When preparing lace magnetic steel, if the height of the loose powder after powder distribution is equal to the height of the magnetic conductive area 7, the green compact obtained after compaction can have a suitable density.
[0104] The magnetic conductive area 7 and the non-magnetic conductive area 8 are located in the same plane, forming a cavity 6 with a smooth surface and upper and lower openings.
[0105] In order to better fix the magnetic conductive area 7 and the non-magnetic conductive area 8, the front side plate 2 and the rear side plate 3 include a magnetic conductive plate 72 ( Fig.13 ), and a non-magnetic plate 82 having a hollow portion 81 ( Fig.14 ); the magnetic conductive portion 71 is nested in the hollow portion 81, so that the magnetic conductive plate 72 is fixed to the non-magnetic conductive plate 82.
[0106] The magnetic conductive plate 72 is fixed to the non-magnetic conductive plate 82 by six M7 bolts 10 .
[0107] The left side plate 4, the right side plate 5 and the non-magnetic plate 82 are provided with a plurality of (six in total) circular channels 11 parallel to the cavity 6, which are used to install the mold 1 inside the orientation molding press used in conjunction therewith.
[0108] When the magnetic conductive plate 72 is fixed to the non-magnetic conductive plate 82 by using the M7 bolt connection 10, the magnetic conductive portion 71 can be fixed to the non-magnetic conductive plate 82 in a nested manner. Therefore, the magnetic conductive plate 72 and the hollow portion 81 have the following functions: on the one hand, they can be used to fix the magnetic conductive portion 71 to be nested in the non-magnetic conductive plate 82; on the other hand, they can play a positioning role, ensuring that the side of the magnetic conductive portion 71 close to the cavity 6 and the side of the non-magnetic conductive plate 82 close to the cavity 6 are located in the same plane; in addition, the design of the magnetic conductive plate 72 can also play a role in strengthening the magnetic field and binding the magnetism.
[0109] The width, height and shape of the magnetic conductive portion 71 are the same as those of the magnetic conductive region 7 .
[0110] The magnetic conductive plate 72 is made of a magnetic conductive material, and the magnetic conductive material is 45#.
[0111] When using the mold 1 to prepare the lace magnetic steel, it needs to be used in conjunction with an orientation molding press, and in order to obtain the lace magnetic steel of the target structure, the upper punch 12 and the lower punch 13 ( Fig.10 , 16 and 17) to design corresponding to the shape of the lace magnet.
[0112] The orientation forming press comprises the mold 1 as described above, and also comprises an upper punch 12 and a lower punch 13. The shape of the surface of the upper punch 12 corresponds to the shape of the upper edge of the lace magnetic steel, and the shape of the surface of the lower punch 13 corresponds to the shape of the lower edge of the lace magnetic steel.
[0113] The upper punch 12 and the lower punch 13 are made of non-magnetic conductive material.
[0114] The preparation method of lace magnetic steel is as follows:
[0115] (1) Before starting the machine, the magnetic field of the press is tested. The cavity magnetic field strength is >16500Gs, and the multi-point detection deviation is <500Gs.
[0116] (2) The mold 1 as described above is lowered until the lower edge of the magnetic conductive area 7 is flush with the surface of the lower punch 13, and the feeder is pushed out to the top of the center of the mold 1 for reciprocating feeding. Magnetic powder is added to the mold 1 until the height of the powder is the same as the height of the magnetic conductive area 7, thereby completing the powder distribution.
[0117] (3) After the feeding is completed, the feeder returns to the original position, and the upper punch 12 moves downward at a high speed of 200 mm / s.
[0118] (4) Starting from the downward movement of the upper punch 12, the coils on both sides of the die 1 are energized to generate a magnetic field. At this time, the magnetic induction lines around will gather towards the magnetic conductive area 7, so the number of magnetic induction lines passing through the magnetic conductive area 7 is much greater than that of other parts. The number of magnetic induction lines gathers and there is an obvious gathering phenomenon, which causes the magnetic powder to rearrange and orient, and the magnetic powder moves to the area with high magnetic field intensity, and finally forms a powder distribution consistent with the appearance of the magnetic conductive area 7 ( Figure 5-6 ).
[0119] (5) The upper punch 12 moves down to the mold closing position at high speed and compresses a portion of the powder. The density of the compressed powder is about 2.24 g / cm 3 At this time, the coil is still powered on and continues to generate a 16000Gs magnetic field.
[0120] (6) The upper punch 12 and the die 1 begin floating pressing, the speed ratio of the upper punch 12 and the die 1 is 1.2:1, and the pressing tonnage is 18T.
[0121] (7) After pressing to the set size, hold the pressure for 4 seconds. After the pressure holding is completed, stop energizing the coils on both sides of the mold 1 and perform reverse demagnetization.
[0122] (8) After demagnetization is completed, pressure is released.
[0123] (9) After the pressure relief is completed, the mold 1 moves downward, and the pressed blank escapes from the mold cavity 6.
[0124] (10) The green compact is sintered at a sintering temperature between 1000-1100°C.
[0125] (11) Slice the lace magnetic steel perpendicular to the cross-section direction to obtain a plurality of sheet-shaped lace magnetic steels; the size of the obtained sheet-shaped lace magnetic steels is as follows: Figure 7 As shown, its thickness is 1.8 mm, a=40 mm, b=30 mm, and radius R=11 mm.
[0126] The properties of the prepared product are shown in Table 1.
[0127] Table 1 Performance of the prepared products
[0128]
[0129] The crack rate of the product of the present invention is ≤0.2%, which is equivalent to the crack rate of the block product; the crack rate of the traditional method is 1%-5%.
[0130] Example 2
[0131] Example 2 The object is to prepare Figure 8 The dimensions of the lace magnet shown meet the following conditions: a=40mm, b=30mm, c=12mm.
[0132] The preparation method is the same as that of Example 1. Those skilled in the art know that the mold and the upper and lower punches can be modified adaptively according to the desired product.
[0133] The size of the magnetic steel obtained is as follows Figure 8 As shown, a=40mm, b=30mm, c=12mm.
[0134] The properties of the prepared product are shown in Table 2.
[0135] Table 2 Performance of the prepared products
[0136]
[0137] The crack rate of the product of the present invention is ≤0.2%, which is equivalent to the crack rate of the block product; the crack rate of the traditional method is 1%-5%.
[0138] Example 3
[0139] Example 2 The object is to prepare Fig. 9 The dimensions of the lace magnet shown meet the following conditions: a=40mm, b=30mm, c=12mm.
[0140] The preparation method is the same as that of Example 1. Those skilled in the art know that the mold and the upper and lower punches can be modified adaptively according to the desired product.
[0141] The size of the magnetic steel obtained is as follows Fig. 9 As shown, a=40mm, b=30mm, c=12mm.
Claims
1. A mold for preparing lace magnetic steel, characterized in that: It includes a front side panel, a rear side panel, a left side panel and a right side panel; The front side plate, the rear side plate, the left side plate and the right side plate form a cavity with upper and lower openings; Wherein, the left side plate and the right side plate are both made of non-magnetic conductive materials; The central areas of the front side plate and the rear side plate close to the cavity are both magnetic conductive areas, and the areas other than the central areas are all non-magnetic conductive areas; The width of the magnetic conductive area is equal to the width of the cavity, and the shape corresponds to the lace magnetic steel; The upper edge shape of the magnetic conductive area is the same as the upper edge shape of the lace magnetic steel, the lower edge shape of the magnetic conductive area is the same as the lower edge shape of the lace magnetic steel, and the left edge and the right edge of the magnetic conductive area are both straight lines; The front side plate and the rear side plate include a magnetic conductive plate provided with a magnetic conductive portion and a non-magnetic conductive plate provided with a hollow portion; the magnetic conductive portion is embedded in the hollow portion, so that the magnetic conductive plate is fixed to the non-magnetic conductive plate; The height of the magnetic conductive area is 2-2.2 times the height of the green compact.
2. The mold according to claim 1, characterized in that The magnetic conductive plate is fixed to the non-magnetic conductive plate by 6-8 M6-M8 bolts.
3. The mold according to claim 1 or 2, characterized in that: The lace magnet is a neodymium iron boron magnet, a samarium cobalt magnet or a ferrite magnet; The front side plate, the rear side plate, the left side plate and the right side plate are connected by bolts; The non-magnetic conductive area, the non-magnetic conductive plate, the left plate, the right plate or the connecting structure are all made of non-magnetic conductive materials; The magnetic conductive area is made of magnetic conductive material.
4. The mold according to claim 3, characterized in that The front side plate and the rear side plate are connected by 3-4 M12-M16 bolts penetrating the left side plate; the front side plate and the rear side plate are connected by 3-4 M12-M16 bolts penetrating the right side plate; And / or, the non-magnetic material is non-magnetic tungsten steel, G60 or 70Mn; And / or, the magnetic conductive material is 45#, Cr 12 , pure iron or iron-cobalt; And / or, the left side plate, the right side plate and the non-magnetic plate are provided with a plurality of circular channels parallel to the mold cavity, which are used to install the mold inside the orientation molding press used in conjunction therewith.
5. An orientation forming press for preparing lace magnetic steel, characterized in that: It comprises the mold according to claim 1 or 2.
6. The orientation molding press according to claim 5, characterized in that The orientation forming press also includes an upper punch and a lower punch.
7. The orientation molding press according to claim 6, characterized in that The shape of the upper punch surface corresponds to the shape of the upper edge of the lace magnetic steel, and the shape of the lower punch surface corresponds to the shape of the lower edge of the lace magnetic steel; And / or, the upper punch and the lower punch are made of non-magnetic conductive material.
8. The orientation molding press according to claim 7, characterized in that The non-magnetic conductive material is non-magnetic tungsten steel, G60 or 70Mn.
9. A method for preparing lace magnetic steel, characterized in that: The method uses the orientation molding press as claimed in claim 6, comprising the following steps: S1. Add magnetic powder to the mold to complete the powder distribution; S2. Under the condition that the coils on both sides of the die are energized, the upper punch moves downward, so that the magnetic powder is piled up in the shape of the magnetic conductive area and then pressed to obtain a compact; S3. Reversely demagnetize the compact and then sinter it.
10. The method according to claim 9, characterized in that Before performing step S1, the magnetic field of the orientation molding press is detected, the cavity magnetic field strength is greater than 16500 Gs, and the multi-point detection deviation is less than 500 Gs; and / or, in step S1, adding magnetic powder to the mold until the height of the powder is the same as the height of the magnetic conductive area; And / or, in step S2, the upper punch moves downward at a speed of 100-300 mm / s; and / or, in step S2, the coil continuously generates a magnetic field of 16000Gs after being energized; And / or, in step S2, the pressing comprises: after the upper punch moves downward to the mold closing position, floating pressing of the upper punch and the mold is performed; And / or, in step S2, the pressure is maintained for 2-5 seconds after the pressing is completed; And / or, in step S3, the reverse demagnetization is followed by pressure relief to obtain a compact; And / or, in step S3, the sintering temperature is 1000-1100°C; And / or, the lace magnetic steel is sliced perpendicular to the cross-sectional direction to obtain a plurality of sheet-shaped lace magnetic steels.
11. The method according to claim 10, characterized in that In step S2, the upper punch moves downward at a speed of 200 mm / s; And / or, the powder density when the upper punch descends to the mold closing position is 2.23-2.25 g / cm 3 ; And / or, in step S2, after the pressure holding is completed, the coils on both sides of the mold are powered off; And / or, the thickness of the sheet lace magnetic steel is 1.7-2.1 mm.
12. The method according to claim 11, characterized in that The powder density when the upper punch descends to the mold closing position is 2.24 g / cm 3 .
13. The method according to claim 11, characterized in that In the floating pressing, the speed ratio of the upper punch to the die is 1.1-1.3:1, and the pressing tonnage is 15-20T.
14. The method according to claim 13, characterized in that During the floating pressing, the speed ratio of the upper punch to the die is 1.2:1; And / or, the pressing tonnage is 18 tons.
15. A lace magnetic steel, characterized in that: It is prepared by the method according to claim 9 or 10.
16. The lace magnetic steel according to claim 15, characterized in that: The residual magnetism of the lace magnetic steel is ≥13.5kGs.